Preparation method and application of Bi12O17Cl2-Ti3C2 composite photocatalyst
By constructing Bi12O17Cl2-Ti3C2 composite photocatalyst, the problem of low activity of Bi12O17Cl2 single-phase photocatalyst was solved, a more efficient degradation effect of tetracycline hydrochloride was achieved, and the photocatalytic performance was improved.
Patent Information
- Application Number
- CN202210678800.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-15
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-06-15
AI Technical Summary
The existing Bi12O17Cl2 as a single-phase photocatalyst has the problem of rapid recombination of photogenerated electron holes, resulting in low activity and difficulty in effectively degrading tetracycline hydrochloride.
Using layered Ti3C2 as a template, Bi12O17Cl2 is grown in situ to construct a two-dimensional/two-dimensional heterojunction to form a Bi12O17Cl2-Ti3C2 composite photocatalyst, which improves the separation efficiency of electrons and holes and enhances its photocatalytic degradation efficiency of tetracycline hydrochloride.
The efficiency of the photocatalytic degradation of tetracycline hydrochloride by Bi12O17Cl2 is improved, its light absorption capacity and band gap are enhanced, a more stable composite material is formed, and the photocatalytic performance is significantly improved.
Smart Images

Figure CN114950510B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of photocatalysis technology and specifically relates to a Bi 12 O 17 Preparation method and application of Cl2-Ti3C2 composite photocatalyst. Background Art
[0002] As a major antibiotic, tetracycline hydrochloride has a rapid and effective antibacterial effect to inhibit bacterial growth and is used for anti-infection treatment of patients. With the increase in the use of tetracycline hydrochloride antibiotics, many drugs are directly or indirectly discharged into the environment, affecting ecological safety and human health. Therefore, it is imperative to strengthen the prevention and control of antibiotic pollution in the environment.
[0003] Photocatalysis is a green and environmentally friendly advanced oxidation technology for removing organic pollution, which can completely mineralize organic matter into CO2 and H2O under the action of the sun. However, the synthesis of efficient, stable, green, and solar energy conversion efficient photocatalysts for the photocatalytic removal of tetracycline hydrochloride is still a difficult task.
[0004] Layered Bi12O 17 Cl2 materials have attracted widespread attention due to their small band gap and strong visible light photocatalytic ability. 12 O 17 As a single-phase photocatalyst, Cl2 inevitably has the problem of rapid recombination of photogenerated electron-hole pairs, which leads to its low activity. However, how to achieve rapid separation of photogenerated electron-hole pairs is of great significance to improving its photocatalytic performance. Summary of the invention
[0005] In view of the above-mentioned deficiencies in the prior art, the present invention aims to provide a 12 O 17 Preparation method of Cl2-Ti3C2 composite photocatalyst, the method uses layered Ti3C2 as template to in-situ grow Bi 12 O 17 Cl2 to construct a two-dimensional / two-dimensional heterojunction to improve its efficiency in photocatalytic degradation of tetracycline hydrochloride.
[0006] To achieve the above object, the present invention provides the following technical solutions: a Bi 12 O 17 The preparation method of Cl2-Ti3C2 composite photocatalyst comprises the following steps:
[0007] (1) Etching of Ti3C2: Take 1.00 g of Ti3AlC2 raw material, slowly add 20 mL of hydrofluoric acid in batches, stir at room temperature for 24-72 h, centrifuge at 3000 r / min for 30 min, wash to pH 6, and dry for 12-36 h;
[0008] (2) Weigh a certain amount of Ti3C2 and dissolve it in 15-45 mL of ethanol, stir evenly, and add 0.95-2.84 g of BiCl3 to completely dissolve;
[0009] (3) Add 15-45 mL of NaOH solution to the above solution, stir for 1-6 h, react in a reactor at 120 °C for 1-24 h, centrifuge, wash with deionized water until neutral, and vacuum dry.
[0010] Furthermore, the doping amount of Ti3C2 in step (2) is 0-20%.
[0011] Furthermore, the mass concentration of the hydrofluoric acid in step (1) is 40%.
[0012] Furthermore, the mass concentration of the NaOH solution in step (3) is 1.0 mol / L.
[0013] Furthermore, the drying in step (3) refers to vacuum drying the washed solid at 60° C. for 12 h.
[0014] The Bi prepared above 12 O 17 Application of Cl2 / Ti3C2 composite photocatalyst in degradation of tetracycline hydrochloride.
