A method for enhanced leaching of vanadium from vanadium-titanium magnetite

Through the oxidation and roasting of vanadium titanium magnetite and calcium-based additives and the leaching treatment of acid-containing ammonium oxalate solution, combined with ammonia water to remove impurities, the problems of low vanadium recovery rate and difficulty in tailing treatment in vanadium titanium magnetite extraction process are solved. It realizes efficient vanadium extraction and comprehensive utilization of resources.

CN114959309BActive Publication Date: 2024-11-22INSTITUTE OF PROCESS ENGINEERING CHINESE ACADEMY OF SCIENCES +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202210629585.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-01
Publication Date
2024-11-22
Estimated Expiration
2042-06-01

AI Technical Summary

Technical Problem

The existing vanadium titanium magnetite vanadium extraction process has problems such as low vanadium recovery rate, high impurity content, large energy consumption and difficult tailings treatment, especially high cost of high acidity or high salinity wastewater treatment, and the traditional method has better effect. Difference.

Method used

The oxidation and roasting of vanadium titanium magnetite and calcium-based additives are used, and the leaching treatment is performed using an acid-containing ammonium oxalate solution to produce a high-solubility vanadium oxalate, which improves the solubility and recovery of vanadium, and reduces the impurity content by removing impurities through ammonia water. Achieve efficient extraction of vanadium.

Benefits of technology

It improves the vanadium recovery rate and vanadium concentration of the leaching liquid, reduces the impurity content and energy consumption, and the tailings do not contain sodium salt, and can be directly mixed with ore and smelted to achieve the comprehensive utilization of vanadium titanium magnetite.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114959309B_ABST
    Figure CN114959309B_ABST
Patent Text Reader

Abstract

The present invention provides a method for enhanced leaching of vanadium from vanadium-titanium magnetite, the method comprising the following steps: (1) mixing vanadium-titanium magnetite and calcium-based additives, performing oxidative roasting, and obtaining roasted clinker; (2) leaching the roasted clinker with an acid-containing ammonium oxalate solution and performing solid-liquid separation to obtain a vanadium-containing liquid. The method has high vanadium recovery rate, high vanadium liquid concentration, and low leaching energy consumption. The vanadium-containing liquid obtained by leaching can be purified by impurity removal, providing favorable conditions for the preparation of high-purity vanadium pentoxide. Moreover, the vanadium extraction process of the present invention does not affect ironmaking, and the tailings after vanadium extraction do not contain sodium salt, and can be directly used for ironmaking, thereby realizing efficient and comprehensive utilization of vanadium-titanium magnetite resources.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of vanadium chemical metallurgy, and in particular to a method for enhanced leaching of vanadium from vanadium-titanium magnetite. Background Art

[0002] Currently, there are two main methods for extracting vanadium from iron concentrate. One is to extract vanadium from blowing slag after iron and steelmaking of vanadium-titanium magnetite; the other is to extract vanadium directly from vanadium-titanium magnetite concentrate.

[0003] Vanadium extraction from vanadium slag is the mainstream process for vanadium extraction from vanadium-titanium magnetite, that is, the process of sodium roasting-water leaching-purification-vanadium precipitation. Enterprises that use vanadium-titanium magnetite as raw materials to produce iron and vanadium products currently use the traditional vanadium slag sodium roasting process to extract vanadium. The basic principle of the sodium roasting process is to use Na2CO3 as an additive, and convert low-valent vanadium into water-soluble pentavalent vanadium sodium salt through high-temperature sodium roasting. Then, the sodium roasting product is directly leached in water to obtain a vanadium-containing leaching solution, and then ammonium salt is added to obtain ammonium polyvanadate precipitation. After reduction roasting, the vanadium oxide product is obtained. The sodium roasting process has a low vanadium recovery rate, and the vanadium recovery rate of a single roasting is about 70%. Due to the long process flow, the vanadium recovery of the entire process from vanadium-titanium magnetite to the final vanadium pentoxide is only 50%, resulting in a waste of vanadium resources.

[0004] Another method of extracting vanadium from vanadium-titanium magnetite is to extract vanadium directly from the ore. The advantage of this method is that the total recovery rate of vanadium is high, which can reach more than 60%. The most studied method of extracting vanadium directly from iron ore is sodium oxidation.

[0005] CN101168802A discloses a method for comprehensive recovery of iron, vanadium and titanium in vanadium-titanium magnetite concentrate, which uses sodium sulfate as a roasting additive, roasts at 1200-1300°C, extracts vanadium after roasting clinker water leaching, and reduces the tailings in a rotary furnace after pelletizing to recover molten iron and titanium slag. The disadvantages of this method are that the roasting temperature is high, the vanadium conversion rate is low, and the vanadium loss rate increases with the increase of vanadium content in the ore. The kiln tail gas produces harmful gas SO2, and the tailings contain sodium after leaching, so it cannot be used for ore blending and ironmaking, otherwise it will corrode the blast furnace lining.

[0006] CN102690944A proposes a method for comprehensive recovery of vanadium, titanium and iron in high-vanadium vanadium-titanium magnetite, firstly, adding any one of sodium salt or calcium salt to high-vanadium vanadium-titanium magnetite, roasting in a rotary hearth furnace and then leaching with acid, separating the leachate and residue, and obtaining vanadium products from the leachate; the tailings are made into reducing pellets, quickly reduced in a rotary hearth furnace, melted and separated in a gas melting furnace or an electric furnace to obtain vanadium-containing molten iron and titanium slag, the vanadium-containing molten iron is blown with oxygen in a converter to extract vanadium, vanadium slag and pig iron are separated, and the vanadium slag is crushed and returned to be mixed with high-vanadium vanadium-titanium magnetite for roasting and acid leaching to extract vanadium. This method combines vanadium extraction from vanadium-titanium magnetite with vanadium extraction from vanadium slag, and can significantly improve the recovery rate of vanadium, but the mixed waste liquid containing acid and sodium salt in the method is difficult to treat.

