A multi-structural composite material snowmobile mold and a snowmobile preparation method

By designing the mold and laying process for snowmobile for multi-structure feature composite materials, the problems of low production efficiency of snowmobile, high manual labor intensity and difficult product quality stability are solved, and high-quality integrated molding of snowmobile body is achieved and Improved stability and reliability.

CN114953499BActive Publication Date: 2024-11-29AEROSPACE RES INST OF MATERIAL & PROCESSING TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210107599.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-28
Publication Date
2024-11-29
Estimated Expiration
2042-01-28

AI Technical Summary

Technical Problem

In the production of multi-structure feature composite snowmobile, the existing technology has problems such as low production efficiency, high manual labor intensity, and difficult to control product quality stability, especially the laying positioning, narrow and long double wing pressing and multiple folds after forming. Technical problems such as rubber leaning.

Method used

A multi-structure characteristic composite material snowmobile mold, including female mold, thickening zone auxiliary positioning mold and silicone rubber soft mold, is used to design the laying process and reasonable pre-compression and curing process to solve the problem of product forming after product forming. Technical problems such as multiple folds and glue leanness.

Benefits of technology

The high-quality integrated molding of the multi-structure characteristic composite snow car body has been achieved, which improves the appearance and internal quality of the product, solves the problems of pressurization and laying positioning of the narrow and long wings, and improves the stability and reliability of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114953499B_ABST
    Figure CN114953499B_ABST
Patent Text Reader

Abstract

The present invention discloses a mold for a multi-structural feature composite snowmobile and a method for preparing the snowmobile. The mold includes a female mold, a thickening area auxiliary positioning mold and a silicone rubber soft mold. The preparation method is: first, the main body prepreg is repeatedly layered in the female mold until the difference between the total layer thickness and the predetermined thickness of the snowmobile main body is 1mm to 1.5mm; then the thickening area prepreg is made into a stacking block, and after the thickening area auxiliary positioning mold is used to locate the corresponding position of the thickening area, the stacking block is used for layering; then the main body prepreg is layered until the total thickness is equal to the predetermined thickness of the snowmobile main body; finally, the silicone rubber soft mold is placed in the double-wing cavity, cured, and the snowmobile is obtained after demolding. The present invention solves the technical problems of multiple wrinkles and poor glue after product molding through the design of the snowmobile molding mold, the multi-structural feature layering process design, and the reasonable pre-compacting and curing process, improves the appearance and internal quality of the product, and realizes the high-quality integrated molding of the multi-structural feature composite snowmobile body.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a multi-structural feature composite material snowmobile mould and a preparation method thereof, belonging to the field of composite materials and processes. Background Art

[0002] Advanced composite materials have the advantages of light weight, high strength, structural integrity, versatility and designability, and are widely used in aviation, aerospace, shipbuilding and other fields. With the development of science and technology, the application of advanced composite materials has extended to the field of high-end sports equipment, which can help athletes improve their performance.

[0003] As one of the high-end sports equipment, bobsleigh (also known as snowmobile) is very similar to a "rocket" on ice. In order to increase the sliding speed of the snowmobile, the snowmobile is required to have a more excellent aerodynamic shape and a lighter body.

[0004] At present, foreign countries have adopted fiber-reinforced composite materials to make snowmobile bodies. However, the hand lay-up process used has the disadvantages of low production efficiency, high labor intensity of manual operation, poor working environment conditions, etc., and the product quality stability is difficult to control, which seriously affects its reliability.

[0005] The domestic aerospace materials and technology research institute has adopted high-end fiber-reinforced composite materials and advanced molding technology to develop the first domestic composite two-person bobsleigh. In order to further improve the performance and reliability of the bobsleigh, it is urgent to solve the technical problems of multi-structural composite bobsleigh layer positioning, narrow and long double-wing pressurization, and multiple wrinkles and poor glue after product molding through mold design optimization, layer structure design and reasonable molding process, improve the appearance and internal quality of the product, realize high-quality integrated molding of the multi-structural composite bobsleigh body, and improve its stability and reliability. Summary of the invention

