Electroluminescent fiber and melt coating preparation method thereof

By combining melt extrusion and solution coating methods, the problems of uneven coating and solvent pollution in the preparation of luminescent fibers are solved, and efficient, low-cost, green and environmentally friendly electroluminescent fiber preparation is achieved, which is suitable for industrial production and smart wearables. field of application.

CN114990882BActive Publication Date: 2024-10-29FUDAN UNIVERSITY

Patent Information

Application Number
CN202210444431.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-25
Publication Date
2024-10-29
Estimated Expiration
2042-04-25

AI Technical Summary

Technical Problem

Existing luminescent fiber preparation methods have problems such as surface tension mismatch leading to uneven coating, use of organic solvents to pollute the environment, and low production efficiency, making it difficult to achieve large-scale preparation and industrial production.

Method used

The melt extrusion process is combined with the solution coating method. By presetting the conductive fiber in the twin-screw extruder, the thermoplastic material and the electroluminescent material are melted and blended, and then extruded and stretched to form a skin-core structure, which is air-cooled or water-cooled. The luminescent fiber is formed to achieve continuous preparation, and the thickness of the luminescent active layer is controlled by regulating the die size and stretching speed.

Benefits of technology

It achieves the continuous large-scale preparation of electroluminescent fibers, avoids the use of solvents, reduces costs, and improves production efficiency. The prepared fibers are soft and weavable, suitable for industrial production, have green and environmentally friendly characteristics, and are suitable for functional clothing and smart wearables. Wearable devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114990882B_ABST
    Figure CN114990882B_ABST
Patent Text Reader

Abstract

The present invention relates to an electroluminescent fiber and a method for preparing the same by melt coating. The method comprises the following steps: (1) loading a luminescent active layer: physically blending a thermoplastic elastomer polymer and an electroluminescent active material in a melt coating device, and then melt coating the mixture on a conductive fiber substrate, and then cooling and solidifying the mixture online to obtain a conductive fiber coated with an electroluminescent active layer; (2) loading a fiber external electrode: loading the external electrode on the conductive fiber coated with the electroluminescent active layer in a twisted or twisted manner to obtain an electroluminescent fiber; (3) insulating packaging: melt coating a transparent insulating polymer on the outside of the electroluminescent fiber to obtain an electroluminescent fiber. Compared with the prior art, the luminescent fiber prepared by the present invention can reach a maximum of 200 cd / m 2 The luminous intensity is high and it can work normally after washing and bending. The luminous fiber has good flexibility and can be further woven into luminous fabrics, which has great application prospects in the field of smart wearable electronic devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of functional textiles, and in particular to an electroluminescent fiber and a melt-coating preparation method thereof. Background Art

[0002] As a new functional textile material, electroluminescent fiber has attracted extensive attention from the scientific and industrial communities. Clothing containing luminescent materials plays an important role in transportation, firefighting, fashion design, stage performances and other fields. Currently, the luminescent fibers on the market are mostly luminous fibers and fluorescent fibers. They mainly absorb energy through light and then convert it into light radiation. Generally, they are made of polyester, nylon or polypropylene as the base material, and rare earth long afterglow luminescent materials and nano-level functional additives are added. The light conversion functional fiber is made through a special spinning process. The fiber has various colors when there is visible light, and can emit various colors of light when there is no visible light.

[0003] At present, the preparation of luminescent fibers mostly adopts solution coating. On the one hand, due to the surface tension mismatch between the luminescent slurry and the conductive fiber substrate, it is easy to cause problems such as beading and uneven coating; on the other hand, the use of organic solvents in some slurries is easy to pollute the environment; secondly, the solution method often requires multiple steps of coating process to obtain functional devices, with low production efficiency, which is not conducive to large-scale preparation. Summary of the invention

[0004] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and provide an electroluminescent fiber and its melt coating preparation method which are colorful, soft and weavable, simple in technology, efficient, mild in conditions, low in cost, green, economical and environmentally friendly, suitable for industrial production.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] The inventors understand that the melt extrusion process is an efficient, continuous, low-cost, and widely adaptable molding and processing method, and is a relatively mature technology in the field of polymer material processing. The advantages of melt extrusion such as continuous production, high production efficiency, wide application range, and simple equipment determine the important position of extrusion molding in polymer processing.

