Polyester packaging material
Through the combination of polymethylpentene and light-scattering pigments, the trade-off problem between high brightness and high light-blocking properties of packaging materials is solved, achieving low-load uniform color appearance and excellent light blocking at all angles, improving physical properties and Recyclability reduces cost and performance trade-offs.
Patent Information
- Application Number
- CN202210574915.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-08-16
- Filing Date
- 2018-12-27
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2038-12-27
AI Technical Summary
When existing packaging materials achieve high brightness values, high light blocking properties and uniform color appearance at all angles, it is difficult to reduce the additive load at the same time, resulting in increased costs and reduced physical properties. Moreover, there is a trade-off between light blocking and brightness, which affects recyclability. properties and gloss.
Using a combination of polymethylpentene and light-scattering pigments, the synergy at low loading levels produces a uniform color appearance and excellent light blocking properties across angles, reducing the use of colorants and opacifiers and improving physical properties and recyclability. .
The result is a low-cost, low-load, bright white color-matched packaging that improves physical properties and recyclability while maintaining high light blocking and brightness, avoiding the cost and performance tradeoffs typical of opacifiers.
Smart Images

Figure CN114989576B_ABST
Abstract
Description
[0001] This application is a divisional application of the Chinese patent application with the application date of December 27, 2018, application number "201880084393.5", and invention name "Polyester Packaging Material".
[0002] CROSS-REFERENCE TO RELATED APPLICATIONS
[0003] This application claims priority and the benefit of U.S. Provisional Patent Application Serial No. 62 / 611,713, entitled “White Polyester Packaging Material,” filed on December 29, 2017. This application also claims priority and the benefit of U.S. Provisional Patent Application Serial No. 62 / 764,783, entitled “White Polyester Packaging Material,” filed on August 16, 2018. Each application is incorporated herein by reference in its entirety. Technical Field
[0004] The present invention relates to packaging. In particular, the present invention relates to packaging having a high lightness value, high light blocking properties, a low percentage of additives, and a goniochromatic appearance (uniform color across all viewing angles). Background Art
[0005] In the packaging sector, plastics have replaced other materials such as glass. This substitution minimizes breakage, reduces weight and reduces the energy consumed in manufacturing and transportation.
[0006] Attracting consumers to purchase individual or family-sized containers involves trademarks and trade dress. One element of valuable trade dress is the color of the container. One element of valuable trademarks is consistent visibility of color. For some products, such as milk, light-colored or bright white containers are desired.
[0007] Lightness may be defined in the CIELAB color space, which mathematically describes all visible colors in three dimensions: L* for lightness, a* for green-red, and b* for blue-yellow. Figure 1 The CIELAB color scale is depicted. In the CIELAB color space, the L* axis runs from top to bottom. The maximum value of L* is 100, which would be a perfect reflecting diffuser (i.e., the brightest white). The minimum value of L* is 0, which would be a perfect absorber (i.e., the darkest black). Positive a* is red. Negative a* is green. Positive b* is yellow. Negative b* is blue.
[0008] One of the most important properties of the CIELAB model is device independence. This means that the color is defined independently of the nature of the color's generation or the device that displays the color. The L* value of the CIELAB color scale can be obtained using any CIELAB color measurement instrument and calculated using this formula:
[0009]
[0010] Where Y is the CIE tristimulus value, and Y n The CIELAB model allows quantification of how bright a product actually is. Brightness is usually achieved by adding highly reflective and minimally absorbing components such as titanium dioxide (TiO2).
[0011] Gonioapparent packaging maintains color and appearance across all viewing angles. Regardless of the consumer's viewing position, gonioapparent packaging is beneficial for uniform color consistency and brand recognition. In contrast, gonioapparent packaging shows color differences across viewing angles. Metallic or pearlescent effects are gonioapparent. Although metallic or pearlescent effects may be eye-catching, they may lead to reduced brand recognition and color non-uniformity.
[0012] like Figure 3 Phase separated mixtures as depicted in are produced when immiscible polymers are mixed. However, when these phase separated mixtures are subjected to orientation stress (e.g., blow molding, biaxial sheet orientation, uniaxial stretching, thermoforming, or fiber spinning), the smaller spheres of immiscible components flatten out. The problem is that such immiscible components may not flatten out completely, resulting in internal overlapping voids within the structured polymer, such as Figure 4 These voids create a large number of light scattering surfaces that reflect light in a non-uniform manner, resulting in color differences across viewing angles that vary by more than 10 units DE. CMC The effect of different colors with different angles (i.e. pearlescent appearance or metallic appearance) is achieved.
[0013] Gonioappearance can be measured using a multi-angle spectrophotometer such as the MA-T12 from X-Rite. ASTM E2175 describes the standard practice for specifying the geometry of a multi-angle spectrophotometer. CMC The calculated color difference between near specular viewing angle and far specular viewing angle can be used to quantify the amount of angular flop. Using a 45° incident light source and measuring the color at near specular (15°) and far specular (110°), the color difference indicates the change in appearance over a range of viewing angles. Figure 2Such a measurement for the angle-dependent color shift is shown. For such a measurement, greater than 10 units DE CMC Differences of are significant and indicate dichroic flop. Less than 10 units DE CMC The differences are not significant and indicate an angle-homogeneous appearance.
[0014] Light blocking is also required due to the need to conceal the contents of the package or to prevent the quality of the packaged product from deteriorating during the period between packaging and consumption. Light exposure may cause undesirable changes to the packaged items. When the product is sensitive to light radiation, it is difficult to achieve prevention of this degradation. For example, in milk, light has not only harmful photochemical effects but also ionizing effects. Specifically, riboflavin undergoes photodegradation when exposed to light between 200nm and 520nm. This degradation adversely affects the taste and smell of milk.
[0015] Light blocking (light barriers) limits certain wavelengths of light from passing through the packaging walls. This can be achieved through reflection or absorption, which prevents harmful effects on the contents contained within the package. However, typical methods of achieving light blocking are associated with performance tradeoffs in other critical areas of the package.
[0016] Bright white can reflect almost all light, thereby protecting the product from further degradation. In the past, in order to obtain bright white containers, packagers added colorants or sunscreens. Such additional colorants or sunscreens increase the cost of the container and may cause a vortex appearance (i.e., colorants and / or sunscreens do not seem to be fully dispersed in the composition), which may have a negative impact on consumer product perception. Sunscreens may also cause physical properties to reduce due to high pigment content, reduced recycling capacity and lower glossiness. For PET blow molding bottles or thermoforming parts, due to the high reflectivity of infrared light, high levels of sunscreens cause difficulty in reheating.
[0017] To overcome high reflectivity, absorbing pigments and / or dyes are often used to increase light blocking and reduce the total colorant content. However, adding absorbing pigments also reduces the brightness of the package. To date, creating brighter packages with high light blocking has required sacrificing brightness, light blocking or high loading levels (affecting cost, physical properties, gloss, recyclability).