[0006] The object of the present invention is to overcome the above-mentioned defects and provide a multi-structural feature composite snowmobile mold and a snowmobile preparation method, wherein the snowmobile mold comprises a female mold, a thickening area auxiliary positioning mold and a silicone rubber soft mold; the female mold is provided with a molding cavity corresponding to the shape of the snowmobile main body, and the molding cavity comprises a body cavity and a double-wing cavity; the thickening area auxiliary positioning mold is used to perform shape-following positioning in the female mold according to the shape of the thickening area; the shape of the silicone rubber soft mold corresponds to the double-wing cavity of the female mold, and after the silicone rubber soft mold is placed in the double-wing cavity, it expands when cured under vacuum conditions to achieve the molding of the double wings; the snowmobile preparation method comprises: (1) cutting hot-melt prepreg according to the three-dimensional model of the snowmobile to obtain prepregs corresponding to the sizes of the snowmobile main body and the thickening area, which are respectively recorded as main body prepreg and thickening area prepreg; (2) using the main body prepreg to repeatedly lay layers in the female mold, Until the difference between the total thickness of the layers and the predetermined thickness of the snowmobile body is 1mm to 1.5mm; (3) The thickening area prepreg is layered to obtain a thickening area block with a thickness of 0.8mm to 2mm, and the thickening area block is vacuumed and pre-compacted; (4) The thickening area auxiliary positioning mold is used to locate the corresponding position of the thickening area in the female mold, and the thickening area block obtained in step (3) is layered at the corresponding position of the thickening area until the total thickness of the layers is equal to the predetermined thickness of the thickening area; (5) The main body prepreg is used to repeatedly layer in the female mold until the total thickness of the layers is equal to the predetermined thickness of the snowmobile body; (6) A silicone rubber soft mold is placed in the double-wing cavity of the female mold, and the female mold is wrapped with isolation material, breathable material and vacuum bag in turn, and then cured under vacuum conditions; (7) The product is demoulded and polished to obtain a multi-structural feature composite snowmobile. The present invention solves the technical problems of multiple wrinkles and glue deficiency after product molding through the design of a multi-structural feature composite material snowmobile molding mold, multi-structural feature layup process design, and reasonable pre-compacting and curing processes, thereby improving the appearance and internal quality of the product and achieving high-quality integrated molding of a multi-structural feature composite material snowmobile body.

[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0008] A method for preparing a composite snowmobile with multiple structural features, using a composite snowmobile mold with multiple structural features, wherein the snowmobile mold includes a female mold, a thickened area auxiliary positioning mold, and a silicone rubber soft mold;

[0009] The female mold is provided with a molding cavity corresponding to the shape of the snowmobile body, and the molding cavity includes a body cavity and a double-wing cavity; the thickened area auxiliary positioning mold is used to perform shape-following positioning in the female mold according to the shape of the thickened area; the shape of the silicone rubber soft mold corresponds to the double-wing cavity of the female mold, and after the silicone rubber soft mold is placed in the double-wing cavity, it expands when solidified under vacuum conditions to achieve the molding of the double wings;

[0010] The preparation method of the composite snowmobile with multiple structural features comprises the following steps:

[0011] (1) Cutting hot-melt prepreg according to the three-dimensional model of the snowmobile to obtain prepregs corresponding to the sizes of the snowmobile body and the thickened area, which are respectively recorded as the body prepreg and the thickened area prepreg;

[0012] (2) Repeatedly layering the main body prepreg in the female mold until the difference between the total layer thickness and the predetermined thickness of the snowmobile body is 1 mm to 1.5 mm;

[0013] (3) Laying the prepreg in the thickened area to obtain a thickened area block material with a thickness of 0.8 mm to 2 mm, and vacuuming and pre-compacting the thickened area block material;

[0014] (4) using the thickening area auxiliary positioning mold to locate the corresponding position of the thickening area in the female mold, and using the thickening area block material obtained in step (3) to lay layers at the corresponding position of the thickening area until the total thickness of the layers is equal to the predetermined thickness of the thickening area;

[0015] (5) Repeatedly layer the main body prepreg in the female mold until the total layer thickness is equal to the predetermined thickness of the snowmobile body;

[0016] (6) placing a silicone rubber soft mold in the double-wing cavity of the female mold, wrapping the female mold with an isolation material, a breathable material, and a vacuum bag in sequence, and curing the mold under vacuum conditions;

[0017] (7) The product is demolded and polished to obtain a composite snowmobile with multiple structural features.

[0018] Furthermore, in step (1) of the preparation method, the thickness of the obtained main body prepreg and thickened area prepreg is 0.1 mm to 0.3 mm;

[0019] The main body prepreg includes carbon fiber reinforced hot melt prepreg and glass fiber reinforced hot melt prepreg, or carbon fiber reinforced hot melt prepreg and aramid fiber reinforced hot melt prepreg.