[0007] CN102703688A proposes a method for extracting vanadium from vanadium-titanium magnetite by leaching carbonate after oxidation roasting. The method uses calcium salt instead of sodium salt for roasting, which solves the problem of sodium content in tailings. The tailings can be recycled. However, after roasting, the clinker uses sodium carbonate or sodium bicarbonate as a leaching agent and ammonium salt as a vanadium precipitation agent, resulting in the waste liquid containing NH 4+ and N a+ The mixed salt makes waste liquid treatment difficult and costly.

[0008] In view of the common high-acidity or high-salinity wastewater problem in the current vanadium extraction process, CN102560086A, CN101168802A, CN104003442A, CN104294047A, CN104831090A and CN103952565A etc. propose a method of leaching vanadium by using an ammonium salt (or ammonia water) leaching agent after blank roasting or calcification of vanadium slag. In this method, ammonium metavanadate can be directly crystallized in the leaching solution, and the liquid after crystallization can be recycled, which can completely solve the problem of vanadium precipitation wastewater, and the tailings after leaching do not contain sodium salt, and can be directly used for ore smelting. However, the main problem of this series of methods is that the easily decomposable ammonium salt (ammonium carbonate, ammonium bicarbonate or ammonia water) is used as the leaching agent, the concentration of the leaching agent is high, the ammonia volatilization is serious, and the liquid-to-solid ratio is large (usually 2:1-10:1), resulting in large reagent consumption and a poor operating environment. Moreover, similar methods are directly used in the roasting process of vanadium-titanium magnetite with poor results.

[0009] CN105087864A discloses a method for directly producing titanium carbide from vanadium-titanium magnetite, wherein the method directly uses vanadium-titanium magnetite and solid carbon as main raw materials to prepare carbon-containing balls / blocks, and produces titanium carbide slag and ferrovanadium by heating once in an induction furnace; wherein the ferrovanadium can be directly cast into ingots for sale or blown to prepare vanadium slag and steel for sale; the titanium carbide slag is finely ground after cooling, and granular elemental iron and titanium carbide powder are separated after weak magnetic, strong magnetic and flotation separation and sold separately; the raw materials are in percentage by mass: vanadium-titanium magnetite 50-80%, solid carbon 15-40%, binder 0.5-15%, calcium carbonate 0.5-35%; the vanadium-titanium magnetite involved contains 8-60% iron; the solid carbon includes coal, petroleum coke, semi-coke, coke and mixtures thereof, and the fixed carbon content is >60%. The method is a method for producing ferrovanadium by directly reducing vanadium-titanium magnetite with carbon, and no oxidizing gas is introduced during the reduction process, and the reduction of vanadium and iron is achieved by adding excess carbon to maintain a reducing atmosphere. However, the obtained product is crude ferrovanadium slag, which needs to be further blown to obtain vanadium slag. Therefore, this method cannot directly obtain vanadium products, but only vanadium raw materials.

[0010] CN109207721B discloses a method for obtaining ammonium metavanadate from vanadium-titanium magnetite. The method uses ammonium oxalate solution to leach vanadium-titanium magnetite roasted clinker, and after leaching, the ammonium metavanadate crystals are mixed with tailings, and hot water is used to dissolve the ammonium metavanadate to separate the ammonium metavanadate from the leached residue. The vanadium-dissolving solution is evaporated and crystallized to obtain ammonium metavanadate crystals. However, the problem with this process is that part of the ammonium oxalate enters the vanadium-dissolving solution during the hot water vanadium dissolving process, which will cause the loss of ammonium oxalate in the leaching solution. At the same time, the solubility of ammonium metavanadate is significantly affected by temperature, and the high temperature of the system needs to be maintained, but it is still difficult to accumulate the vanadium concentration in the liquid phase.

[0011] In recent years, environmentally friendly roasting and leaching processes have received more and more attention. Clean methods for directly extracting vanadium from vanadium-titanium magnetite need further research. Summary of the invention

[0012] In view of the problems existing in the prior art, the present invention provides a method for enhanced leaching of vanadium from vanadium-titanium magnetite. The method has high vanadium recovery rate in the leaching process, low impurity element content, low reaction temperature, low energy consumption and broad application prospects.

[0013] To achieve this object, the present invention adopts the following technical solutions:

[0014] The present invention provides a method for enhanced leaching of vanadium from vanadium-titanium magnetite, the method comprising the following steps:

[0015] (1) mixing vanadium-titanium magnetite and a calcium-based additive, and performing oxidative roasting to obtain roasted clinker;

[0016] (2) The roasted clinker is leached with an acid-containing ammonium oxalate solution and solid-liquid separation is performed to obtain a vanadium-containing liquid.

[0017] In the method for enhanced leaching of vanadium from vanadium-titanium magnetite provided by the present invention, vanadium spinel in vanadium-titanium magnetite is decomposed to form calcium vanadate under the action of calcium additive; then in acidic ammonium oxalate solution, calcium vanadate reacts with oxalate to form calcium oxalate with lower solubility; at the same time, under acidic conditions, V 5+ Reduced to V by oxalate 4+ Vanadyl oxalate is generated and dissolved into the liquid phase. The solubility of vanadyl oxalate is very high, and the concentration of V can reach 20-30g / L. In ammonium oxalate solution, V 5+ It exists in the ammonium salt solution in the form of ammonium metavanadate and is affected by NH 4+ Due to the salting-out effect, the solubility of ammonium metavanadate is very low, and the V concentration is only 10-15 g / L. The present invention uses an acid-containing ammonium oxalate solution to facilitate the dissolution of vanadium and increase the vanadium concentration of the solution system. It also has an excellent leaching effect on the difficult-to-leach vanadium-titanium magnetite.

[0018] Preferably, the vanadium-titanium magnetite in step (1) is crushed and ball-milled before mixing.