[0018] U.S. Patent 4,377,616 describes a glossy satin-looking, opaque film composition and a method for making the same. U.S. Patent 5,089,309 describes a translucent resin container with a pearlescent luster. U.S. Patent 4,368,295 describes a film from a composition of a polyester and an olefin polymer. U.S. Patent 3,640,944 describes a modified polyester film for a perforated belt. U.S. Patent 8,575,296 describes a polyester article having a simulated metallic or pearlescent appearance. EP 2035209B1 discloses a preform and a container for a radiation-sensitive product and a method for making the same. U.S. Publication No. 2017 / 0306143A1 discloses a light-blocking composition and an article containing the same.
[0019] The references found above disclose articles having a pearlescent appearance (also described as lustrous, nacreous, or metallic), which is undesirable. Furthermore, these references demonstrate the use of incompatible polymers (e.g., polypropylene) that must be used at high loading levels greater than 5% and do not have a synergistic effect when used in combination with light scattering pigments. In summary, such references do not disclose how to produce an angle-homogeneous appearance with constant color across a wide viewing angle range and synergistically improve light blocking by using low loading levels of incompatible polymers, allowing for reduced additive loading, higher L*, and brighter white appearance.
[0020] Therefore, there is a need for low-cost, angularly uniform compositions made from immiscible polymers. Such compositions are desired to have anti-swirl behavior or any other properties (e.g., physical properties, recyclability, gloss, or reheatability) that provide whiteness and lightness without the typical compromise in light blocking. Summary of the invention
[0021] White articles made with phase separation materials are known to have a nacreous or pearlescent effect (i.e., an appearance that varies with angle). It has been discovered that the use of polymethylpentene and light scattering pigments has an unexpected synergistic effect for such components even at very low addition levels and produces a packaging wall having an appearance that varies with angle and excellent light blocking properties.
[0022] Such a wall comprises a polyester combined with oriented polymethylpentene and a light scattering pigment. From about 0.1% to about 5.0% by weight of the wall is polymethylpentene, and from about 0.1% to about 5.0% by weight of the wall is light scattering pigment. The ratio of polymethylpentene to light scattering pigment in the wall is from about 5:1 to about 1:5. In addition, the wall is angularly homogeneous.
[0023] Combining light scattering pigments with polymethylpentene synergistically increases light reflection, which therefore improves light blocking. Since the synergistic increase in light reflection does not occur until after orientation (e.g., blow molding), L* and whiteness index may be low before orientation. Due to the reduction in the amount of colorant and / or sunscreen, the composition exhibits anti-swirl behavior because lower concentrations may be easier to disperse. Therefore, the disclosed composition provides a low-cost composition with anti-swirl behavior that requires little sunscreen or colorant to produce a bright white color-homogeneous package.
[0024] In the absence of light scattering pigments, packages with extended plate-like light scattering surfaces have an angularly variable appearance, show large color variations across a range of viewing angles, and may be unrecognizable depending on lighting conditions and observer position. Adding light scattering pigments to a composition of a structural polymer (e.g., polyester) and polymethylpentene unexpectedly eliminates the angularly variable color with only small amounts of light scattering pigment (as low as 0.1%).
[0025] In certain embodiments of the present invention, the light scattering pigment is selected from aluminum trihydrate (aluminum hydroxide, Al(OH)3); titanium dioxide (TiO2); barium sulfate (BaSO4); zinc sulfide (ZnS); mica; ultramarine blue (PB 29); metal oxide particles such as Pigment Yellow 53 (PY 53), red iron oxide (PR 101), black iron oxide (PBlk 11), chrome green-black hematite (PG17), cobalt aluminate (PB 28); and combinations thereof.
[0026] Another effect of reducing the amount of pigment or colorant is better physical properties. Colorants and / or sunscreens can promote polymer degradation by increasing shear stress and introducing moisture in polymer processing. Additives also reduce the total amount of structural polymers that can contribute to physical properties. Degraded polymers may cause physical properties (such as maximum load, tensile strength or environmental stress cracking) to decline.
[0027] Another effect of reducing the amount of colorant and / or sunscreen is to improve reheating performance. Colorants and / or sunscreens commonly used to produce white packaging reflect light, including IR light commonly used to reheat packaging materials for thermoforming or bottle blowing. With less IR reflected light, the structured polymer will absorb more effectively and reheat more evenly. Since polymethylpentene produces reflections after orientation, the color and appearance of the oriented sample will be different from the non-oriented (i.e. amorphous) sample.
[0028] Another effect of reducing the amount of colorant and / or opacifier is to improve or maintain gloss. Colorants and / or opacifiers can affect surface smoothness when used at very high loadings, resulting in a less glossy appearance. Reducing the amount of colorant maintains surface smoothness and a highly glossy appearance.
[0029] Another effect of reducing the amount of colorant and / or opacifier is improved recyclability. Colorants and / or opacifiers can be considered as contaminants in the recycling stream. Since polymethylpentene does not show strong reflectivity until after orientation, recycling into non-oriented articles has less impact on recyclability than other pigments and / or colorants.
[0030] In certain embodiments of the present invention, the package wall may include a second pigment or colorant distinct from the light scattering pigment, wherein the second pigment is selected from the group consisting of dyes, pigments, thermochromic pigments, fluorescent pigments, pearlescent pigments, and metallic pigments, or combinations thereof.
[0031] In certain embodiments of the present invention, the incident light source at 45° is used between the 15° near specular reflection and the 110° far specular reflection according to DE. CMC The wall flop was measured to be less than 10 units.
[0032] In certain embodiments of the present invention, the polyester is selected from the group consisting of polyethylene terephthalate (PET), copolymers of PET, polybutylene terephthalate (PBT), copolymers of PBT, polylactic acid (PLA), polytrimethylene terephthalate (PTT), polyethylene naphthalate (PEN), polyethylene furandicarboxylate (PEF), polycyclohexanedimethylene terephthalate (PCT), copolymers of PCT, sulfonated polyesters, copolymers of polyesters, polycaprolactone (PCL), polyhydroxyalkanoate (PHA), and copolymers of PHA.
[0033] In certain embodiments of the invention, the polymethylpentene comprises from about 0.1% to about 3.0%, from about 0.2% to about 2.0%, or from about 0.2% to about 4.0% by weight of the wall.
[0034] In certain embodiments of the present invention, the ratio of polymethylpentene to light scattering pigment in the package wall is from about 4:1 to about 1:4, or from about 3:1 to about 1:3.
[0035] In certain embodiments of the present invention, the light scattering pigment is titanium dioxide (TiO2).
[0036] In certain embodiments of the invention, the walls block greater than about 90%, about 95%, about 98%, about 99%, or about 99.5% of light at wavelengths in the range of about 200 nm to about 1200 nm. In other embodiments, the walls block greater than about 90%, about 95%, about 98%, about 99%, or about 99.5% of light at wavelengths in the range of about 400 nm to about 700 nm.
[0037] In certain embodiments of the present invention, the L* value of the wall according to the CIELAB color space is greater than: about 75, about 80, or about 85.
[0038] In certain embodiments of the invention, the wall is a single layer container wall. In other embodiments, the wall is a multilayer container wall, wherein at least one layer comprises polyester, oriented polymethylpentene, and a light scattering pigment.