[0020] Furthermore, in step (2) of the preparation method, in the hybrid structure obtained by repeatedly layering the main prepreg in the female mold, the volume ratio of the carbon fiber reinforced prepreg is 50% to 80%.

[0021] Furthermore, in step (2) of the preparation method, when the main prepreg is repeatedly layered in the female mold, the main prepreg corresponding to the structural mutation area in the female mold is cut and removed, and an independent mutation area prepreg is used to layer the structural mutation area, and the mutation area prepreg is connected to the adjacent main prepreg in an overlapping manner, with an overlapping width of 20 mm to 50 mm.

[0022] Furthermore, in the step (3) of the preparation method, the temperature during vacuum pre-compaction of the thickened area stack is 50°C to 90°C, and the heat preservation time is 30min to 90min;

[0023] In the steps (2) and (5), after each layer of prepreg with a thickness of 0.5 mm to 2 mm is laid, glue suction and compaction are performed, and the conditions for glue suction and compaction are: temperature 50° C. to 90° C., insulation time 30 min to 90 min, and pressure 0.3 MPa to 0.7 MPa.

[0024] Furthermore, in steps (3) and (4) of the preparation method, the prepreg in the thickening area is laid out in a staggered laying process, and the size of each layer is reduced in the order of laying. Each thickening area layer is surrounded by an inclined surface relative to the corresponding position of the thickening area positioned in the female mold, and the inclination angle of the inclined surface is 10° to 60°.

[0025] Furthermore, the inclination angle of the inclined surface in the preparation method is β=arctan(m / v), wherein m is the thickness of the prepreg in the thickened area, and v is the staggered velocity.

[0026] Furthermore, in step (6) of the preparation method, the process parameters for curing under vacuum conditions are: at a pressure of 0.5MPa to 1.0MPa, heating to 100°C to 250°C at a heating rate of 5°C / h to 40°C / h, keeping temperature for 2h to 8h, and then cooling to 40°C to 70°C at a cooling rate of <30°C / h.

[0027] A composite snowmobile mold with multiple structural features, comprising a female mold, a thickened area auxiliary positioning mold and a silicone rubber soft mold;

[0028] The female mold is provided with a molding cavity corresponding to the shape of the snowmobile body, and the molding cavity includes a body cavity and a double-wing cavity;

[0029] The material used for the auxiliary positioning mold of the thickened area is a flexible or semi-rigid material, which is used to perform conformal positioning in the female mold according to the shape of the thickened area; the shape of the silicone rubber soft mold corresponds to the double-wing cavity of the female mold. After the silicone rubber soft mold is placed in the double-wing cavity, it expands during curing under vacuum conditions to achieve the molding of the double wings.

[0030] Furthermore, the molding surface of the body cavity is provided with a positioning score line groove, the positioning score line groove has a width of 0.2mm to 0.5mm and a depth of 0.2mm to 0.5mm, and is used to form positioning score lines on the outer surface of the snowmobile body, and the positioning score lines are used for assembling the snowmobile with other external devices.

[0031] Furthermore, the single-point expansion amount of the silicone rubber soft mold is X=Hα, where H is the height of the double-wing cavity and α is the thermal expansion coefficient of the silicone rubber material.

[0032] Compared with the prior art, the present invention has at least one of the following beneficial effects:

[0033] (1) The present invention innovatively designs a method for preparing a composite snowmobile with multiple structural features. Through the design of the layering process combined with a reasonable pre-compacting and curing process, the technical problems of multiple wrinkles and lack of glue after product molding are solved, and the high-quality integrated molding of the composite snowmobile body with multiple structural features is achieved;

[0034] (2) The present invention selects the type and proportion of prepreg to form a multi-phase hybrid impact-resistant ply structure. In particular, the carbon fiber reinforced prepreg of the hybrid structure of the snowmobile main body ply accounts for 50%-80%, which can make the snowmobile have good impact resistance while meeting the requirements of light weight and high strength;

[0035] (3) The present invention designs a mold for a composite snowmobile with multiple structural features based on the structural characteristics and streamlined requirements of the composite snowmobile with multiple structural features. The narrow and long wings use a variable expansion silicone rubber soft mold, which can effectively solve the problem of uniform pressurization of the narrow and long wings of the snowmobile. The auxiliary positioning mold of the thickened area is a conformal design, which can quickly and accurately position the ply of the thickened area of ​​the snowmobile. The female mold is provided with a positioning groove to ensure the high-quality preparation of the product and the subsequent smooth assembly with external devices such as the frame.