[0015] Compared with the prior art, the present invention has the following beneficial effects:
[0016] 1. The present invention uses layered Ti3C2 as a template to in-situ grow Bi 12 O 17 Cl2, making Bi 12 O 17 Cl2 and Ti3C2 are evenly dispersed and in good contact with each other, and can easily form a two-dimensional / two-dimensional heterojunction, thereby improving the separation efficiency of electrons and holes and enhancing the efficiency of photocatalytic degradation of tetracycline hydrochloride.
[0017] 2. Bi synthesized by the present invention 12 O 17 Compared with single-phase Bi 12 O 17 Cl2 has stronger light absorption ability and smaller band gap. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 for Bi 12 O 17 XRD spectrum of Cl2-Ti3C2 composite photocatalyst;
[0019] Figure 2 for Bi 12 O 17 SEM spectrum of Cl2-Ti3C2 composite photocatalyst;
[0020] Figure 3 for Bi 12 O 17 Element mapping diagram of Cl2-5%Ti3C2 composite material;
[0021] Figure 4 for Bi 12 O 17 TEM spectrum of Cl2-5%Ti3C2 composite photocatalyst;
[0022] Figure 5 for Bi 12 O 17 XPS spectrum of Cl2-5%Ti3C2 composite photocatalyst;
[0023] Figure 6 For different doping amounts of Bi 12 O 17 UV-visible diffuse reflectance spectrum of Cl2-Ti3C2 composite photocatalyst;
[0024] Figure 7 for Bi 12 O 17 Cl2, Ti3C2 and Bi 12 O 17 Cl2-5%Ti3C2 (αhv) 1 / 2 -Light energy (hv) diagram; Figure 7 Is Figure 6 The data in the figure are transformed, and the band gap of the material is further calculated by making a tangent line.
[0025] Figure 8 For different doping amounts of Bi 12 O 17 Photocurrent-time curve of Cl2-Ti3C2 composite photocatalyst;
[0026] Fig. 9 For different doping amounts of Bi 12 O 17 Performance results of Cl2-Ti3C2 composite photocatalyst in degradation of tetracycline hydrochloride under visible light at 357 nm;
[0027] Fig.10For different doping amounts of Bi 12 O 17 First-order photokinetic constant diagram of Cl2-Ti3C2 composite photocatalyst;
[0028] Fig.11 for Bi 12 O 17 Photodegradation effect diagram of Cl2-5%Ti3C2 composite photocatalyst with different capture agents added. DETAILED DESCRIPTION
[0029] The method of the present invention is described in detail below in conjunction with specific embodiments and accompanying drawings.
[0030] 1. Preparation of Bi 12 O 17 Cl2-Ti3C2 composite photocatalyst Example 1
[0031] A kind of Bi 12 O 17 The preparation method of Cl2-Ti3C2 composite photocatalyst comprises the following steps:
[0032] (1) Etching of Ti3C2: Take 1.00 g of Ti3AlC2 raw material, slowly add 20 mL of 40% hydrofluoric acid in batches, stir at room temperature for 48 h, centrifuge at 3000 r / min for 30 min, wash to pH 6, and dry for 24 h;
[0033] (2) Weigh 9.5 mg of Ti3C2 and dissolve it in 20 mL of ethanol. Stir well and add 0.95 g of BiCl3 to completely dissolve it.
[0034] (3) 15 mL of 1.0 mol / L NaOH solution was added to the above solution, stirred for 3 h, reacted in a reactor at 120 °C for 12 h, centrifuged, washed with deionized water until neutral, and the washed solid was vacuum dried at 60 °C for 12 h to obtain Bi 12 O 17 Cl2-1%Ti3C2. Example 2
[0035] A kind of Bi 12 O 17 The preparation method of Cl2-Ti3C2 composite photocatalyst comprises the following steps:
[0036] (1) Etching of Ti3C2: Take 1.00 g of Ti3AlC2 raw material, slowly add 20 mL of 40% hydrofluoric acid in batches, stir at room temperature for 24 h, centrifuge at 3000 r / min for 30 min, wash to pH 6, and dry for 12 h;
[0037] (2) Weigh 19.0 mg of Ti3C2 and dissolve it in 45 mL of ethanol. Stir well and add 0.95 g of BiCl3 to completely dissolve it.