[0039] In certain embodiments, additional (i.e., components separate from the light scattering pigments) colorants are added to the wall, including: dyes, special effect pigments, or other additives such as UV absorbers, antioxidant stabilizers, dispersants, waxes, slip additives, other polymers, or other components such as thermochromic pigments, fluorescent pigments, pearlescent pigments, and metallic pigments.
[0040] In certain embodiments of the invention, polymethylpentene is oriented by injection stretch blow molding, extrusion blow molding, film or sheet uniaxial or biaxial orientation, film blowing, thermoforming or fiber spinning. There are no particular restrictions on orientation. Typically, a higher degree of orientation results in a higher reflective surface and higher light blocking.
[0041] Finally, a method of producing a packaging wall is disclosed whereby polyester, polymethylpentene, and a light scattering pigment are combined to produce a mixture having from about 0.1 wt % to about 5.0 wt % polymethylpentene and from about 0.1 wt % to about 5.0 wt % light scattering pigment. Furthermore, the ratio of polymethylpentene to light scattering pigment is from about 5:1 to about 1:5. The wall is then produced by subjecting the mixture to an orienting stress to orient the structural polymer.
[0042] In certain embodiments, the density of the mixture before being subjected to the orientation stress is equal to or less than the density of the polyester. In other embodiments, the density of the wall after being subjected to the orientation stress is equal to or less than the density of the polyester.
[0043] In one non-limiting embodiment, the product can be added to a container having a wall having oriented polyester, polymethylpentene and light scattering pigment and optionally other pigments and / or colorants. The container can then be sealed.
[0044] It is to be understood that both the foregoing general description and the following detailed description are exemplary and not restrictive of the invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 It is a diagram of the CIELAB L*, a*, b* color space;
[0046] Figure 2 is a graph of color measurement for angular flop;
[0047] Figure 3 is an exemplary embodiment of a mixture of immiscible polymers; and
[0048] Figure 4 is an exemplary embodiment of a mixture of immiscible polymers undergoing orientation. DETAILED DESCRIPTION
[0049] Embodiments disclosed herein include compositions that can be used for making bright white packaging. Embodiments include packaging walls, which include, are substantially composed of, or are composed of: polyester, about 0.1 % by weight to about 5.0 % by weight of polymethylpentene and about 0.1 % by weight to about 5.0 % by weight of light scattering pigment, wherein the ratio of polymethylpentene to light scattering pigment is about 5:1 to about 1:5, and the wall is homochromatic with angle. Once subjected to biaxial orientation stress (e.g., blow molding), packaging walls are exactly the bright white color greater than about 75 according to the L* value of CIELAB color scale. In addition, in some embodiments, the light blocking of the composition for the light in the wavelength of about 200nm to about 1200nm is greater than 90%.
[0050] Polyester structural polymer
[0051] As used herein, the term "structural polymer" refers to a polymer material that constitutes the majority of the composition and provides most of the mechanical properties to an article, such as a plastic container. Preferably, the structural polymer is a polyester polymer. Figure 3 and Figure 4 In the embodiment of the present invention, the structural polymer is indicated by reference numeral 100.
[0052] Any polyester is a candidate for use in the present invention. Polyesters formed from monohydric or polyhydric alcohols and acids or their esters encompass many different suitable types of polyesters for use in the present invention. The monomer units may be formed by the reaction of an aliphatic portion, an aromatic portion, or both. It is desirable that the polyester be transparent or translucent.
[0053] Non-limiting examples of polyesters include terephthalate esters, terephthalate glycol esters, lactides, (hydroxy)alkanoates, copolyesters of terephthalic acid residues, 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 1,4-cyclohexanedimethanol, and the like, or combinations thereof.
[0054] In addition, homopolyesters or copolyesters, such as homopolymers and copolymers of terephthalic acid and isophthalic acid, can be used. Linear polyesters can be produced by condensing one or more dicarboxylic acids or their lower alkyl diesters with one or more glycols, such as dimethyl terephthalate, terephthalic acid, isophthalic acid, phthalic acid, 2,5-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid or 2,7-naphthalene dicarboxylic acid, succinic acid, sebacic acid, adipic acid, azelaic acid, biphenyl carboxylic acid and hexahydroterephthalic acid, or bis-p-carboxyphenoxyethane, such as ethylene glycol, pentanediol and 1,4-cyclohexanedimethanol.
[0055] Among these various polyester candidates, terephthalates such as polyethylene terephthalate (PET) or polybutylene terephthalate (PBT), lactides such as polylactic acid (PLA), and hydroxyalkanoates such as polyhydroxybutyrate (PHB) or polyhydroxybutyrate-co-valerate (PHBV) are desirable due to commercial availability. Although PLA and PHBV are emerging as bio-derived thermoplastic polyesters that can replace PET in some cases, PET is preferred due to its ubiquity and cost. In some embodiments, PET can be blended with other polyesters.
[0056] Polymethylpentene
[0057] As used herein, "polymethylpentene" refers to a thermoplastic homopolymer or copolymer consisting primarily of 4-methyl-1-pentene units. Polymethylpentene may include copolymers with 1-decene, 1-hexadecene, 1-octadecene, or a combination thereof. Figure 3 and Figure 4 , polymethylpentene is designated by reference numeral 110 and is incompatible with the polyester structural polymer 100 and constitutes a minor dispersed phase. In a non-limiting embodiment, polymethylpentene 110 is present in an amount of about 0.1% to about 5.0% by weight of the composition.
[0058] When present in a wall for packaging, the polymethylpentene 110 is present at about 0.1 wt % to about 5.0 wt %, or about 0.1 wt % to about 3.0 wt %, or about 0.2 wt % to about 2.0 wt %, or about 0.2 wt % to about 4.0 wt %, or about 0.1 wt % to about 0.5 wt %, or about 0.1 wt % to about 0.7 wt %, or about 0.1 wt % to about 1.0 wt %, or about 0.5 wt % to about 2.0 wt %, based on the weight of the wall.
[0059] Reference Figure 3 and Figure 4Without being bound by any particular theory, it is believed that when the structured polymer 100 and the dispersed phase of polymethylpentene 110 are subjected to an orientation stress (e.g., blow molding), the rigidity and surface tension of the polymethylpentene 110 allow the structured polymer 100 to flow around the polymethylpentene 110. The polymethylpentene 110 maintains its shape within a reasonable tolerance, resulting in the formation of voids 120 within the structured polymer 100. The light scattering pigment is dispersed within the structured polymer 100 even though it may have been dispersed in the polymethylpentene 110 at one time. The light scattering pigment scatters light in a range of directions and destroys the angularly variable color appearance caused by the voids 120, thereby producing an angularly uniform color appearance. Therefore, when combined with the light scattering pigment in the composition for forming a container by an orientation process (e.g., blow molding), once oriented, the polymethylpentene 110 imparts an angularly uniform color appearance to the container wall.
[0060] In some embodiments, the compositions and packaging walls disclosed herein are free of polypropylene.