[0007] Based on the above problems, this technology combines the invented melt extrusion process with the solution coating method, and creatively proposes a new method for preparing functional devices, namely the melt coating method. The process first pre-places conductive fibers in a twin-screw extruder, then melts and blends the thermoplastic material and the electroluminescent active material, extrudes and stretches them onto the surface of the fiber electrode to form a skin-core structure, and finally uses air cooling or water cooling to shape the luminescent fiber and collect it on a reel. The thickness of the luminescent active layer is effectively controlled by the designed die size and stretching speed. The use of this new process not only makes it more convenient and quick to realize the continuous large-scale preparation of devices, but also does not use any solvents, truly embodying the concept of green environmental protection. The prepared weavable luminescent fibers have important application value in functional clothing, and are expected to bring new technological upgrades to the field of wearable smart devices, as follows:

[0008] A method for preparing an electroluminescent fiber by melt coating, the method comprising the following steps:

[0009] (1) Loading the luminescent active layer: physically blending the thermoplastic elastomer polymer and the electroluminescent active material in a melt coating device, then melt coating the polymer on the conductive fiber substrate, and then cooling and solidifying the conductive fiber online to obtain the conductive fiber coated with the electroluminescent active layer;

[0010] (2) Loading the fiber external electrode: Loading the external electrode on the conductive fiber coated with the electroluminescent active layer in a twisted or twisted manner to obtain the electroluminescent fiber;

[0011] (3) Insulation packaging: A transparent insulating polymer is melt-coated on the outside of the electroluminescent fiber to obtain the electroluminescent fiber.

[0012] Furthermore, the conductive fiber includes one or more of metal conductive fiber, metal-particle-plated chemical fiber, ion gel fiber, and conductive polymer composite fiber;

[0013] The diameter of the conductive fiber is 50-300 μm, preferably 100-200 μm; the conductivity of the conductive fiber is 10 -4 -10 4 S / cm, preferably 10 -3 -10S / cm.

[0014] Furthermore, the thermoplastic elastomer polymer is a solid resin, including fluororesin, cyanoresin, polystyrene, ABS, polytetrafluoroethylene, polyarylate, polyurethane resin or polyamide, with a weight average molecular weight (Mw) of 50,000-150,000; the thermoplastic elastomer polymer accounts for 20-80wt% in the electroluminescent active layer, preferably 30-50wt%.

[0015] Further, the electroluminescent active material is an inorganic electroluminescent material, including CaS, SrS, ZnS, CaGa2S4, SrGa2S4, SiO2:Ge, SiO2:Er, GaN or Zn2SiO4;

[0016] The particle size of the electroluminescent active material is 10-50 μm, preferably 20-40 μm, and the proportion of the electroluminescent active material in the electroluminescent active layer is 20-80 wt %, preferably 30-50 wt %.

[0017] Furthermore, the outer electrode is a metal wire, including a copper wire, a steel wire, a titanium wire or a tungsten wire; the diameter of the metal wire is 10-100 μm, preferably 30-70 μm, and the conductivity is 10 -4 -10 4 S / cm, preferably 10 -3 -10S / cm.

[0018] Furthermore, the transparent insulating polymer is a solid transparent resin selected from SBS, epoxy resin, acrylate resin, polyurethane resin, polytetrafluoroethylene resin or silicone resin, and the weight average molecular weight of the solid transparent resin is 20,000-100,000.

[0019] Furthermore, the thickness of the electroluminescent active layer is 20-150 μm, preferably 40-100 μm, and the thickness of the coated transparent insulating polymer is 10-80 μm, preferably 20-50 μm.

[0020] Furthermore, the coating process steps of step (3) include melt extrusion, air cooling and winding, the melting temperature is 50-180°C, preferably 80-140°C, the time is 10-30min, preferably 15-25min; the air cooling temperature is 5-30°C, preferably 10-20°C, the air cooling speed is 1-20L / min, preferably 5-10L / min; the winding speed is 3-15m / min, preferably 5-10m / min.