[0036] (4) The present invention continuously layers the flat part of the snowmobile body, overlaps the layers in the structural mutation areas such as the special-shaped frame and the narrow and long double wings, and adopts stacked blocks and staggered layers in the thickened area, which solves the technical problems of multiple wrinkles, lack of glue, defects, etc. after the product is formed, and improves the appearance and internal quality of the product;

[0037] (5) The preparation method of the present invention is stable and reliable, and has strong applicability;

[0038] (6) The two-person bobsleigh and four-person bobsleigh products prepared by the method of the present invention have smooth surfaces, meet the aerodynamic shape requirements of the products, have internal defects of less than 1%, and have stable and reliable product quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 A schematic diagram of the structure of a composite material snowmobile with structural characteristics according to an embodiment of the present invention;

[0040] Figure 2 It is a schematic diagram of the female mold in the mold of the composite material snowmobile with multiple structural characteristics of the present invention;

[0041] Figure 3 It is a schematic diagram of a typical thickened area auxiliary positioning mold in a multi-structural feature composite material snowmobile mold of the present invention;

[0042] Figure 4 It is a schematic diagram of a silicone rubber soft mold casting mold for making a silicone rubber soft mold in a mold for a multi-structural feature composite material snowmobile of the present invention;

[0043] Figure 5 This is a flow chart of a method for preparing a composite snowmobile with multiple structural features according to the present invention. DETAILED DESCRIPTION

[0044] The following detailed description of the present invention will make the features and advantages of the present invention more clear and explicit.

[0045] The word "exemplary" is used exclusively herein to mean "serving as an example, embodiment, or illustration." Any embodiment described herein as "exemplary" is not necessarily to be construed as preferred or advantageous over other embodiments. Although various aspects of the embodiments are shown in the drawings, the drawings are not necessarily drawn to scale unless otherwise noted.

[0046] A multi-structure feature composite material snowmobile mold and a preparation method thereof, such as Figure 2 , Figure 3 and Figure 4 The molding molds used include a female molding mold, a thickening area auxiliary positioning mold and a silicone rubber soft mold, wherein the silicone rubber soft mold is made by using a narrow and long double-wing silicone rubber soft mold casting mold.

[0047] like Figure 5 The specific preparation method of the multi-structure characteristic composite material snowmobile includes the following steps:

[0048] (1) Assemble the female mold for molding and raise the female mold to a certain height to facilitate the laying operation;

[0049] (2) Using hot melt prepreg, accurately calculate the material size of the ply according to the three-dimensional model of the product, and use automatic unloading equipment to accurately cut the material;

[0050] (3) using the hot-melt prepreg cut in step (2) to lay the main body of the snowmobile;

[0051] (4) Repeat step (3) until the difference between the total thickness of the ply and the predetermined thickness of the snowmobile body is 1 mm to 1.5 mm;

[0052] (5) Using the hot-melt prepreg cut in step (2) to lay the thickened area stacking blocks, the stacking block thickness is designed to be 0.8 mm to 2 mm;

[0053] (6) vacuum pre-compacting the thickened area blocks in step (5);

[0054] (7) The stacked blocks pre-compacted in step (6) are used to lay the thickened area, and the position of the thickened area is positioned using an auxiliary positioning mold.

[0055] (8) Repeat step (3) to complete the plying of the remaining 1 mm to 1.5 mm thick ply;

[0056] (9) A silicone rubber soft mold is placed in the double-wing cavity of the female mold, and the female mold is sequentially covered with an isolation material, a breathable material, and a vacuum bag, and then vacuumed and cured.

[0057] (10) After curing, the product is demolded and partially polished to remove edge burrs, completing the preparation of the multi-structural feature composite snowmobile.

[0058] In a preferred embodiment, in step (1), the female mold is raised to a height of 30-70 cm.

[0059] In a preferred embodiment, in step (3), the main body prepreg is cut at the structural mutation areas such as the edges of the double-wing cavity of the female mold and the protrusion of the front pusher mold, and then covered with a separate hot-melt prepreg. The prepreg is connected to the adjacent main body prepreg in an overlapping manner with an overlapping width of 20mm-50mm.