[0061] Light scattering pigments
[0062] As used herein, "light scattering pigment" refers to any inclusion within a structured polymer 100 or within an immiscible polymer that interacts with incident light by primarily diffracting light and optionally scattering and / or absorbing. Diffraction occurs due to the difference in refractive index between the light scattering pigment and the immiscible polymer or structured polymer 100. The light scattering pigment may only diffract, as in the case of titanium dioxide (TiO2), or the light scattering pigment may both scatter and absorb, as in the case of black iron oxide (PBlk 11). Some examples of light scattering pigments include titanium dioxide (TiO2); ultramarine blue (PB 29); metal oxide particles such as red iron oxide (PR 101), black iron oxide (PBlk 11), chrome green black hematite (PG 17) or cobalt aluminate (PB 28); aluminum trihydrate (Al(OH)3); barium sulfate (BaSO4); zinc sulfide (ZnS) or mica.
[0063] When present in a wall for packaging, the light scattering pigment is present at about 0.1 wt % to about 5.0 wt %, or about 0.1 wt % to about 4.0 wt %, or about 0.1 wt % to about 3.0 wt %, or about 0.2 wt % to about 2.0 wt %, or about 0.2 wt % to about 4.0 wt %, or about 0.1 wt % to about 0.5 wt %, or about 0.1 wt % to about 0.7 wt %, or about 0.1 wt % to about 1.0 wt %, or about 0.5 wt % to about 2.0 wt %, based on the weight of the wall.
[0064] In addition, the ratio of polymethylpentene to light scattering pigment is from about 5:1 to about 1:5, or from about 4:1 to about 1:4, or from about 3:1 to about 1:3, or from about 2.5:1 to about 1:2.5, or from about 2:1 to about 1:2, or from about 1.5:1 to about 1:1.5, or from about 1.25:1 to about 1:1.25, or from about 0.75:1 to about 3:1, or from about 0.5:1 to about 3:1, from about 0.75:1 to about 2:1, or from about 0.5:1 to about 2:1.
[0065] Chromatic flop
[0066] The angular flop of the surface 200 can be measured using a multi-angle spectrophotometer (e.g., MA-T12 from X-Rite). The color difference from the original light source 210 between the initial specular viewing angle 220, the near specular viewing angle 230, and the far specular viewing angle 240, as calculated using CIELAB DECMC, can be used to quantify the magnitude of the angular flop. The original light source 210 can approach the surface 200 at any desired angle. For example, Figure 2 As depicted, light source 210 may approach the surface at an incident angle of approximately 45 degrees. In addition, near specular viewing angle 230 forms an angle with initial specular viewing angle 220 that is less than the angle formed by far specular viewing angle 240 and initial specular viewing angle 220. For example, Figure 2 As depicted, the near specular viewing angle 230 may be 15 degrees and the far specular viewing angle 240 may be 110 degrees.
[0067] Colorants
[0068] Composition of the present invention optionally comprises at least one colorant.Colorant can absorb the first light wavelength range in the spectrum of the light wavelength of about 200nm to about 1200nm.Suitable colorant comprises any organic dye, organic pigment, inorganic dye and inorganic pigment commonly used as colorant in polymer application.The example of such colorant comprises the colorant of various colors shown below.Hereinafter, symbol "CI" means dye index.
[0069] Black colorants include, for example, carbon black, copper oxide, manganese dioxide, aniline black, activated carbon, non-magnetic ferrite, magnetic ferrite, and magnetite.
[0070] The yellow pigment includes CI Pigment Yellow 13, CI Pigment Yellow 14, CI Pigment Yellow 17, CI Pigment Yellow 74, CI Pigment Yellow 93, CI Pigment Yellow 155, CI Pigment Yellow 180, and CI Pigment Yellow 185, for example.
[0071] Orange colorants include red chrome yellow, molybdenum orange, permanent orange GTR, pyrazolone orange, vulcan orange, indanthrene Brilliant Orange RK, benzidine orange G, indanthrene Brilliant Orange GK, CI Pigment Orange 31, CI Pigment Orange 43, for example.
[0072] The red colorant includes CI Pigment Red 52, CI Pigment Red 53, CI Pigment Red 19, CI Pigment Red 48:1, CI Pigment Red 48:2, CI Pigment Red 48:3, CI Pigment Red 57:1, CI Pigment Red 122, CI Pigment Red 150, and CI Pigment Red 184, for example.
[0073] Violet colorants include, for example, CI Pigment Violet 23, manganese violet, fast violet B, and methyl violet lake.
[0074] The blue colorant includes CI Pigment Blue 15, CI Pigment Blue 15:2, CI Pigment Blue 15:3, CI Pigment Blue 15:4, CI Pigment Blue 16, and CI Pigment Blue 60, for example.
[0075] Green colorants include chrome green, chromium oxide, pigment green B, micalite green lake, final yellow green G, and CI Pigment Green 7, for example.
[0076] White colorants include compounds such as zinc powder, titanium oxide, antimony white, and zinc sulfide.
[0077] Colorants may include non-conventional pigments. Examples of such non-conventional (also called "effect pigments") are: thermochromic pigments, fluorescent pigments, pearlescent pigments, metallic pigments and combinations thereof. Such "effect pigments" are separate compounds relative to light scattering pigments.
[0078] Coloring agent can be used separately, or two or more kinds of coloring agents of different colors can also be used together.Multiple coloring agents of the same color system can also be used together.The ratio of optional coloring agent to structural polymer 100 is not particularly limited, and can be appropriately selected in a wide range according to various conditions (such as the type of structural polymer 100 or the desired characteristics of the desired color to be achieved).As an example, based on 100 parts by weight of structural polymer 100, the ratio of the coloring agent used for structural polymer 100 can be preferably 0.0001 parts by weight or 5 parts by weight or less, and more preferably 0.0004 parts by weight or more and 5 parts by weight or less.
[0079] L* Value
[0080] On the CIELAB L*, a*, b* color space, L* values greater than about 80 appear bright. In the present invention, the L* value of the composition after orientation can be about: 70, 75, 80, 85, 90, 95 or 97 to 99.5, which is generally a maximum. Before orienting the polymethylpentene, the L* value can have a lower range. In a preferred embodiment, the L* value of the wall of the white package is greater than 80 or greater than 85 or greater than 90 or greater than 95.
[0081] Light Blocking
[0082] Light blockage is a quantitative characteristic of the amount of light that is prevented from passing through a sample over a range of wavelengths. Light blockage can be measured as the average amount of light that is prevented from passing through the sample from 400nm to 700nm. Light blockage can also be measured as optical density. Optical density is the -log of the ratio of light that passes through the sample. 10 . This is useful for measuring samples with very high light blocking. For example, an optical density of 3 means that 99.9% of the light is prevented from passing through. In the present invention, the wall can prevent about: 75%, 80%, 85%, 90%, 95%, 97%, 98%, 99%, or 99.5% to 100% of the light from passing through the wall.
[0083] Spectrum of light wavelengths
[0084] The relevant spectrum of light blocked by the disclosed container is not limited to the visible spectrum. In fact, light within the ultraviolet spectrum and infrared spectrum may cause undesirable changes in the product. In a non-limiting example, the spectrum of light wavelengths blocked by the combination of structured polymer 100 and polymethylpentene, light scattering pigments and / or colorants includes: about 200nm to about 1200nm; about 250nm to about 1000nm; about 300nm to about 900nm; about 350nm to about 800nm; about 400nm to about 700nm; about 350nm to about 600nm; and 350nm to 550nm.