[0019] Preferably, the proportion of -200 mesh in the particle size of the vanadium-titanium magnetite after crushing and ball milling is 70 to 90%, for example, it can be 70%, 72%, 75%, 78%, 80%, 82%, 85%, 88% or 90%, etc., but is not limited to the listed values, and other unlisted values ​​within this range are also applicable.

[0020] Preferably, the vanadium-titanium magnetite contains a spinel phase and an ilmenite phase.

[0021] Preferably, the vanadium-titanium magnetite contains any one or a combination of at least two of the impurity elements such as iron, aluminum, silicon or magnesium.

[0022] Preferably, the content of vanadium pentoxide in the vanadium-titanium magnetite is 1.2-1.8wt%, for example, it can be 1.2wt%, 1.3wt%, 1.4wt%, 1.5wt%, 1.6wt%, 1.7wt% or 1.8wt%, etc., but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0023] Preferably, the calcium-based additive in step (1) comprises a calcium compound, preferably calcium carbonate and / or calcium oxide.

[0024] Preferably, the calcium-based additive is 1 to 5wt% of the mass of the vanadium-titanium magnetite, for example, it can be 1wt%, 1.5wt%, 1.9wt%, 2.4wt%, 2.8wt%, 3.3wt%, 3.7wt%, 4.2wt%, 4.6wt% or 5wt%, etc., but is not limited to the listed values, and other unlisted values ​​within this range are also applicable.

[0025] The present invention preferably controls the quality of the calcium-based additive within the above range to avoid the formation of calcium vanadate and silicate, thereby reducing the leaching rate, while effectively ensuring that the vanadium in the vanadium-titanium magnetite reacts effectively and can be subsequently leached efficiently.

[0026] Preferably, the temperature of the oxidative roasting in step (1) is 1050-1250°C, for example, it can be 1050°C, 1073°C, 1095°C, 1117°C, 1139°C, 1162°C, 1184°C, 1206°C, 1228°C or 1250°C, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0027] The present invention further preferably controls the temperature of the chemical roasting within the above range to avoid the formation of a more stable mineral phase caused by high temperature. The formation of these stable mineral calcium silicate phases will cause the encapsulation of vanadium, resulting in a decrease in the leaching rate during leaching.

[0028] Preferably, the oxidative roasting time is 0.5 to 1.5 h, for example, 0.5 h, 0.6 h, 0.7 h, 0.8 h, 0.9 h, 1.0 h, 1.1 h, 1.2 h, 1.4 h or 1.5 h, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0029] The present invention further preferably sets the oxidative roasting time within the above range, which is more conducive to ensuring the oxidation of vanadium and avoiding the problem of decreased vanadium conversion rate caused by over-burning.

[0030] Preferably, the fuel used in the oxidative roasting process is any one of pulverized coal, heavy oil, natural gas or coal gas, or a combination of at least two of them, wherein typical but non-limiting combinations are a combination of pulverized coal and natural gas, a combination of pulverized coal and coal gas, a combination of heavy oil and natural gas, and a combination of natural gas and coal gas, etc.

[0031] Preferably, the acid-containing ammonium oxalate solution in step (2) is a mixed solution of ammonium oxalate and acid.

[0032] In the present invention, ammonium oxalate and acid can be mixed first, and then the mixed acid-containing ammonium oxalate solution can be subjected to leaching treatment. Alternatively, roasted clinker and ammonium oxalate can be mixed first, and then acid can be added to form an acid-containing ammonium oxalate solution; or roasted clinker and acid can be mixed first, and then ammonium oxalate can be added to form an acid-containing ammonium oxalate solution; or roasted clinker, acid and ammonium oxalate can be added to the container at the same time. There is no special restriction on the order of adding materials.

[0033] Preferably, the mass fraction of ammonium oxalate in the acid-containing ammonium oxalate solution is 6 to 9wt%, for example, it can be 6wt%, 6.4wt%, 6.7wt%, 7wt%, 7.4wt%, 7.7wt%, 8wt%, 8.4wt%, 8.7wt% or 9wt%, etc., but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0034] Preferably, the pH of the acid-containing ammonium oxalate solution in step (2) is 2 to 5, for example, 2, 2.5, 2.8, 3, 3.2, 3.7, 4, 4.4, 4.7 or 5, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0035] In the present invention, the pH of the acid-containing ammonium oxalate solution is preferably 2 to 5, which is more conducive to the dissolution of vanadium, increases the concentration of vanadium in the solution system, and can effectively reduce the liquid-solid ratio.

[0036] The vanadium-containing liquid obtained by the present invention can be further post-processed according to actual needs, and the obtained leaching slag does not contain sodium salt and can be directly used for ironmaking with ore, thereby realizing the comprehensive utilization of vanadium-titanium magnetite.

[0037] Preferably, the acid in the acid-containing ammonium oxalate solution comprises any one of sulfuric acid, hydrochloric acid, acetic acid, formic acid or oxalic acid, or a combination of at least two thereof, wherein typical but non-limiting combinations are a combination of sulfuric acid and hydrochloric acid, a combination of oxalic acid and hydrochloric acid, a combination of oxalic acid and acetic acid, a combination of sulfuric acid and formic acid, and a combination of hydrochloric acid and acetic acid, etc.

[0038] Preferably, the mass ratio of the acid-containing ammonium oxalate solution to the roasted clinker in step (2) is 0.5 to 1:1, for example, it can be 0.5:1, 0.56:1, 0.62:1, 0.67:1, 0.73:1, 0.78:1, 0.84:1, 0.89:1, 0.95:1 or 1:1, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0039] The present invention further preferably has a mass ratio of the acid-containing ammonium oxalate solution to the roasted clinker of 0.5 to 1:1, which can better ensure the leaching conversion effect.

[0040] Preferably, the temperature of the leaching treatment is 60-80°C, for example, it can be 60°C, 63°C, 65°C, 67°C, 69°C, 72°C, 74°C, 76°C, 78°C or 80°C, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0041] The present invention adopts the acid-containing ammonium oxalate solution, so that the leaching temperature can be reduced to below 80° C., and the energy consumption of the leaching process can be significantly reduced.