[0060] In a preferred embodiment, in step (6), the pre-compacting temperature is 50°C to 90°C, and the holding time is 30min to 90min.

[0061] In a preferred embodiment, the female mold molding surface has a mounting block positioning groove, the groove width is 0.2mm-0.5mm, and the depth is 0.2mm-0.5mm.

[0062] In a preferred embodiment, the silicone rubber soft mold adopts a variable expansion design based on the double-wing cavity structure, and the single-point expansion X=Hα, where H is the height of the double-wing cavity and α is the thermal expansion coefficient of the silicone rubber material.

[0063] In a preferred embodiment, the thickened area auxiliary positioning mold is made of flexible or semi-rigid material to facilitate conformal positioning.

[0064] In a preferred embodiment, the position of the thickening area in the auxiliary positioning mold for the thickening area is set based on the female mold forming 0 layer, that is, the positioning structure of the auxiliary positioning mold for the thickening area is designed based on the structural characteristics of the female mold when no layer is laid; when the auxiliary positioning mold is used to position the thickening area, the position needs to be adjusted according to the thickness of the layer material.

[0065] In a preferred embodiment, the hot-melt prepreg obtained in step (2) has a thickness of 0.1 mm to 0.3 mm.

[0066] In a preferred embodiment, the snowmobile body laminate structure is a carbon fiber / glass fiber hybrid structure or a carbon fiber / aramid fiber hybrid structure.

[0067] In a preferred embodiment, the volume proportion of the hybrid structure carbon fiber reinforced prepreg of the snowmobile body ply is 50% to 80%.

[0068] In a preferred embodiment, the plies in the thickened area are laid using a staggered laying process to ensure that an inclination angle β is formed in the circumferential direction after laying, β=arctan(m / v), and the range of β is 10° to 60°.

[0069] In a preferred embodiment, in steps (3), (4) and (8), glue suction and compaction are performed every time a thickness of 0.5 mm to 2 mm is completed, the glue suction temperature is 50° C. to 90° C., the insulation time is 30 min to 90 min, and the pressure is 0.3 MPa to 0.7 MPa.

[0070] In a preferred embodiment, the vacuum curing conditions in step (9) are: under a pressure of 0.5MPa to 1.0MPa, heating to 100°C to 250°C at a heating rate of 5°C / h to 40°C / h, keeping the temperature for 2h to 8h, and then cooling to 40°C to 70°C, with a cooling rate of <30°C / h.

[0071] Embodiment 1:

[0072] like Figure 1In this embodiment, the two-man snowmobile structure includes a snowmobile body and a thickening area, wherein the snowmobile body includes a vehicle wall, a special-shaped end frame 1 for the docking interface, anti-collision wings 2, a front pusher recessed area 3, and the thickening area includes an opening thickening area 8, a mounting block thickening area 5, a side wall reinforcement thickening area 6, and a rear pusher thickening area 7. Among them, the thickness of the vehicle wall of the snowmobile body is 3mm, the special-shaped end frame 1 for the docking interface, the anti-collision wings 2, and the front pusher recessed area 3 correspond to the structural mutation area of ​​the female mold, the thickness of the opening thickening area 8 and the side wall reinforcement thickening area 6 are both 6mm, the mounting block thickening area 5 is 8mm, and the rear pusher thickening area 7 is 10mm. The snowmobile body is prepared by using a single-layer carbon fiber reinforced hot-melt prepreg with a thickness of 0.15mm and a single-layer glass fiber reinforced hot-melt prepreg with a thickness of 0.25mm, and the carbon fiber reinforced hot-melt prepreg accounts for about 70%. The thickening area is prepared by using a single-layer carbon fiber reinforced hot-melt prepreg with a thickness of 0.15mm.

[0073] The implementation steps are as follows:

[0074] (1) Assemble the female mold for molding and raise the female mold to a height of 40 cm to facilitate the laying operation;

[0075] (2) Using hot melt prepreg, accurately calculate the material size of the ply according to the three-dimensional model of the product, and use automatic unloading equipment to accurately cut the material;

[0076] (3) Use the hot-melt prepreg cut in step (2) to lay the main body of the snowmobile. Cut the prepreg at the edges of the double-wing cavity of the mold, the protrusion of the front pusher mold, and other structural mutation areas. Use a separate hot-melt prepreg for cladding. The prepreg and the adjacent prepreg are overlapped to form a continuous overlap with a width of 20 mm. The main body of the snowmobile is laid with 14 layers of carbon fiber reinforced hot-melt prepreg and 4 layers of glass fiber reinforced hot-melt prepreg.