[0038] (3) Add 20 mL of 1.0 mol / L NaOH solution to the above solution, stir for 1 h, react in a reactor at 120 °C for 1 h, centrifuge, wash with deionized water until neutral, and vacuum dry the washed crystals at 60 °C for 12 h to obtain Bi 12 O 17 Cl2-2%Ti3C2. Example 3
[0039] A kind of Bi 12 O 17 The preparation method of Cl2-Ti3C2 composite photocatalyst comprises the following steps:
[0040] (1) Etching of Ti3C2: Take 1.00 g of Ti3AlC2 raw material, slowly add 20 mL of 40% hydrofluoric acid in batches, stir at room temperature for 72 h, centrifuge at 3000 r / min for 30 min, wash to pH 6, and dry for 36 h;
[0041] (2) Weigh 47.5 mg of Ti3C2 and dissolve it in 15 mL of ethanol. Stir well and add 0.95 g of BiCl3 to completely dissolve it.
[0042] (3) 45 mL of 1.0 mol / L NaOH solution was added to the above solution, stirred for 6 h, reacted in a reactor at 120 °C for 24 h, centrifuged, washed with deionized water until neutral, and the washed solid was vacuum dried at 60 °C for 12 h to obtain Bi 12 O 17 Cl2-5%Ti3C2. Example 4
[0043] A kind of Bi 12 O 17 The preparation method of Cl2 / Ti3C2 composite photocatalyst comprises the following steps:
[0044] (1) Etching of Ti3C2: Take 1.00 g of Ti3AlC2 raw material, slowly add 20 mL of 40% hydrofluoric acid in batches, stir at room temperature for 48 h, centrifuge at 3000 r / min for 30 min, wash to pH 6, and dry for 24 h;
[0045] (2) Weigh 95.0 mg of Ti3C2 and dissolve it in 30 mL of ethanol. Stir well and add 0.95 g of BiCl3 to completely dissolve it.
[0046] (3) 15 mL of 1.0 mol / L NaOH solution was added to the above solution, stirred for 4 h, reacted in a reactor at 120 °C for 20 h, centrifuged, washed with deionized water until neutral, and the washed solid was vacuum dried at 60 °C for 12 h to obtain Bi 12 O 17 Cl2-10%Ti3C2. Example 5
[0047] A kind of Bi 12 O 17 The preparation method of Cl2 / Ti3C2 composite photocatalyst comprises the following steps:
[0048] (1) Etching of Ti3C2: Take 1.00 g of Ti3AlC2 raw material, slowly add 20 mL of 40% hydrofluoric acid in batches, stir at room temperature for 48 h, centrifuge at 3000 r / min for 30 min, wash to pH 6, and dry for 24 h;
[0049] (2) Weigh 190.0 mg of Ti3C2 and dissolve it in 30 mL of ethanol. Stir well and add 0.95 g of BiCl3 to completely dissolve it.
[0050] (3) 15 mL of 1.0 mol / L NaOH solution was added to the above solution, stirred for 4 h, reacted in a reactor at 120 °C for 20 h, centrifuged, washed with deionized water until neutral, and the washed solid was vacuum dried at 60 °C for 12 h to obtain Bi 12 O 17 Cl2-20%Ti3C2.
[0051] 2. Bi prepared by the present invention 12 O 17 Test and Analysis of Cl2-Ti3C2 Composite Photocatalyst
[0052] 2.1) X-ray powder diffraction test (XRD)
[0053] The sample phase was analyzed using the XRD-6100 X-ray diffraction analyzer from Shimadzu Corporation, Japan. The test conditions were: X-ray tube Cu target (λ=0.154056nm), tube current 40mA and tube voltage 40kV, scanning range 5-80°, and scanning speed 4° / min. The sample was ground into powder suitable for diffraction experiments, then the sample powder was placed in the XRD sample aluminum slot, pressed into a test piece with a very flat surface, and installed on the instrument for testing under the above conditions. The results are as follows: Figure 1 As shown in the figure, we can see that Bi 12 O 17 Cl2 characteristic peaks (115), (117) and (200), which indicates that Bi 12 O 17 Cl2 was successfully prepared. The test results of the original Ti3C2 also showed that the aluminum layer (Al) in Ti3AlC2 was successfully etched to obtain a multilayered Ti3C2. In the prepared composite materials with different proportions, the peak of Ti3C2 was not obvious, which may be due to its small amount, while Bi 12 O 17 The peak of Cl2 is obvious, which indicates that the surface composite material is successfully prepared.