[0085] Blocking properties
[0086] The packaging may provide other barrier properties, such as barrier properties to moisture, oxygen, microorganisms, grease, or carbon dioxide. Indeed, in certain embodiments, the packaging wall may contain an oxygen scavenger. Examples of such oxygen scavengers are: polybutadiene-PET block copolymers with transition metal salts used as catalysts; polyalkylene glycols, copolymers thereof, and blends thereof; and copolyetheresters.
[0087] density
[0088] Polymethylpentene has the particular advantage of low density. Low density reduces overall part weight and results in cost savings. For example, the density of polymethylpentene is 0.83 g / cm 3, while the density of polyester terephthalate is 1.39 g / cm 3 . For example, by combining 5 parts of polymethylpentene with 100 parts of polyester terephthalate, the composite density is reduced by 3.1%. Since many plastic products are made to a specific volume, this results in a lower product weight and less polymer consumption. Light scattering pigments such as TiO2, BaSO4 or ZnS have very high densities, which can cause an increase in product weight when incorporated into structural polymers. For example, with the incorporation of 5 parts of TiO2, the composite density increases by 3.2%. Instead, using a combination of 5 parts of polymethylpentene and 5 parts of TiO2, for example, the total weight of the container is equal to the total weight of the PET container.
[0089] Packaging products
[0090] The white light blocking compositions disclosed herein can be used to manufacture packaging articles having various forms. Suitable articles include, but are not limited to, flexible sheet films, flexible bags, pouches, semi-rigid and rigid containers such as bottles (e.g., PET bottles), trays, and containers.
[0091] Typical flexible films and bags include those used for packaging various food items and may be composed of one layer or multiple layers to form an entire film or bag-like packaging material. The white light blocking composition of the present invention may be used in one layer, some layers, or all layers of such packaging materials.
[0092] Typical rigid or semi-rigid products include plastic, paper or paperboard containers, such as those for milk, juice, soft drinks, alcohol, and thermoformed trays or cups with a thickness in the range of about 100 μm to about 1000 μm. The wall of such products may include a single material layer or multiple material layers. The product may also be in the form of a bottle or can, or a crown, a cover, a crown or cover liner, a plastisol or a gasket. The white light blocking composition of the present invention can be used as an integral layer or a part of a semi-rigid or rigid packaging product formed, or as an outer coating or inner coating or lining of a semi-rigid or rigid packaging product formed. As a liner, the white light blocking composition can be extruded into a film together with the rigid product itself, such as in a coextrusion, extrusion coating or extrusion lamination process, so as to form a liner in situ during the production of the product; or it can be adhered to the outer surface of the product by heating and / or pressure, by an adhesive or by any other suitable method after the product is produced.
[0093] In a non-limiting embodiment, the container comprises a bottom connected to the sidewall that limits the inner space. The container can be formed by the composition that white light blocks. In such an embodiment, the container can also include a top, which includes an opening connected to the sidewall that optionally has a seal for opening. Photosensitive products (such as food such as milk) can be placed in the inner space. The composition that white light blocks can surround all or part of the container or is limited to opening. Finally, the container can be oxygen-resistant.
[0094] In one non-limiting embodiment of the present invention, the composition of the present invention (e.g., structural polymer substrate, polymethylpentene and light scattering pigment, and optionally other pigments and / or colorants) can be used to form a monolayer bottle. In another non-limiting embodiment of the present invention, the composition of the present invention can form one or more layers of a multilayer bottle.
[0095] In addition to articles suitable for packaging food and beverages, articles used to package other products may also benefit from the present invention. Such products may include pharmaceuticals, light-sensitive medical products, audio / visual films, etc. Product labeling purposes may also require that the packaging be bright white so that a particular trade dress can be printed on the container.
[0096] Product wall
[0097] In some embodiments, the present invention relates to the use of the compositions described herein as a component of a wall used in a desired white packaging for photosensitive materials.
[0098] The wall can be a rigid wall, a flexible sheet, or an adhesive film. It can be homogeneous or a laminate or coated with other polymers. If it is laminated or coated, the white color and light blocking properties can be retained in a layer of the wall that alone does not function satisfactorily (e.g., not bright white enough). However, if the layer is combined with other light-blocking white layers, the article can function satisfactorily (e.g., appear bright white and block light).
[0099] Package wall of the present invention can be single layer or multilayer structure.In some embodiments using multilayer wall, outer layer and internal layer can be structural layer, have one or more protective layers comprising structure and polymethylpentene between them.In some embodiments, outer layer and internal layer comprise polyolefin, polyester or nylon.In certain embodiments, preferred single layer design.Such layer can have the advantage of simple manufacturing and cost.
[0100] Manufacturing method
[0101] Compositions of the present invention can be manufactured by mixing polyester structural polymers (such as PET) with polymethylpentene, light scattering pigments and optional other pigments and / or colorants. Such compositions can be manufactured by any method known to those skilled in the art. In certain embodiments, before mixing, some or part of light scattering pigments and / or colorants may be present in the basic structural polymer or the polymethylpentene. The residual sunscreen or colorant can exist as a result of a recovery process (i.e., recycling). In some embodiments, structural polymers, polymethylpentene, light scattering pigments and optional other pigments and / or colorants are mixed by tumbling in a hopper. Other optional ingredients can be added during this mixing process, or added to the mixture after the above-mentioned mixing, or added to the individual components before the above-mentioned mixing step.
[0102] The compositions of the present invention can also be prepared by adding the ingredients separately and mixing the ingredients before melt processing the composition to form an article. In some embodiments, mixing can be just before the melt processing zone (meltprocess zone). In other embodiments, one or more ingredients can be premixed in a separate step before all the ingredients are put together.
[0103] Composition of the present invention can also be produced by melt kneading. In such non-limiting embodiments, polyester structure polymer, polymethylpentene, light scattering pigment and optional colorant (and other components, if present) are melt kneaded to prepare the resin product kneaded. Melt kneading is carried out substantially without using organic solvent, yet, a small amount of organic liquid (comprising organic solvent) can be present as processing aid to for example control the dusting (dusting) of polymer. The polymer composition kneaded can optionally include additives such as release agents such as wax and additives such as charge control agents. Additives are kneaded together with polyester structure polymer, polymethylpentene, light scattering pigment and optional colorant and are dispersed in the polymer composition kneaded.
[0104] In another aspect, the present invention provides a package, whether rigid, semi-rigid, foldable, covered or flexible or a combination of these, comprising a wall formed from the composition described herein. Such a package can be formed by methods well known to those skilled in the art.
[0105] Among the techniques that can be used to make the articles, molding, stretch blow molding, extrusion, thermoforming, extrusion blow molding, biaxial orientation and (especially for multilayer structures) coextrusion and lamination using adhesives to tie the layers are common. Orientation of the polymer (e.g. by stretch blow molding) is particularly attractive for polyesters because of the known mechanical advantages that result.