[0077] (4) Repeat step (3) until the remaining ply material has a thickness of 1 mm, that is, the difference between the total ply thickness of the snowmobile body and the predetermined thickness of the snowmobile body is 1 mm;

[0078] (5) Use the hot-melt prepreg cut in step (2) to lay the thickening area stacking blocks. The thickness of the thickening area stacking blocks is designed to be 1 mm, wherein 3 stacking blocks are made for each characteristic area of ​​the opening thickening area and the side wall reinforcement thickening area, 5 stacking blocks are made for each characteristic area of ​​the installation block thickening area, and 7 stacking blocks are made for each characteristic area of ​​the rear push handle thickening area. The staggered speed v = 0.15 mm / layer, β = 45°.

[0079] (6) The thickened area blocks in step (5) are pre-compacted by vacuum evacuation at a temperature of 50° C. for 30 minutes.

[0080] (7) The stacked blocks pre-compacted in step (6) are used to pave the thickened area. The position of the thickened area is positioned using an auxiliary positioning mold and the position is adjusted according to the thickness of the ply material, that is, the total thickness of the ply of the main body of the snowmobile.

[0081] (8) Repeat step (3) to complete the plying of the remaining 1 mm thickness, that is, repeat step (3) until the total plying thickness is equal to the predetermined thickness of the snowmobile body. During the entire plying process, glue suction and compaction are performed when the 7 layers of carbon fiber reinforced hot melt prepreg are completed, when the 4 layers of glass fiber reinforced hot melt prepreg are completed, and when the thickening area is completed. The glue suction temperature is 50°C, the insulation time is 30 minutes, and the pressure is 0.3MPa.

[0082] (9) Place a silicone rubber soft mold in the double-wing cavity of the female mold, cover it with isolation material, breathable material, and vacuum bag in sequence, evacuate, and cure. Under a pressure of 0.5 MPa, heat up to 120°C at a heating rate of 25±5°C / h, keep warm for 2 hours, then reduce to 60°C, with a cooling rate of <30°C / h.

[0083] (10) After the curing is completed, the product is demolded and partially polished to remove edge burrs, thereby completing the preparation of the composite two-person bobsleigh with multiple structural features.

[0084] Example 2

[0085] like Figure 1 In this embodiment, the four-person snowmobile includes a snowmobile body and a thickening area, wherein the snowmobile body includes a vehicle wall, a special-shaped end frame 1 of the docking interface, anti-collision wings 2, a front push handle recessed area 3 and a middle push handle special-shaped area 4, and the thickening area includes an opening thickening area 8, a mounting block thickening area 5, a side wall reinforcement thickening area 6 and a rear push handle thickening area 7. Among them, the thickness of the snowmobile body vehicle wall is 4mm, the thickness of the opening thickening area 8 and the side wall reinforcement thickening area 6 are both 6mm, the mounting block thickening area 5 is 8mm, and the rear push handle thickening area 7 is 12mm. It is prepared by using a carbon fiber reinforced hot-melt prepreg with a single layer thickness of 0.2mm and an aramid fiber reinforced hot-melt prepreg with a single layer thickness of 0.1mm, and the carbon fiber reinforced hot-melt prepreg accounts for about 75%. The thickening area is prepared by using a carbon fiber reinforced hot-melt prepreg with a single layer thickness of 0.2mm.

[0086] The implementation steps are as follows:

[0087] (1) Assemble the female mold for molding and raise the mold to a height of 50 cm to facilitate the laying operation;

[0088] (2) Using hot melt prepreg, accurately calculate the material size of the ply according to the three-dimensional model of the product, and use automatic unloading equipment to accurately cut the material;

[0089] (3) The hot-melt prepreg cut in step (2) is used to lay the main body of the snowmobile. The prepreg is cut at the edges of the double-wing cavity of the mold and the protrusion of the front pusher mold, and a separate hot-melt prepreg is used for cladding. The prepreg and the adjacent prepreg are overlapped to form a continuous overlap with a width of 50 mm. The main body of the car body is laid with 15 layers of carbon fiber reinforced hot-melt prepreg and 10 layers of aramid fiber reinforced hot-melt prepreg.