[0042] Preferably, the leaching treatment time is 0.5 to 1 h, for example, it can be 0.5 h, 0.56 h, 0.60 h, 0.65 h, 0.70 h, 0.75 h, 0.80 h, 0.85 h, 0.95 h or 1 h, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0043] Preferably, the method further comprises:

[0044] (3) the vanadium-containing liquid is subjected to hydrolysis, impurity removal and solid-liquid separation to obtain a vanadium-containing purified liquid;

[0045] Preferably, the impurity remover for hydrolysis is aqueous ammonia.

[0046] Preferably, the concentration of the aqueous ammonia is 20-28wt%, for example, it can be 20wt%, 21wt%, 22wt%, 23wt%, 24wt%, 25wt%, 26wt%, 27wt% or 28wt%, etc., but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0047] Preferably, the impurity removal temperature is 70-80°C, for example, it can be 70°C, 72°C, 73°C, 74°C, 75°C, 76°C, 77°C, 78°C, 79°C or 80°C, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0048] Preferably, the hydrolysis and impurity removal comprises: mixing a first portion of ammonia water and a vanadium-containing liquid to perform a first stage of impurity removal, and then adding a second portion of ammonia water to perform a second stage of impurity removal.

[0049] Under acidic conditions, elements such as Fe and Al easily enter the liquid phase and form complex ions with oxalate. The complex structure needs to be opened to effectively remove Fe and Al. Adjusting the liquid phase to alkaline can effectively open the complex structure and change the ion form, so that Fe and Al ions are hydrolyzed to form Fe(OH)2 and Al(OH)3 precipitates. During the hydrolysis vanadium precipitation process, the stirring rate and pH need to be controlled step by step to make Fe(OH)2 and Al(OH)3 form precipitates with large specific surface area, and impurities such as Si and P are removed synergistically to obtain purified vanadium liquid, creating favorable conditions for the subsequent preparation of high-purity vanadium.

[0050] Preferably, after mixing the first part of ammonia water and the vanadium-containing liquid, the pH of the system is 7.5-8.0, for example, 7.5, 7.6, 7.7, 7.8, 7.9 or 8.0, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0051] Preferably, the stirring speed of the first stage impurity removal is 500-700 r / min, for example, it can be 500 r / min, 520 r / min, 540 r / min, 560 r / min, 580 r / min, 610 r / min, 630 r / min, 650 r / min, 670 r / min or 700 r / min, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0052] The present invention further ensures good filtering performance of removing impurity mud by controlling the stirring rate and pH in steps.

[0053] Preferably, the time for removing impurities in the first stage is 1 to 2 hours, for example, it can be 1 hour, 1.2 hours, 1.3 hours, 1.4 hours, 1.5 hours, 1.6 hours, 1.7 hours, 1.8 hours, 1.9 hours or 2 hours, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0054] Preferably, after adding the second portion of aqueous ammonia, the pH of the system is 8.0 to 9.0, for example, 8.0, 8.2, 8.3, 8.4, 8.5, 8.6, 8.7, 8.8, 8.9 or 9.0, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0055] Preferably, the stirring speed of the second stage impurity removal is 200-400r / min, for example, it can be 200r / min, 220r / min, 240r / min, 260r / min, 280r / min, 310r / min, 330r / min, 350r / min, 370r / min or 400r / min, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0056] In the present invention, the stirring rates of the first stage impurity removal and the second stage impurity removal have a great influence on the impurity removal effect. It is further preferred that the stirring rates of the impurity removal are within the above range, which can better reduce the impurity content in the purified liquid.

[0057] Preferably, the time for removing impurities in the second stage is 3 to 5 hours, for example, it can be 3 hours, 3.3 hours, 3.5 hours, 3.7 hours, 3.9 hours, 4.0 hours, 4.4 hours, 4.6 hours, 4.8 hours or 5 hours, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0058] As a preferred technical solution of the present invention, the method comprises the following steps:

[0059] (1) mixing vanadium-titanium magnetite and a calcium-based additive, wherein the calcium-based additive is 1 to 5 wt% of the mass of the vanadium-titanium magnetite, and oxidatively roasting at 1050 to 1250° C. for 0.5 to 1.5 h to obtain a roasted clinker;

[0060] (2) the roasted clinker is subjected to a leaching treatment at 60 to 80° C. for 0.5 to 1 h in an acidic ammonium oxalate solution containing 6 to 9 wt % ammonium oxalate and having a pH of 2 to 5, followed by solid-liquid separation, wherein the mass ratio of the acidic ammonium oxalate solution to the roasted clinker is 0.5 to 1:1, to obtain a vanadium-containing liquid;

[0061] (3) Mix the first part of ammonia water and the vanadium-containing liquid until the pH value is 7.5-8.0, and carry out the first stage of impurity removal at 500-700 r / min for 1-2 hours, then add the second part of ammonia water until the pH value is 8.0-9.0, and carry out the second stage of impurity removal at 200-400 r / min for 3-5 hours, and then separate the solid and liquid to obtain the vanadium-containing purified liquid.

[0062] The present invention has no special limitation on the solid-liquid separation in the above process. Any device and method for solid-liquid separation known to those skilled in the art can be used, and can also be adjusted according to the actual process, such as filtration, centrifugation or sedimentation separation, or a combination of different methods.