[0021] Furthermore, in step (2), the pitch of twisting or twisting is 0.1-1.5 mm, preferably 0.3-1 mm, and the speed is 3-10 m / min, preferably 5-7 m / min; in step (1), the loading process includes melt blending extrusion, air cooling and winding, the melt blending temperature is 200-500°C, preferably 250-400°C, and the time is 10-30 min, preferably 15-25 min; the air cooling temperature is 5-30°C, preferably 10-20°C, and the air cooling speed is 1-20 L / min, preferably 5-10 L / min; the winding speed is 3-15 m / min, preferably 5-10 m / min.

[0022] An electroluminescent fiber prepared by the method as described above comprises, from inside to outside, a conductive fiber, a luminescent active layer, an external electrode and a transparent encapsulation layer, thereby forming an electrode-luminescent layer-electrode structure, i.e., a sandwich structure.

[0023] Compared with the prior art, the present invention has the following advantages:

[0024] (1) The electroluminescent fiber of the present invention is mainly composed of a conductive substrate, an active layer, an external electrode and a packaging layer. By adjusting the concentration, viscosity, ratio and coating process parameters of the molten material, an electroluminescent fiber with considerable brightness, long service life and controllable diameter is finally obtained;

[0025] (2) The process of the present invention combines the melt extrusion method with the solution coating method, and realizes the continuous preparation of electroluminescent fibers through equipment assembly and modification. Moreover, the technology is simple, efficient, mild in conditions, low in cost, green, economical and environmentally friendly, and suitable for industrial production;

[0026] (3) The luminescent fibers prepared by the present invention are of various colors, soft and weavable, and have broad application prospects in the field of functional clothing. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a schematic diagram of the structure of the luminous fiber of the present invention;

[0028] Figure 2 Schematic diagram of luminous fabric formed by weaving luminous fibers with ordinary yarns. DETAILED DESCRIPTION

[0029] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0030] An electroluminescent fiber, which comprises, from the inside to the outside, a conductive fiber, a luminescent active layer, an external electrode and a transparent encapsulation layer, wherein the thickness of the electroluminescent active layer is 20-150 μm, preferably 40-100 μm, and the thickness of the coated transparent insulating polymer is 10-80 μm, preferably 20-50 μm. Thus, an electrode-luminescent layer-electrode structure, i.e., a sandwich structure, is formed. The preparation method comprises the following steps:

[0031] (1) Loading the luminescent active layer: physically blending the thermoplastic elastomer polymer and the electroluminescent active material in a melt coating device, then melt coating the mixture on a conductive fiber substrate, and then cooling and solidifying the mixture online to obtain a conductive fiber coated with the electroluminescent active layer; the conductive fiber comprises one or more of a metal conductive fiber, a metal-coated chemical fiber, an ion gel fiber, and a conductive polymer composite fiber; the diameter of the conductive fiber is 50-300 μm, preferably 100-200 μm; the conductivity of the conductive fiber is 10 -4 -10 4 S / cm, preferably 10 -3 -10S / cm. The thermoplastic elastomer polymer is a solid resin, including fluororesin, cyanoresin, polystyrene, ABS, polytetrafluoroethylene, polyarylate, polyurethane resin or polyamide, with a weight average molecular weight (Mw) of 50,000-150,000; the thermoplastic elastomer polymer accounts for 20-80wt% in the electroluminescent active layer, preferably 30-50wt%. The electroluminescent active material is an inorganic electroluminescent material, including CaS, SrS, ZnS, CaGa2S4, SrGa2S4, SiO2:Ge, SiO2:Er, GaN or Zn2SiO4; the particle size of the electroluminescent active material is 10-50μm, preferably 20-40μm, and the proportion of the electroluminescent active layer is 20-80wt%, preferably 30-50wt%. The loading process includes melt blending extrusion, air cooling and winding, the melt blending temperature is 200-500°C, preferably 250-400°C, the time is 10-30min, preferably 15-25min; the air cooling temperature is 5-30°C, preferably 10-20°C, the air cooling speed is 1-20L / min, preferably 5-10L / min; the winding speed is 3-15m / min, preferably 5-10m / min.