[0090] (4) Repeat step (3) until the remaining ply material has a thickness of 1 mm, that is, the difference between the total ply thickness of the snowmobile body and the predetermined thickness of the snowmobile body is 1 mm;

[0091] (5) Use the hot-melt prepreg cut in step (2) to lay the thickening area stacking blocks. The thickness of the stacking blocks is designed to be 1 mm. Two stacking blocks are made in each characteristic area of ​​the opening thickening area and the side wall reinforcement thickening area, four stacking blocks are made in each characteristic area of ​​the installation block thickening area, and eight stacking blocks are made in each characteristic area of ​​the rear push handle thickening area. The staggered speed v = 0.25 mm / layer, β = 39°.

[0092] (6) The thickened area blocks in step (5) are pre-compacted by vacuum evacuation at a temperature of 60° C. for 40 minutes.

[0093] (7) The stacked blocks pre-compacted in step (6) are used to pave the thickened area. The position of the thickened area is positioned using an auxiliary positioning mold, and the position is adjusted according to the thickness of the pavement material, that is, the total thickness of the pavement of the snowmobile body.

[0094] (8) Repeat step (3) to complete the plying of the remaining 1 mm thickness, that is, repeat step (3) until the total plying thickness is equal to the predetermined thickness of the snowmobile body. During the entire plying process, glue suction and compaction are performed when 10 layers of carbon fiber reinforced hot melt prepreg are completed, 10 layers of aramid fiber reinforced hot melt prepreg are completed, and the thickening area is completed. The glue suction temperature is 60°C, the insulation time is 40 minutes, and the pressure is 0.4MPa.

[0095] (9) Place a silicone rubber soft mold in the double-wing cavity of the female mold, cover it with isolation material, breathable material, and vacuum bag in sequence, evacuate, and cure. Under a pressure of 0.6MPa, heat up to 180℃ at a heating rate of 25±5℃ / h, keep warm for 4h, then reduce to 70℃, with a cooling rate of <30℃ / h.

[0096] (10) After the curing is completed, the product is demolded and partially polished to remove edge burrs, thus completing the preparation of the composite four-person bobsleigh with multiple structural features.

[0097] The present invention optimizes and designs the pre-compacting process parameters and the curing process parameters through a large number of experiments, and adopts reasonable pre-compacting and curing processes to effectively ensure the quality and dimensional accuracy of the product; the product defect percentage is less than 1%.

[0098] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.

[0099] The contents not described in detail in the specification of the present invention belong to the common knowledge of those skilled in the art.

Claims

1. A method for preparing a composite snowmobile with multiple structural features, characterized in that: A multi-structure feature composite material snowmobile mold is used for molding, wherein the snowmobile mold comprises a female mold, a thickened area auxiliary positioning mold and a silicone rubber soft mold; The female mold is provided with a molding cavity corresponding to the shape of the snowmobile body, and the molding cavity includes a body cavity and a double-wing cavity; the thickened area auxiliary positioning mold is used to perform shape-following positioning in the female mold according to the shape of the thickened area; the shape of the silicone rubber soft mold corresponds to the double-wing cavity of the female mold, and after the silicone rubber soft mold is placed in the double-wing cavity, it expands when solidified under vacuum conditions to achieve the molding of the double wings; The preparation method of the composite snowmobile with multiple structural features comprises the following steps: (1) Cutting hot-melt prepreg according to the three-dimensional model of the snowmobile to obtain prepregs corresponding to the sizes of the snowmobile body and the thickened area, which are respectively recorded as the body prepreg and the thickened area prepreg; (2) Repeatedly layering the main body prepreg in the female mold until the difference between the total layer thickness and the predetermined thickness of the snowmobile body is 1 mm to 1.5 mm; (3) Laying the prepreg in the thickened area to obtain a thickened area block material with a thickness of 0.8 mm to 2 mm, and vacuuming and pre-compacting the thickened area block material; (4) using the thickening area auxiliary positioning mold to locate the corresponding position of the thickening area in the female mold, and using the thickening area block material obtained in step (3) to lay layers at the corresponding position of the thickening area until the total thickness of the layers is equal to the predetermined thickness of the thickening area; (5) Repeatedly layer the main body prepreg in the female mold until the total layer thickness is equal to the predetermined thickness of the snowmobile body; (6) placing a silicone rubber soft mold in the double-wing cavity of the female mold, wrapping the female mold with auxiliary materials, and curing under vacuum conditions; (7) After demolding the product, a composite snowmobile with multiple structural features is obtained; The main prepreg includes carbon fiber reinforced hot melt prepreg and glass fiber reinforced hot melt prepreg, or carbon fiber reinforced hot melt prepreg and aramid fiber reinforced hot melt prepreg; In the step (2), the volume ratio of the carbon fiber reinforced prepreg in the hybrid structure obtained by repeatedly layering the main prepreg in the female mold is 50% to 80%; The single-point expansion of the silicone rubber soft mold is X=Hα, where H is the height of the double-wing cavity and α is the thermal expansion coefficient of the silicone rubber material.