[0063] Compared with the prior art, the present invention has at least the following beneficial effects:

[0064] (1) The method for enhanced leaching of vanadium from vanadium-titanium magnetite provided by the present invention adopts an acid-containing ammonium oxalate solution to enhance the leaching of vanadium-titanium magnetite roasted clinker, with a high vanadium extraction rate. Under preferred conditions, the vanadium content of the tailings is less than 0.2wt%, the V concentration in the obtained purified liquid is ≥20g / L, the vanadium concentration is high, the concentrations of Al and Fe in the purified liquid are respectively <0.2g / L, the total impurity content is ≤0.4g / L, and the filtration time of the filter mud is <1.5min, thereby realizing efficient extraction of vanadium from vanadium-titanium magnetite;

[0065] (2) The method for enhanced leaching of vanadium from vanadium-titanium magnetite provided by the present invention generates V 4+ , enters the solution in the form of vanadium oxalate. Compared with ammonium metavanadate, its solubility is greatly improved, which can increase the vanadium concentration in the solution, reduce the leaching liquid-solid ratio, reduce the reaction temperature, and reduce the reaction energy consumption of the leaching process;

[0066] (3) The method for enhanced leaching of vanadium from vanadium-titanium magnetite provided by the present invention uses a calcium-based additive as an auxiliary material in the roasting process, and the roasting process does not generate harmful gases, and the roasting process is clean and environmentally friendly;

[0067] (4) The tailings after vanadium extraction from the method for enhanced leaching of vanadium from vanadium-titanium magnetite provided by the present invention do not contain sodium salt and can be directly used for ironmaking with ore, thereby realizing the comprehensive utilization of vanadium-titanium magnetite resources. BRIEF DESCRIPTION OF THE DRAWINGS

[0068] Figure 1 It is a flow chart of a method for enhanced leaching of vanadium from vanadium-titanium magnetite provided in a specific embodiment of the present invention. DETAILED DESCRIPTION

[0069] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.

[0070] The present invention is further described in detail below. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.

[0071] As a specific embodiment of the present invention, a method for enhanced leaching of vanadium from vanadium-titanium magnetite is provided, and its flow diagram is as follows: Figure 1 As shown, the method comprises the following steps:

[0072] (1) mixing vanadium-titanium magnetite and a calcium-based additive, wherein the calcium-based additive is 1 to 5 wt% of the mass of the vanadium-titanium magnetite, and oxidatively roasting at 1050 to 1250° C. for 0.5 to 1.5 h to obtain a roasted clinker;

[0073] (2) the roasted clinker is subjected to a leaching treatment at 60 to 80° C. for 0.5 to 1 h in an acidic ammonium oxalate solution containing 6 to 9 wt % ammonium oxalate and having a pH of 2 to 5, followed by solid-liquid separation, wherein the mass ratio of the acidic ammonium oxalate solution to the roasted clinker is 0.5 to 1:1, to obtain a vanadium-containing liquid and a tailings free of sodium;

[0074] (3) Mix the first part of ammonia water and the vanadium-containing liquid to a pH of 7.5-8.0, and perform the first stage of impurity removal at 500-700 r / min for 1-2 hours, then add the second part of ammonia water to a pH of 8.0-9.0, and perform the second stage of impurity removal at 200-400 r / min for 3-5 hours, and then perform solid-liquid separation to obtain vanadium-containing purified liquid and impurity-removed mud. The vanadium-containing liquid can be directly crystallized to obtain ammonium metavanadate, and vanadium pentoxide can be obtained after calcination without further treatment.

[0075] Example 1

[0076] This embodiment provides a method for enhanced leaching of vanadium from vanadium-titanium magnetite, the method comprising the following steps:

[0077] (1) mixing vanadium-titanium magnetite (the particle size of -200 mesh after crushing and ball milling accounts for 70%, and the V2O5 content is 1.67wt%) and calcium carbonate, wherein the calcium carbonate is 5wt% of the mass of the vanadium-titanium magnetite, and oxidative roasting is performed at 1050° C. for 1.5 h, using coal powder as a fuel for the roasting, to obtain roasted clinker;

[0078] (2) the roasted clinker is leached at 70° C. for 0.8 h in an acidic ammonium oxalate solution containing 8.5 wt % ammonium oxalate and having a pH of 2.2 (the molar ratio of oxalic acid to formic acid is 2:1), and filtered, wherein the mass ratio of the acidic ammonium oxalate solution to the roasted clinker is 0.8:1, to obtain a vanadium-containing liquid and a tailings free of sodium; the tailings can be directly used for ore blending and ironmaking;

[0079] (3) Mix the first part of ammonia water (concentration 27 wt%) and the vanadium-containing liquid to a pH of 7.5, and carry out the first stage of impurity removal at 700 r / min and 70° C. for 1 hour, then add the second part of ammonia water (concentration 27 wt%) to a pH of 8.0, and carry out the second stage of impurity removal at 400 r / min and 70° C. for 3 hours, and then filter to obtain the vanadium-containing purified liquid and impurity-removed mud.

[0080] Example 2

[0081] This embodiment provides a method for enhanced leaching of vanadium from vanadium-titanium magnetite, the method comprising the following steps:

[0082] (1) mixing vanadium-titanium magnetite (the particle size of -200 mesh after crushing and ball milling accounts for 80%, and the V2O5 content is 1.76wt%) and calcium carbonate, wherein the calcium carbonate is 1wt% of the mass of the vanadium-titanium magnetite, and oxidative roasting is performed at 1250° C. for 0.5 h, using natural gas as a fuel for the roasting, to obtain roasted clinker;

[0083] (2) the roasted clinker is leached at 75° C. for 1 h with an acidic ammonium oxalate solution (the acid is acetic acid) containing 8.2 wt % ammonium oxalate and a pH of 3.3, and filtered, wherein the mass ratio of the acidic ammonium oxalate solution to the roasted clinker is 1:1, to obtain a vanadium-containing liquid and a tailings free of sodium; the tailings can be directly used for ore blending and ironmaking;

[0084] (3) Mix the first part of ammonia water (concentration 20 wt%) and the vanadium-containing liquid to a pH of 7.5, and carry out the first stage of impurity removal at 600 r / min and 80° C. for 1 hour, then add the second part of ammonia water (concentration 20 wt%) to a pH of 8.5, and carry out the second stage of impurity removal at 300 r / min and 80° C. for 3 hours, and then filter to obtain the vanadium-containing purified liquid and impurity-removed mud.