[0106] The melt processing zone for making articles can be operated under conventional conditions that effectively make the expected articles (e.g., preforms, bottles, trays, and other articles described below). In one embodiment, such conditions are effective for processing the melt without substantially increasing the IV of the melt and it is not effective in promoting transesterification reactions. In some preferred embodiments, suitable operating conditions for effectively establishing physical blends of structural polymers, polymethylpentene, light scattering pigments, and colorants are temperatures in the melt processing zone in the range of about 200° C. to about 300° C. in less than about 6 minutes of total cycle time, and generally without applying vacuum and under a positive pressure of about 0 psig to about 900 psig. In some embodiments, the residence time of the melt on the screw can be in the range of about 1 minute to about 4 minutes.
[0107] Specific articles include preforms, trays, containers, and rigid packaging for packaging food, beverages, cosmetics, medicines, and personal care products that are expected to be bright white packaging and need to block light. The example of a beverage container is a bottle for holding beer and juice, and the present invention is particularly useful in bottle applications for holding milk or any other beverage, where it is expected that the packaging is bright white and light adversely affects the flavor, fragrance, performance (preventing vitamin degradation) or color of the beverage. Rigid packaging includes a food tray and a lid. The example of a food tray application includes a double bakeable food tray or a refrigerated food tray in a base container and a lid (whether a thermoformed lid or a film), wherein when exposed to light, the freshness of the food contents may decrease. It is also found that the composition of the present invention is used in the manufacture of a container for a drug or medical device.
[0108] Masterbatch
[0109] In another aspect, the composition of the present invention can be used as a masterbatch blended with a polymer or a component containing a polymer. In such a composition, for example, the concentration of polymethylpentene, light scattering pigments and optional other pigments and / or colorants will be higher so that the final blended product has a suitable amount of these components. The masterbatch can also include a certain amount of polyester structural polymers blended with the masterbatch. In other embodiments, the masterbatch can include a polyester structural polymer that is compatible with a second structural polymer to be blended into the masterbatch. In other embodiments, the masterbatch can include polymethylpentene and a second functional polymer, one or both of which may be incompatible with the structural polymer.
[0110] definition
[0111] In this specification and the appended claims, reference will be made to a number of terms which shall be defined to have the following meanings.
[0112] As used herein, the terms "a", "an", and "the" etc. refer to both the singular and the plural, unless the context clearly indicates otherwise. For example, "a bottle" refers to a single bottle or more than one bottle.
[0113] In addition, as used herein, the description of one or more method steps does not exclude the presence of additional method steps before or after the steps of the combination. Additional steps may also be intermediate steps of the described steps. In addition, it should be understood that the letter markings of process steps or components are convenient means for identifying individual activities or components, and the letter markings may be arranged in any order.
[0114] In the case of numerical ranges in this application, it should be understood that the range includes all integers and fractions thereof between the range limits. Numerical ranges clearly include numbers less than the endpoints and numbers between the ranges. For example, a range from 1 to 3 includes integers 1, 2, and 3 and any fractions between these integers.
[0115] As used herein, "masterbatch" refers to a mixture of polymethylpentene, light scattering pigments and optional colorants with optional structural polymers, and optional other polymers and optional other additives, which is typically diluted with at least additional structural polymer before forming an article. In this way, the concentration of polymethylpentene, light scattering pigments and / or colorants is higher than the concentration in the formed article.
[0116] The following examples are included to illustrate preferred embodiments of the present invention, which relate to the usability of PET base resins blended with polymethylpentene and light scattering pigments to make bright white packaging. It should be appreciated by those skilled in the art that the techniques disclosed in the following examples represent techniques discovered by the inventors to function well in the practice of the present invention, and thus can be considered to constitute modes for its practice. However, in light of the present disclosure, it should be appreciated by those skilled in the art that many changes can be made to the specific embodiments disclosed and still obtain like or similar results without departing from the spirit and scope of the present invention.
[0117] Example
[0118] The following materials are referenced in Table 1 below:
[0119] PMP - polymethylpentene, grade RT-31 from Mitsui Chemicals America, Inc., the grade used in Control 5 and Example 6 was RT-18 from Mitsui Chemicals America, Inc.
[0120] PET - Polyethylene terephthalate, grade PQB-4 from Polyquest, Inc., 0.80 IV bottle grade polymer.
[0121] PETG - diol modified copolyester, Skygreen K2012 grade from SK Chemicals.
[0122] TiO2 - Titanium dioxide, light scattering pigment, CI Pigment White 6, Grade CR-834 from Tronox Limited, general purpose rutile grade.
[0123] PPRO - Polypropylene from Plastics Solutions, Inc. HP 3500 grade, 35 melt flow homopolymer.
[0124] ZnS - Zinc Sulfide, Light Scattering Pigment, CI Pigment White 7, Sachtloth HD-S grade from Venator.
[0125] PBlk 7 - Carbon black, Black Pearls 4350 from Cabot.
[0126] PBlk 11 - Black Iron Oxide, CI Pigment Black 11, Bayferrox 318M grade from Lanxess.
[0127] SB 104-CI Solvent Blue 104, a non-light scattering colorant, is a Keyplast Blue KR grade from Milliken.
[0128] TiO2 MB-65% TiO2 and 35% PET were extruded in a 25 mm co-rotating twin screw extruder at 300 RPM and 250°C and cut into pellets.
[0129] ZnS MB-50% ZnS and 50% PET were extruded in a 25 mm co-rotating twin screw extruder at 300 RPM and 250°C and cut into pellets.
[0130] SB 104MB-10% SB 104 and 89.3% PETG, 0.5% epoxidized soybean oil and 0.2%
[0131] BNX 1010 antioxidant stabilizer grade was extruded in a 25 mm co-rotating twin screw extruder at 300 RPM and 250°C and cut into pellets.