2. The method for preparing a composite snowmobile with multiple structural features according to claim 1, characterized in that: In the step (1), the thickness of the obtained main body prepreg and thickened area prepreg is 0.1 mm to 0.3 mm.

3. The method for preparing a composite snowmobile with multiple structural features according to claim 1, characterized in that: In the step (2), when the main body prepreg is repeatedly layered in the female mold, the main body prepreg corresponding to the structural mutation area in the female mold is cut and removed, and an independent mutation area prepreg is used to layer the structural mutation area, and the mutation area prepreg is connected to the adjacent main body prepreg in an overlapping manner, with an overlapping width of 20 mm to 50 mm.

4. The method for preparing a composite snowmobile with multiple structural features according to claim 1, characterized in that: In the step (3), the temperature of the thickened area stacked blocks during vacuum pre-compaction is 50°C to 90°C, and the heat preservation time is 30min to 90min; In the steps (2) and (5), after each layer of prepreg with a thickness of 0.5 mm to 2 mm is laid, glue suction and compaction are performed, and the conditions for glue suction and compaction are: temperature 50° C. to 90° C., insulation time 30 min to 90 min, and pressure 0.3 MPa to 0.7 MPa.

5. The method for preparing a composite snowmobile with multiple structural features according to claim 1, characterized in that: In the steps (3) and (4), the prepreg in the thickening area is laid out in a staggered laying process, and the size of each layer is reduced in the order of laying. The layers in each thickening area are surrounded by an inclined surface relative to the corresponding position of the thickening area in the female mold, and the inclination angle of the inclined surface is 10° to 60°.

6. The method for preparing a composite snowmobile with multiple structural features according to claim 5, characterized in that: The inclination angle β of the inclined surface is arctan (m / v), wherein m is the thickness of the prepreg in the thickened area, and v is the staggered velocity.

7. The method for preparing a composite snowmobile with multiple structural features according to claim 1, characterized in that: In the step (6), the process parameters for curing under vacuum conditions are: at a pressure of 0.5MPa to 1.0MPa, heating to 100°C to 250°C at a heating rate of 5°C / h to 40°C / h, keeping the temperature for 2h to 8h, and then cooling to 40°C to 70°C at a cooling rate of <30°C / h.

8. A mold for a multi-structural composite snowmobile, characterized in that: It includes a female mold, a thickening area auxiliary positioning mold and a silicone rubber soft mold; The female mold is provided with a molding cavity corresponding to the shape of the snowmobile body, and the molding cavity includes a body cavity and a double-wing cavity; The material used for the auxiliary positioning mold of the thickened area is a flexible or semi-rigid material, which is used to perform conformal positioning in the female mold according to the shape of the thickened area; the shape of the silicone rubber soft mold corresponds to the double-wing cavity of the female mold, and after the silicone rubber soft mold is placed in the double-wing cavity, it expands when solidified under vacuum conditions to achieve the molding of the double wings; The single-point expansion of the silicone rubber soft mold is X=Hα, where H is the height of the double-wing cavity and α is the thermal expansion coefficient of the silicone rubber material.

9. The multi-structural composite snowmobile mold according to claim 8, characterized in that: The molding surface of the body cavity is provided with a positioning score line groove, the width of the positioning score line groove is 0.2mm~0.5mm, and the depth is 0.2mm~0.5mm, which is used to form a positioning score line on the outer surface of the snow vehicle body. The positioning score line is used for the assembly of the snow vehicle and other external devices.

Citation Information

Patent Citations

  • Semi-soft die used for assisting racing boat moulding and one shot forming technology for racing boat

    CN104494165A

  • Composite conical section forming die pressurized by using soft die

    CN112536946A