[0085] Example 3

[0086] This embodiment provides a method for enhanced leaching of vanadium from vanadium-titanium magnetite, the method comprising the following steps:

[0087] (1) mixing vanadium-titanium magnetite (the particle size of -200 mesh after crushing and ball milling accounts for 90%, and the V2O5 content is 1.65wt%) and calcium oxide, wherein the calcium oxide is 3wt% of the mass of the vanadium-titanium magnetite, and oxidative roasting is performed at 1050° C. for 1.5 h, using natural gas as a fuel for the roasting, to obtain roasted clinker;

[0088] (2) the roasted clinker is leached at 65° C. for 0.9 h in an acidic ammonium oxalate solution (the acid is sulfuric acid) containing 7 wt % ammonium oxalate and a pH of 3.5, and filtered, wherein the mass ratio of the acidic ammonium oxalate solution to the roasted clinker is 1:1, to obtain a vanadium-containing liquid and a tailings free of sodium; the tailings can be directly used for ore blending and ironmaking;

[0089] (3) Mix the first part of ammonia water (concentration 24 wt%) and the vanadium-containing liquid to a pH of 7.6, and carry out the first stage of impurity removal at 550 r / min and 75° C. for 1.5 h, then add the second part of ammonia water (concentration 24 wt%) to a pH of 8.2, and carry out the second stage of impurity removal at 320 r / min and 75° C. for 4.5 h, and then filter to obtain the vanadium-containing purified liquid and impurity-removed mud.

[0090] Example 4

[0091] This embodiment provides a method for enhanced leaching of vanadium from vanadium-titanium magnetite, the method comprising the following steps:

[0092] (1) mixing vanadium-titanium magnetite (the particle size of -200 mesh after crushing and ball milling accounts for 75%, and the V2O5 content is 1.67wt%) and calcium oxide, wherein the calcium oxide is 2.5wt% of the mass of the vanadium-titanium magnetite, and oxidative roasting is performed at 1150° C. for 1 hour, using coal powder and natural gas as fuel at the same time, to obtain roasted clinker;

[0093] (2) the roasted clinker is leached at 70° C. for 0.6 h in an acidic ammonium oxalate solution (the acid is hydrochloric acid) containing 7.8 wt % ammonium oxalate and a pH of 0.5, and filtered, wherein the mass ratio of the acidic ammonium oxalate solution to the roasted clinker is 0.5:1, to obtain a vanadium-containing liquid and a tailings free of sodium; the tailings can be directly used for ore blending and ironmaking;

[0094] (3) Mix the first part of ammonia water (concentration 28 wt%) and the vanadium-containing liquid to a pH of 7.5, and carry out the first stage of impurity removal at 660 r / min and 77° C. for 1.8 h. Then add the second part of ammonia water (concentration 28 wt%) to a pH of 8.7, and carry out the second stage of impurity removal at 350 r / min and 77° C. for 3.5 h. Then, filter to obtain the vanadium-containing purified liquid and impurity-removed mud.

[0095] Example 5

[0096] This embodiment provides a method for enhanced leaching of vanadium from vanadium-titanium magnetite, the method comprising the following steps:

[0097] (1) mixing vanadium-titanium magnetite (the particle size of -200 mesh after crushing and ball milling accounts for 88%, and the V2O5 content is 1.59wt%) and calcium carbonate, wherein the calcium carbonate is 3.5wt% of the mass of the vanadium-titanium magnetite, and oxidative roasting is performed at 1100° C. for 0.8 h, using coal powder and heavy oil as fuel at the same time, to obtain roasted clinker;

[0098] (2) the roasted clinker is leached at 80° C. for 0.8 h in an acidic ammonium oxalate solution (the acid is oxalic acid) containing 7 wt % ammonium oxalate and pH 4, and filtered, wherein the mass ratio of the acidic ammonium oxalate solution to the roasted clinker is 0.8:1, to obtain a vanadium-containing liquid and a tailings free of sodium; the tailings can be directly used for ore blending and ironmaking;

[0099] (3) Mix the first part of ammonia water (concentration 24 wt%) and the vanadium-containing liquid to a pH of 7.7, and carry out the first stage of impurity removal at 550 r / min and 72° C. for 1.2 h, then add the second part of ammonia water (concentration 24 wt%) to a pH of 8.4, and carry out the second stage of impurity removal at 300 r / min and 72° C. for 3.5 h, and then filter to obtain the vanadium-containing purified liquid and impurity-removed mud.

[0100] Example 6

[0101] This embodiment provides a method for enhanced leaching of vanadium from vanadium-titanium magnetite, the method comprising the following steps:

[0102] (1) mixing vanadium-titanium magnetite (the particle size of -200 mesh after crushing and ball milling accounts for 78%, and the V2O5 content is 1.67wt%) and calcium carbonate, wherein the calcium carbonate is 4.6wt% of the mass of the vanadium-titanium magnetite, and oxidative roasting is performed at 1200° C. for 1.2 h, using coal powder and heavy oil as fuel at the same time, to obtain roasted clinker;

[0103] (2) the roasted clinker is leached at 60° C. for 1 h with an acid-containing ammonium oxalate solution (the acid is oxalic acid) containing 8 wt % ammonium oxalate and a pH of 2, and filtered, wherein the mass ratio of the acid-containing ammonium oxalate solution to the roasted clinker is 1:1, to obtain a vanadium-containing liquid and a tailings free of sodium; the tailings can be directly used for ore blending and ironmaking;

[0104] (3) Mix the first part of ammonia water (concentration 25 wt%) and the vanadium-containing liquid to a pH of 7.6, and carry out the first stage of impurity removal at 600 r / min and 74° C. for 1.5 h, then add the second part of ammonia water (concentration 25 wt%) to a pH of 8.5, and carry out the second stage of impurity removal at 300 r / min and 74° C. for 4 h, and then filter to obtain the vanadium-containing purified liquid and impurity-removed mud.