[0132] Examples 6, 7a, 7b, 7c, 7d, 8a, 8b, 8c, 9 and 10 all used pre-made masterbatches. The composition of each masterbatch is listed in Table 1. All masterbatch compositions were extruded at 300 RPM in a 25 mm co-rotating twin screw extruder and cut into pellets. Each masterbatch was added to the feed port of the extrusion step of the blow molding process in the amount shown in Table 1 below:
[0133] Table 1: Masterbatch samples used in Examples and Comparative Examples
[0134]
[0135] For all samples, the additives were mixed at the feed throat of the extrusion step of the blow molding process on a Nissei ASB 50M blow molding machine. The bottles were blown to an axial orientation of 3.3x and a circumferential orientation of 3.3x, with an overall wall orientation of 10.9x 2 The final composition of each sample is shown in Table 2 below:
[0136] Table 2: Final bottle composition
[0137] name PMP TiO2 PPRO ZnS PBlk 7 PBlk 11 SB 104 PET Example 1a 6.00% 94.00% Embodiment 1b 7.80% 92.20% Example 1c 3.00% 3.90% 93.10% Example 1d 2.40% 3.12% 94.48% Example 2a 10.00% 90.00% Example 2b 3.25% 96.75% Example 2c 1.63% 5.00% 93.38% Example 3 1.50% 0.50% 98.00% Example 4 1.50% 0.25% 98.25% Example 5 1.50% 0.60% 97.90% Example 6 2.50% 2.50% 95.00% Example 7a 6.00% 0.06% 93.94% Example 7b 7.80% 0.06% 92.14% Example 7c 3.00% 3.90% 0.06% 93.04% Example 7d 3.00% 3.90% 0.03% 93.07% Example 8a 10.00% 0.06% 89.94% Example 8b 3.25% 0.06% 96.69% Example 8c 1.63% 5.00% 0.06% 93.32% Example 9 0.750% 2.25% 97.00% Example 10 0.750% 2.25% 0.02% 96.98%
[0138] The above reference composition was then subjected to orientation forces and its appearance characteristics were measured. The measurement results are shown in the following Table 3:
[0139] Table 3: Measured appearance characteristics
[0140]
[0141] Embodiments 1a, 1b, 1c, 1d
[0142] Examples 1a, 1b, 1c and 1d show that there is synergy when the oriented packaging wall combines PMP and light scattering pigment. Example 1a using only PMP has an appearance of color change with angle and 96.2% light blocking. Example 1b using only light scattering pigment requires a very high level of masterbatch to achieve the same light blocking of 96.3%. By using half of the light blocking contribution from Example 1a and Example 1b, those skilled in the art will foresee the same light blocking performance. However, Example 1c shows that light blocking is improved while maintaining a color-homogeneous appearance with angle. Example 1d shows synergy by reducing the total amount of both PMP and light scattering pigment by 20% while still matching the light blocking of Example 1a and Example 1b and maintaining a color-homogeneous appearance with angle.
[0143] Comparative Examples 2a, 2b, 2c
[0144] Embodiment 2a, embodiment 2b and embodiment 2c show that there is no synergy when oriented packaging wall combines different olefin polymers and light scattering pigment. Embodiment 2a using PPRO needs very high load level and still can't realize light blocking similar to embodiment 1. Only embodiment 2b using light scattering pigment matches the light blocking of embodiment 2a.By using half light blocking contribution from embodiment 1a and embodiment 1b, those skilled in the art will foresee identical light blocking performance.Yet embodiment 2c illustrates that light blocking is slightly worse than embodiment 2a and embodiment 2b.
[0145] Example 3 and Comparative Example 4
[0146] Example 3 and Comparative Example 4 show that at a ratio of PMP to light scattering pigment of about 3:1, a flop appearance is produced and the color is maintained across a range of viewing angles. However, increasing the PMP:light scattering pigment up to about 6:1 produces flop and the color is no longer maintained across a range of viewing angles.
[0147] Comparative Example 5
[0148] Comparative Example 5 shows that the use of non-light scattering pigments does not provide an angularly uniform appearance. The added colorant must be a light scattering pigment, not an absorbing dye.
[0149] Example 6
[0150] Example 6 shows that in the case of Example 6, other light scattering pigments, CI Pigment White 7, zinc sulfide, can be used.
[0151] Examples 7a to 7d
[0152] Examples 7a, 7b and 7c show that Examples 7a, 7b and 7c use the same structural polymer, PMP and light scattering pigment as Examples 1a, 1b and 1c, but add 0.060% of PBlk 11 to the final composition. Since the light blocking is so high, the optical density can be used to measure the synergy of light blocking. Example 7d shows that due to the synergy between PMP and TiO2, the same light blocking can be achieved, but the amount of PBlk 11 is reduced, resulting in a higher L* and brighter white while maintaining a uniform color appearance with angle.
[0153] Comparative Examples 8a to 8c
[0154] Examples 8a, 8b and 8c used the same structural polymer, PPRO and light scattering pigment as Examples 2a, 2b and 2c, but added 0.060% of PBlk 11 to the final composition. Since there is no synergistic effect between PPRO and TiO2, the L* appearance of Example 7c is lower than that of Examples 8a and 8b.
[0155] Examples 9 and 10
[0156] Examples 9 and 10 show that there is a synergistic effect when the oriented package wall combines PMP and light scattering pigments. Example 9 using PMP and TiO2 has a color flop appearance and 91.5% light blocking. Example 10 uses PMP, TiO2 and carbon black (PBlk 7) and also has a color flop appearance but also blocks all light.
[0157] Although illustrated and described above with reference to certain specific embodiments, the present invention is not intended to be limited to the details shown. On the contrary, various modifications can be made in detail within the scope and scope of the equivalents of the claims and without departing from the spirit of the present invention. For example, it is clearly intended that all ranges widely listed in this document include within their scope all narrower ranges that fall within the broader range. It is also clearly intended that the steps of the method of using the various compositions disclosed above are not limited to any particular order.
[0158] The present invention also includes the following embodiments:
[0159] Embodiment 1. A packaging wall comprising:
[0160] Polyester;
[0161] from about 0.1 wt % to about 5.0 wt % polymethylpentene; and
[0162] from about 0.1 wt. % to about 5.0 wt. % of a light scattering pigment,
[0163] wherein the ratio of polymethylpentene to light scattering pigment is from about 5:1 to about 1:5, and wherein the wall is angularly homogeneous.
[0164] Embodiment 2. A wall according to embodiment 1, wherein the incident light source at 45° is used at DE between 15° near specular reflection and 110° far specular reflection. CMC The measured flop was less than 10 units.
[0165] Embodiment 3. A wall according to embodiment 1, wherein the polyester is selected from: polyethylene terephthalate (PET) and copolymers, polybutylene terephthalate (PBT) and copolymers, polylactic acid (PLA), polytrimethylene terephthalate (PTT), polyethylene naphthalate (PEN), polyethylene furandicarboxylate (PEF), polycyclohexanedimethylene terephthalate (PCT) and copolymers, sulfonated polyesters and copolymers, polycaprolactone (PCL) or polyhydroxyalkanoate (PHA) and copolymers.
[0166] Embodiment 4. The wall of Embodiment 3, wherein the polyester is polyethylene terephthalate.
[0167] Embodiment 5. A wall according to embodiment 3, wherein the light scattering pigment is selected from: titanium dioxide (TiO2); ultramarine blue (PB29); metal oxide particles such as red iron oxide (PR101), black iron oxide (PBlk11), chrome green-black hematite (PG 17) or cobalt aluminate (PB28); aluminum trihydrate (Al(OH)3); barium sulfate (BaSO4); zinc sulfide (ZnS) or mica.
[0168] Embodiment 6. The wall according to embodiment 5, wherein the light scattering pigment contained in the composition is titanium dioxide (TiO2).
[0169] Embodiment 7. The wall of Embodiment 1, wherein the wall blocks greater than about 90% of light for light having a wavelength in the range of about 400 nm to about 700 nm.
[0170] Embodiment 8. The wall of Embodiment 1, wherein the wall has an L* value of greater than about 75 according to the CIELAB color space.
[0171] Embodiment 9. A wall according to embodiment 1, wherein the wall is a single-layer container wall.
[0172] Embodiment 10. The wall of Embodiment 1, wherein the composition further comprises a second pigment or colorant selected from the group consisting of dyes, thermochromic pigments, fluorescent pigments, pearlescent pigments, metallic pigments, and combinations thereof.