[0032] (2) Loading fiber external electrode: The external electrode is loaded on the conductive fiber coated with the electroluminescent active layer in a twisted or twisted manner to obtain the electroluminescent fiber; the external electrode is a metal wire, including copper wire, steel wire, titanium wire or tungsten wire; the diameter of the metal wire is 10-100 μm, preferably 30-70 μm, and the conductivity is 10 -4 -10 4 S / cm, preferably 10 -3 -10S / cm. The twisting or twisting pitch is 0.1-1.5mm, preferably 0.3-1mm, and the speed is 3-10m / min, preferably 5-7m / min;

[0033] (3) Insulation packaging: melt-coat a transparent insulating polymer on the outside of the electroluminescent fiber to obtain an electroluminescent fiber. The transparent insulating polymer is a solid transparent resin selected from SBS, epoxy resin, acrylate resin, polyurethane resin, polytetrafluoroethylene resin or silicone resin, and the weight average molecular weight of the solid transparent resin is 20,000-100,000. The coating process steps include melt extrusion, air cooling and winding. The melting temperature is 50-180°C, preferably 80-140°C, and the time is 10-30min, preferably 15-25min; the air cooling temperature is 5-30°C, preferably 10-20°C, and the air cooling speed is 1-20L / min, preferably 5-10L / min; the winding speed is 3-15m / min, preferably 5-10m / min.

[0034] On the basis of being in accordance with the common sense in the art, the above-mentioned advantageous conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.

[0035] The reagents and raw materials used in the present invention are all commercially available. Room temperature refers to an ambient temperature of 10°C-30°C.

[0036] The various devices in the following embodiments are all commercially available devices. Figure 1 shown.

[0037] Example 1

[0038] An electroluminescent fiber and a melt-coating preparation method thereof, comprising the following steps:

[0039] Step 1: Start the melt blending device, add 50 g of zinc sulfide powder (diameter 20 μm) and 50 g of fluororesin into the device at room temperature 25°C, heat and blend at 300°C for 15 minutes to obtain a uniformly dispersed slurry.

[0040] The second step: turn on the winding and air cooling device, and evenly coat the slurry on the surface of the copper wire fiber (diameter 120μm) at a speed of 10m / min, then cool it online at an air cooling temperature of 20℃ and an air cooling speed of 5L / min. Finally, collect and wind it on the bobbin. The thickness of the active layer is controlled at about 50μm.

[0041] Step 3: Turn on the twisting device and twist the copper wire fiber (100 μm in diameter) on the fiber in the second step at a pitch of 0.4 mm and a twisting speed of 3 m / min. Finally, collect and wind it on a bobbin to obtain a twisted electroluminescent fiber.

[0042] Step 4: Turn on the packaging device, heat and melt the ABS at 150°C at room temperature of 25°C, and then evenly coat it on the fiber surface obtained in the third step at a speed of 5m / min, and then cool it online at an air-cooling temperature of 20°C and an air-cooling speed of 5L / min. Finally, collect and wind it on the bobbin, and the thickness of the packaging layer is controlled at about 15μm.

[0043] The prepared luminescent fiber reached 180cd / m after applying a 2000Hz, 100V sinusoidal AC voltage. 2 The luminous intensity is very high and it can still work normally and stably after being washed and bent.

[0044] Example 2

[0045] An electroluminescent fiber and a melt-coating preparation method thereof, comprising the following steps:

[0046] Step 1: Start the melt blending extrusion device, add 50g of CaS luminescent powder (diameter 30μm) and 80g of cyano resin into the device at room temperature 25°C, heat and blend at 400°C for 20min to obtain a uniformly dispersed slurry.

[0047] The second step: turn on the winding and air cooling device, and evenly coat the slurry on the surface of the copper wire fiber (diameter 150μm) at a speed of 15m / min, then cool it online at an air cooling temperature of 15°C and an air cooling speed of 8L / min. Finally, collect and wind it on the bobbin. The thickness of the active layer is controlled at about 40μm.