[0105] Example 7

[0106] This embodiment provides a method for enhanced leaching of vanadium from vanadium-titanium magnetite, the method comprising the following steps:

[0107] (1) mixing vanadium-titanium magnetite (the particle size of -200 mesh after crushing and ball milling accounts for 82%, and the V2O5 content is 1.69wt%) and calcium carbonate, wherein the calcium carbonate is 2.9wt% of the mass of the vanadium-titanium magnetite, and oxidative roasting is performed at 1090° C. for 1.4 h, using coal powder and coal gas as fuel at the same time, to obtain roasted clinker;

[0108] (2) the roasted clinker is leached at 70° C. for 1 h with an acid-containing ammonium oxalate solution (the acid is oxalic acid) containing 9 wt % ammonium oxalate and a pH of 2.5, and filtered, wherein the mass ratio of the acid-containing ammonium oxalate solution to the roasted clinker is 0.5:1, to obtain a vanadium-containing liquid and a tailings free of sodium; the tailings can be directly used for ore blending and ironmaking;

[0109] (3) Mix the first part of ammonia water (concentration 23 wt%) and the vanadium-containing liquid to a pH of 8.0, and carry out the first stage of impurity removal at 500 r / min and 74° C. for 2 h, then add the second part of ammonia water (concentration 23 wt%) to a pH of 9.0, and carry out the second stage of impurity removal at 200 r / min and 74° C. for 5 h, and then filter to obtain the vanadium-containing purified liquid and impurity-removed mud.

[0110] Example 8

[0111] Except for adjusting the pH to 1.5 in step (2), the rest is the same as Example 7.

[0112] Example 9

[0113] Except for adjusting the pH to 6 in step (2), the rest is the same as Example 7.

[0114] Example 10

[0115] Except that the temperature of the first stage impurity removal and the second stage impurity removal in step (3) are both adjusted to 60° C., the rest is the same as Example 7.

[0116] Embodiment 11

[0117] Except that the temperature of the first stage impurity removal and the second stage impurity removal in step (3) are both adjusted to 90° C., the rest is the same as Example 7.

[0118] Example 12

[0119] Except that only the first stage of impurity removal is performed in step (3), the rest is the same as Example 7.

[0120] Example 13

[0121] Except that only the second stage of impurity removal is performed in step (3), the rest is the same as Example 7.

[0122] Embodiment 14

[0123] Except that the stirring speed of the first stage impurity removal in step (3) is adjusted to 300 r / min and the stirring speed of the second stage impurity removal is adjusted to 600 r / min, the rest is the same as Example 7.

[0124] Comparative Example 1

[0125] Except that no acid is added in step (2), the rest is the same as Example 7.

[0126] Comparative Example 2

[0127] Except that ammonium oxalate is not added in step (2), the rest is the same as Example 7.

[0128] Comparative Example 3

[0129] Except that 9% oxalic acid is used to replace the ammonium oxalate solution in step (2) and the pH adjustment process using oxalic acid is omitted, the rest is the same as Example 7.

[0130] Test method: The vanadium content in the tailings is detected by titration, and the vanadium concentration, aluminum concentration and iron concentration in the vanadium-containing purified liquid are detected by ICP, and the time required for filtering and removing the sludge in step (3) is calculated.

[0131] The test results of the above embodiments and comparative examples are shown in Table 1.

[0132] Table 1

[0133]

[0134]

[0135] From Table 1, we can see the following points:

[0136] (1) It can be seen from Examples 1-7 that the method for enhanced leaching of vanadium from vanadium-titanium magnetite provided by the present invention has a high vanadium leaching rate of more than 90%, and the vanadium content of the tailings is less than 0.2%, the V concentration in the obtained purified liquid is ≥20 g / L, the concentrations of Al and Fe in the purified liquid are respectively less than 0.2 g / L, the total impurity content is ≤0.4 g / L, and the filtration time of the filter mud is less than 1.5 min;

[0137] (2) It can be seen from Example 1 and Comparative Examples 1 to 3 that in Example 1, an acid-containing ammonium oxalate solution is used for leaching. Compared with Comparative Example 1 in which no acid is added, Comparative Example 2 in which no ammonium oxalate is added, and Comparative Example 3 in which oxalic acid is used instead of ammonium oxalate, the leaching rate of Example 1 is as high as 91%, the vanadium content in the tailings is only 0.15%, and the total impurity content in the purified liquid is only 0.33 g / L, while the leaching rates in Comparative Examples 1 to 3 are only 69%, 30%, and 67%, respectively, and the vanadium concentrations in the purified liquid are only 11 g / L, 10 g / L, and 8 g / L, respectively, and the total impurity content in Comparative Example 3 is relatively higher. This shows that the present invention uses an acid-containing ammonium oxalate solution for leaching, and the interaction between oxalate, ammonium ions, and acid significantly improves the conversion rate and extraction rate of vanadium and reduces the content of impurities;

[0138] (3) It can be seen from the combination of Example 1 and Examples 8 to 9 that in Example 1, an acidic ammonium oxalate solution with a pH of 2.2 is used for leaching. Compared with Examples 8 to 9 in which the pH is 1.5 and 6 respectively, in Example 1, not only is the leaching rate high but also the impurity content is low, and the filtration time is only 1.1 min. In Example 8, the pH is adjusted too low, the impurity content of Al and Fe in the purified liquid is high, and the sludge removal filtration speed is slow. In Example 9, the pH is adjusted to alkaline, the vanadium conversion rate is low, and the vanadium concentration in the purified liquid is significantly reduced. This shows that the present invention significantly improves the leaching rate and the purity of the purified liquid and reduces the filtration time by preferably controlling the pH of the acidic ammonium oxalate solution within a specific range, thereby reducing the production time.