[0054] 2.2) Scanning electron microscope test (SEM)
[0055] The prepared composite photocatalyst was tested by field emission scanning electron microscope (SEM) Hitachi SU8220. The specific operation was as follows: a small amount of powder sample was added to ethanol, dispersed evenly, and then dripped onto a silicon wafer for testing, and different magnifications were adjusted. The results are shown in Figure 2. Figure 2 As shown, Ti3C2 is a multilayer structure, Bi 12 O 17 Cl2 is a flake structure with a large size; Ti3C2-Bi 12 O 17 Cl2 all have flake structures, but the sizes vary. 12 O 17 Cl2-5%Ti3C2 was tested by X-ray energy dispersive spectrometer (EDS), which confirmed that it contained Ti, C, Bi, O, Cl and other elements. The results of element mapping showed that in Bi 12 O 17 The elements in the Cl2-5%Ti3C2 composite material are evenly distributed. Figure 3 shown.
[0056] 2.3) Transmission electron microscopy (TEM)
[0057] A 2100F transmission electron microscope (Japan, JEOL) was used. The samples to be tested were fully ground in a mortar before testing, so that the sample particles could be as small as possible. Then, ethanol was added to the ground samples and ultrasonically dissolved for about 30 minutes. The evenly dispersed mixed solution was then added to the copper mesh using a pipette and dried under an infrared lamp for 30 minutes to obtain the samples required for the test. The test voltage was 200 KV. The results are shown in Figure 2. Figure 4 As shown in the figure, it can be seen that Bi 12 O 17 The Cl2-5%Ti3C2 composite photocatalyst contains Ti3C2 and Bi 12 O 17 Cl2.
[0058] 2.4) X-ray Photoelectron Spectroscopy (XPS)
[0059] The instrument model used was ThermoScientific Escalab250Xi AI Ka target (hv=1486.6eV), power 150W, sensitivity 350keps, and analysis chamber vacuum degree 10 -8 mbar. The angle between the detector and the sample surface is 90°, and the analysis area is 700*300um. The results are as follows Figure 5 As shown in the figure, it can be seen that Bi 12 O 17 Elements such as Bi, O, Ti, C and Cl exist in the Cl2-Ti3C2 composite photocatalyst.
[0060] 2.5) Ultraviolet visible diffuse reflectance spectroscopy test (UV-vis DRS)
[0061] The UV-vis DRS analysis test uses a UV-2550 UV-visible spectrometer (Shimadzu, Japan). Before the sample is tested, barium sulfate (BaSO4) must be used as a reference to subtract the background. Under the UV-vis DRS analysis test, the light response of the sample to be tested under different wavelengths of light can be obtained, and then the sample to be tested can be analyzed. Figure 6 For different doping amounts of Bi 12 O 17 The UV-visible diffuse reflectance spectrum of Cl2-Ti3C2 composite photocatalyst shows that Ti3C2 has absorption in the entire band, Bi 12 O 17 Cl2 has the worst light absorption performance, and the light absorption increases with the increase of Ti3C2 proportion. Figure 6 The calculated structure of the energy bands shows that Bi 12 O 17The band gap of Cl2 is 2.71eV, Ti3C2 is 1.05eV, and Bi 12 O 17 The band gap of Cl2-5%Ti3C2 is 2.51eV, and the band gap has become smaller.
[0062] 2.6) Photoelectric performance test
[0063] Experimental conditions: The photocurrent was tested using a CHI 660D electrochemical workstation. A three-electrode system was used, with Ag / AgCl electrode and Pt electrode as the reference electrode and counter electrode respectively. The sample was evenly dispersed and then dropped onto 1cm × 2cm fluorine-doped tin oxide (FTO) as the working electrode. The lingt 300 from Porphyra was used as the light source, and the electrolyte solution was a 0.2 M (mole per liter) Na2SO4 solution. At room temperature, the photocurrent of different samples was tested under open circuit voltage in dark and illuminated conditions. The results are shown in the figure. Figure 8 As shown: Photocurrent test shows that Bi 12 O 17 Cl2-5%Ti3C2 has the largest photocurrent, achieving the most effective separation of its photogenerated electrons and holes, so its photodegradation efficiency is the best.
[0064] 3. Application of the prepared composite photocatalyst for degradation of tetracycline hydrochloride
[0065] 3.1) The degradation performance of tetracycline hydrochloride was studied under irradiation with a 300 W xenon lamp (UV was filtered out, HV>420 nm).