[0173] Embodiment 11. A wall according to embodiment 1, wherein the structural polymer is polyethylene terephthalate (PET), polymethylpentene constitutes about 0.1 wt % to about 5.0 wt % of the wall, the light scattering pigment is titanium dioxide constituting about 0.1 wt % to about 5.0 wt % of the wall, the ratio of PMP to light scattering pigment is 5:1 to 1:5, the L* value of the wall is greater than 75 according to the CIELAB color scale, and the wall blocks more than 90% of light for light with a wavelength in the range of 400 nm to 700 nm.
[0174] Embodiment 12. A wall according to embodiment 1, wherein the structural polymer is polyethylene terephthalate (PET), polymethylpentene is present at 0.1% to 3.0%, the light scattering pigment is titanium dioxide present at 0.2% to 4.0%, the ratio of PMP to light scattering pigment is 3:1 to 1:3, the L* value of the wall is greater than 80 according to the CIELAB color scale, and the wall blocks more than 98% of light for light with a wavelength in the range of 400nm to 700nm.
[0175] Embodiment 13. A packaging wall is manufactured by the following steps:
[0176] mixing a polyester, a polymethylpentene, and a light scattering pigment to produce a mixture, wherein the polymethylpentene comprises from about 0.1 wt % to about 5.0 wt % of the mixture, the light scattering pigment comprises from about 0.1 wt % to about 5.0 wt % of the mixture, and the ratio of polymethylpentene to light scattering pigment in the mixture is from about 5:1 to about 1:5; and
[0177] The mixture is subjected to an orientation stress to produce a wall having an angularly uniform color appearance.
[0178] Embodiment 14. A wall made according to the method of Embodiment 13, wherein the density of the mixture before being subjected to the orientation stress is equal to or less than the density of the polyester.
[0179] Embodiment 15. A wall made according to the method of Embodiment 13, wherein the density of the wall after being subjected to an orientation stress is equal to or less than the density of the polyester.
[0180] Embodiment 16. A wall made according to the method of Embodiment 13, wherein the orienting stress is selected from the group consisting of: blow molding, uniaxial or biaxial sheet orientation, thermoforming, or fiber spinning.
[0181] Embodiment 17. A method of producing a container wall, comprising:
[0182] mixing a polyester, a polymethylpentene, and a light scattering pigment to produce a mixture, wherein the polymethylpentene comprises from about 0.1 wt % to about 5.0 wt % of the mixture, the light scattering pigment comprises from about 0.1 wt % to about 5.0 wt % of the mixture, and the ratio of polymethylpentene to light scattering pigment in the mixture is from about 5:1 to about 50:1; and
[0183] The mixture is subjected to an orientation stress to produce the wall, wherein the wall is angularly homogeneous.
[0184] Embodiment 18. A method for producing a container wall according to embodiment 17, wherein the density of the mixture before being subjected to orientation stress is equal to or lower than the density of the polyester.
[0185] Embodiment 19. A method of producing a container wall according to Embodiment 17, wherein the density of the wall after being subjected to orientation stress is equal to or lower than the density of the polyester.
[0186] Embodiment 20. The method for producing a container wall according to embodiment 17, wherein the orientation stress is selected from the group consisting of: blow molding, uniaxial or biaxial sheet orientation, thermoforming or fiber spinning.
Claims
1. A packaging product wall, comprising: Polyester; 0.1 wt % to 5.0 wt % polymethylpentene, based on the total weight of the wall; and 0.1 to 5.0 wt. %, based on the total weight of the wall, of a light scattering pigment that interacts with incident light primarily by diffracting the light, wherein the ratio of polymethylpentene to light scattering pigment is 5:1 to 1:5, and The incident light source was 45° between the near specular reflection of 15° and the far specular reflection of 110°, and the CIELAB DE CMC The wall has a goniochromaticity of less than 10 units as measured.
2. The packaging article wall according to claim 1, wherein the polyester is selected from: polyethylene terephthalate, copolymers of polyethylene terephthalate, polybutylene terephthalate, copolymers of polybutylene terephthalate, polylactic acid, polytrimethylene terephthalate, polyethylene naphthalate, polyethylene furandicarboxylate, polycyclohexane dimethyl terephthalate, copolymers of polycyclohexane dimethyl terephthalate, sulfonated polyesters, copolymers of polyesters, polycaprolactone, polyhydroxyalkanoate and copolymers of polyhydroxyalkanoate.
3. The packaging article wall of claim 2, wherein the polyester is polyethylene terephthalate.
4. The packaging article wall of claim 1, wherein the light scattering pigment is selected from the group consisting of titanium dioxide, ultramarine blue, metal oxide particles, aluminum trihydrate, barium sulfate, zinc sulfide, and mica.
5. The packaging article wall according to claim 4, wherein the metal oxide particles are selected from the group consisting of red iron oxide, black iron oxide, chrome green-black hematite and cobalt aluminate.
6. The packaging article wall of claim 4, wherein the light scattering pigment is titanium dioxide.
7. The packaging article wall of claim 1, wherein the wall further comprises a second colorant selected from the group consisting of dyes, thermochromic pigments, fluorescent pigments, pearlescent pigments, metallic pigments, and combinations thereof.
8. The packaging product wall according to claim 1, in: (a) the wall blocks light by 75% or more for light having a wavelength in the range of 400 nm to 700 nm; or (b) The L* value of the wall according to the CIELAB color space is greater than 75.
9. A packaging article comprising a packaging article wall according to any one of claims 1 to 8.
10. The packaging product according to claim 9, wherein the product is: (a) Films, bags, sachets or trays; (b) a bottle, can, crown, cap, crown liner, cap liner or gasket; or (c) External coatings, internal coatings or linings.
11. The packaging article of claim 9, wherein the packaging article is a film and / or is flexible.
12. The packaging article of claim 9, wherein the packaging article comprises a plurality of layers.
13. A packaging article according to claim 12, wherein a first layer of the packaging article comprising the packaging article wall is laminated to a second layer.
14. A method of manufacturing a packaging product, The following steps are involved: (a) mixing a polyester, a polymethylpentene, and a light scattering pigment that interacts with incident light primarily by diffracting the light to form a mixture, wherein the mixture comprises 0.1 wt % to 5.0 wt % of the polymethylpentene, based on the total weight of the mixture, and 0.1 wt % to 5.0 wt % of the light scattering pigment, based on the total weight of the mixture, and wherein the ratio of polymethylpentene to light scattering pigment in the mixture is 5:1 to 50:1; and (b) subjecting the mixture to orientation to produce the packaging article, wherein the mixture is oriented at a 45° incident light source between 15° near specular reflection and 110° far specular reflection using a CIELAB DE CMC The packaging article has a goniochromaticity of less than 10 units.
15. The method according to claim 14, in: (a) the density of the blend before being oriented or the density of the packaging article after being oriented is equal to or less than the density of the polyester; (b) the orientation is selected from the group consisting of blow molding, uniaxial or biaxial sheet orientation, thermoforming and fiber spinning; or (c) The orientation is selected from the group consisting of: molding, extrusion, extrusion blow molding, biaxial orientation, coextrusion and lamination.
16. The method of claim 14, wherein step (b) comprises coextrusion to produce a film that is attached to another article.