[0139] (4) It can be seen from the combination of Example 1 and Examples 10 to 11 that the impurity removal temperature is too high or too low, which will lead to high Al and Fe impurity contents in the vanadium-containing purified liquid, and the impurity removal mud is difficult to filter. The present invention significantly improves the filtration efficiency and reduces the impurity content in the purified liquid by controlling the impurity removal temperature within a specific range;

[0140] (5) It can be seen from Example 1 and Examples 12 to 14 that the method of step-by-step purification and impurity removal is not adopted in Examples 12 to 13, which will result in high Al and Fe impurity contents in the vanadium-containing purified liquid, and the impurity removal sludge is difficult to filter; in the process of step-by-step impurity removal in Example 14, too fast or too slow rate will result in high Al and Fe impurity contents in the vanadium-containing purified liquid, and the impurity removal sludge is difficult to filter. This shows that the present invention significantly improves the impurity removal effect and shortens the filtration time by optimizing the two-step impurity removal method and strictly controlling the stirring rate in each step of the impurity removal process.

[0141] The present invention illustrates the detailed structural features of the present invention through the above embodiments, but the present invention is not limited to the above detailed structural features, that is, it does not mean that the present invention must rely on the above detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for enhancing the leaching of vanadium from vanadium-titanium magnetite by increasing the vanadium concentration of the solution system, characterized in that: The method comprises the following steps: (1) mixing vanadium-titanium magnetite and a calcium-based additive, and performing oxidative roasting, wherein the vanadium spinel in the vanadium-titanium magnetite is decomposed to generate calcium vanadate under the action of the calcium-based additive, and a roasted clinker is obtained; (2) The roasted clinker is leached with an acidic ammonium oxalate solution, and calcium vanadate reacts with oxalate to form calcium oxalate. 5+ Restored to V 4+ Producing vanadium oxalate, and performing solid-liquid separation to obtain a vanadium-containing liquid with a V concentration of 20 to 30 g / L, wherein the pH of the acid-containing ammonium oxalate solution is 2 to 5, and the mass ratio of the acid-containing ammonium oxalate solution to the roasted clinker is 0.5 to 1:1; The vanadium-titanium magnetite contains a spinel phase and an ilmenite phase; The vanadium-titanium magnetite contains any one or a combination of at least two of the impurity elements such as iron, aluminum, silicon or magnesium; The content of vanadium pentoxide in the vanadium-titanium magnetite is 1.2-1.8wt%; The acid-containing ammonium oxalate solution is a mixed solution of ammonium oxalate and acid; The acid in the acid-containing ammonium oxalate solution includes any one of sulfuric acid, hydrochloric acid, acetic acid, formic acid or oxalic acid, or a combination of at least two thereof; The method further comprises: (3) The vanadium-containing liquid is subjected to hydrolysis and impurity removal and solid-liquid separation in sequence to obtain a vanadium-containing purified liquid; the hydrolysis and impurity removal comprises: mixing a first portion of ammonia water and the vanadium-containing liquid to perform a first stage of impurity removal, and then adding a second portion of ammonia water to perform a second stage of impurity removal.

2. The method according to claim 1, characterized in that The calcium-based additive in step (1) includes calcium carbonate and / or calcium oxide.

3. The method according to claim 1, characterized in that The calcium-based additive is 1-5 wt% of the mass of the vanadium-titanium magnetite.

4. The method according to claim 1 or 2, characterized in that: The temperature of the oxidative roasting in step (1) is 1050-1250°C.

5. The method according to claim 1, characterized in that The oxidation roasting time is 0.5 to 1.5 hours.

6. The method according to claim 1, characterized in that The fuel used in the oxidation roasting process is any one of pulverized coal, heavy oil, natural gas or coal gas, or a combination of at least two of them.

7. The method according to claim 1, characterized in that The mass fraction of ammonium oxalate in the acid-containing ammonium oxalate solution is 6-9wt%.

8. The method according to claim 1, characterized in that The temperature of the leaching treatment is 60-80°C.

9. The method according to claim 1, characterized in that: The leaching treatment time is 0.5 to 1 hour.

10. The method according to claim 1, characterized in that The impurity remover for hydrolysis is aqueous ammonia.

11. The method according to claim 1, characterized in that: The concentration of ammonia water is 20-28 wt%.

12. The method according to claim 1, characterized in that The impurity removal temperature is 70-80℃.

13. The method according to claim 1, characterized in that After mixing the first part of ammonia water and the vanadium-containing liquid, the pH of the system is 7.5-8.

0.

14. The method according to claim 1, characterized in that The stirring speed of the first stage impurity removal is 500-700 r / min.

15. The method according to claim 1, characterized in that The time for removing impurities in the first stage is 1 to 2 hours.

16. The method according to claim 1, characterized in that After adding the second portion of aqueous ammonia, the pH of the system was 8.0-9.

0.

17. The method according to claim 1, characterized in that The stirring speed of the second stage impurity removal is 200-400 r / min.

18. The method according to claim 1, characterized in that The time for removing impurities in the second stage is 3 to 5 hours.

19. The method according to claim 1, characterized in that The method comprises the following steps: (1) mixing vanadium-titanium magnetite and a calcium-based additive, wherein the calcium-based additive is 1 to 5 wt% of the mass of the vanadium-titanium magnetite, and oxidatively roasting at 1050 to 1250° C. for 0.5 to 1.5 h to obtain a roasted clinker; (2) the roasted clinker is subjected to a leaching treatment at 60 to 80° C. for 0.5 to 1 h in an acidic ammonium oxalate solution containing 6 to 9 wt % ammonium oxalate and having a pH of 2 to 5, followed by solid-liquid separation, wherein the mass ratio of the acidic ammonium oxalate solution to the roasted clinker is 0.5 to 1:1, to obtain a vanadium-containing liquid; (3) Mix the first part of ammonia water and the vanadium-containing liquid until the pH value is 7.5-8.0, and carry out the first stage of impurity removal at 500-700 r / min for 1-2 hours, then add the second part of ammonia water until the pH value is 8.0-9.0, and carry out the second stage of impurity removal at 200-400 r / min for 3-5 hours, and then separate the solid and liquid to obtain the vanadium-containing purified liquid.

Citation Information

Cited By

  • Method for extracting vanadium from vanadium titano-magnetite

    CN121250142A