[0066] The concentration of tetracycline hydrochloride is 20 mg / / L. Take 100 ml of tetracycline hydrochloride and add it to a 100 ml beaker. Add 20 mg of catalyst and add a magnet for magnetic stirring. The stirring rate is 500 r / min. Adsorb for 30 minutes in the dark before the photodegradation experiment. The total illumination time is 1 hour. Sampling is performed every 10 minutes, and 3 mL is taken each time. The obtained solution is filtered with an aqueous 0.22μm filter head, and the absorbance of the solution is tested using UV-vis spectroscopy. The characteristic absorption peak of tetracycline hydrochloride is at 357nm, so its absorbance value is detected at 357 nm. The results are as follows: Fig. 9 As shown, the composite photocatalyst 5% Ti3C2-Bi 12 O 17 Cl2 performed best, with a degradation rate of 62%, while pure Bi 12 O 17 The degradation rate of Cl2 is only 36%, and the 12 O 17 Cl2-5%Ti3C2 is pure Bi 12 O 17Cl2 is 1.7 times. According to ln(C0 / C)=kt, the first-order photodynamic constant k is calculated, Bi 12 O 17 The first-order photodynamic constant of Cl2-5%Ti3C2 is also the largest.
[0067] 3.2) Conduct free radical capture experiments under conditions equivalent to those for the photodegradation of tetracycline hydrochloride.
[0068] Under the condition of 300 W xenon lamp visible light (UV filtered, HV>420 nm), tetracycline hydrochloride concentration was 20 mg / / L, 100 ml tetracycline hydrochloride was added to a 100 ml beaker, 20 mg catalyst was added, various capture agents (isopropanol, sodium oxalate and benzoquinone concentration were 5.0 mM) were added as ·OH h + and O 2- The capture agent. A magnetic particle was added for magnetic stirring at a rate of 500 revolutions per minute. The adsorption was carried out in the dark for 30 minutes before photodegradation. The total illumination time was 1 hour. Samples were taken every 10 minutes, and 3 mL was taken each time. The solution was filtered with a 0.22 μm aqueous filter head, and the absorbance of the solution was tested using UV-vis spectroscopy. The characteristic absorption peak of tetracycline hydrochloride is at 357 nm, so its absorbance value was detected at 357 nm. Fig.11 for Bi 12 O 17 The photodegradation effect diagram of Cl2-5%Ti3C2 composite photocatalyst with different capture agents is shown in the figure: the addition of isopropanol and sodium oxalate has little effect, while the addition of benzoquinone significantly reduces its degradation efficiency, indicating that its active free radical is superoxide free radical (·O 2- ).
[0069] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A Bi 12 O 17 Cl 2 -Ti 3 C 2 Preparation method of composite photocatalyst, It is characterized in that The steps include: (1) Ti 3 C 2 Etching: Take 1.00 g of Ti 3 AlC 2 Raw materials, slowly add 20 mL of hydrofluoric acid in batches, stir at room temperature for 24-72 h, centrifuge at 3000 r / min for 30 min, wash until pH is 6, and dry for 12-36 h; (2) Weigh a certain amount of Ti 3 C 2 Dissolve in 15-45 mL of ethanol, stir well, and add 0.95 g of BiCl 3 Completely dissolved; the Ti 3 C 2 The doping amount is BiCl 3 0-10% of mass; (3) Add 15-45 mL of NaOH solution to the above solution, stir for 1-6 h, react in a reactor at 120 °C for 1-24 h, centrifuge, wash with deionized water until neutral, and dry.
2. Bi according to claim 1 12 O 17 Cl 2 -Ti 3 C 2 Preparation method of composite photocatalyst, It is characterized in that The mass concentration of the hydrofluoric acid in step (1) is 40%.
3. Bi according to claim 1 12 O 17 Cl 2 -Ti 3 C 2 Preparation method of composite photocatalyst, It is characterized in that The mass concentration of the NaOH solution in step (3) is 1.0 mol / L.
4. Bi according to claim 1 12 O 17 Cl 2 -Ti 3 C 2 Preparation method of composite photocatalyst, It is characterized in that The drying in step (3) refers to vacuum drying the washed solid at 60° C. for 12 h.
5. A Bi 12 O 17 Cl 2 -Ti 3 C 2 Application of composite photocatalysts, It is characterized in that Bi prepared by any one of the methods of claims 1 to 4 12 O 17 Cl 2 -Ti 3 C 2 Application of composite photocatalyst in degradation of tetracycline hydrochloride.
Citation Information
Patent Citations
Preparation method for bismuth oxychloride photocatalyst and application of bismuth oxychloride photocatalyst to degradation of sulfamethazine
CN107376949A