[0048] Step 3: Turn on the twisting device, and load the conductive fiber onto the fiber in the second step with a copper wire fiber (diameter 50 μm) at a twisting speed of 5 m / min with a pitch of 1.5 mm. Finally, collect and wind it on a bobbin to obtain the electroluminescent fiber.

[0049] Step 4: Turn on the packaging device, heat and melt the SBS at 180°C at room temperature of 25°C, and then evenly coat it on the fiber surface obtained in the third step at a speed of 8m / min, and then cool it online at an air-cooling temperature of 15°C and an air-cooling speed of 8L / min. Finally, collect and wind it on a bobbin, and the thickness of the packaging layer is controlled at about 10μm.

[0050] The prepared luminescent fiber can reach 100cd / m after applying a 2000Hz, 80V sinusoidal AC voltage. 2 The luminous intensity is very high and it can still work normally and stably after being washed and bent.

[0051] Example 3

[0052] An electroluminescent fiber and a melt-coating preparation method thereof, comprising the following steps:

[0053] Step 1: Turn on the melt blending device, add 50 g of GaN powder (diameter 20 μm) and 100 g of polystyrene into the device at room temperature 25°C, heat and blend at 350°C for 25 minutes to obtain a uniformly dispersed slurry.

[0054] The second step: turn on the winding and air cooling device, and evenly coat the slurry on the surface of the copper wire fiber (diameter 190μm) at a speed of 8m / min, then cool it online at an air cooling temperature of 18°C ​​and an air cooling speed of 7L / min. Finally, collect and wind it on the bobbin. The thickness of the active layer is controlled at about 30μm.

[0055] Step 3: Turn on the twisting device and twist the copper wire fiber (80 μm in diameter) on the fiber in the second step at a pitch of 2 mm and a twisting speed of 8 m / min. Finally, collect and wind it on a bobbin to obtain a twisted electroluminescent fiber.

[0056] Step 4: Turn on the packaging device, heat and melt the polyurethane at 150°C at room temperature of 25°C, and then evenly coat it on the fiber surface obtained in the third step at a speed of 10m / min, and then cool it online at an air-cooling temperature of 18°C ​​and an air-cooling speed of 10L / min. Finally, collect and wind it on a bobbin, and the thickness of the packaging layer is controlled at about 15μm.

[0057] The prepared luminescent fiber can reach 200cd / m after applying a 2000Hz, 150V sinusoidal AC voltage. 2 The luminous intensity is high and it can still work normally and stably after being washed, bent, etc.

[0058] Example 4

[0059] An electroluminescent fiber and a melt-coating preparation method thereof, comprising the following steps:

[0060] Step 1: Turn on the melt blending extrusion device, add 80g SiO2:Ge luminescent powder (diameter 10μm) and 200g polytetrafluoroethylene into the device at room temperature 25°C, heat and blend at 380°C for 30min to obtain a uniformly dispersed slurry.

[0061] The second step: turn on the winding and air cooling device, and evenly coat the slurry on the surface of the copper wire fiber (diameter 100μm) at a speed of 20m / min, then cool it online at an air cooling temperature of 20℃ and an air cooling speed of 10L / min. Finally, collect and wind it on the bobbin. The thickness of the active layer is controlled at about 25μm.

[0062] Step 3: Turn on the twisting device, load the conductive fiber onto the fiber in the second step with a copper wire fiber (diameter 50 μm) at a twisting speed of 8 m / min with a pitch of 1 mm, and finally collect and wind it on a bobbin to obtain the electroluminescent fiber.

[0063] Step 4: Turn on the packaging device, heat and melt the silicone resin at 160°C at room temperature of 25°C, and then evenly coat it on the fiber surface obtained in the third step at a speed of 6m / min, and then cool it online at an air-cooling temperature of 20°C and an air-cooling speed of 6L / min. Finally, collect and wind it on a bobbin, and the thickness of the packaging layer is controlled at about 20μm.

[0064] The prepared luminescent fiber can reach a maximum of 90cd / m after applying a 2000Hz, 60V sinusoidal AC voltage. 2 The luminous intensity is high and it can still work normally and stably after being washed, bent, etc.

[0065] In summary, the luminescent fiber prepared by the present invention can reach a maximum of 200 cd / m2 under the application of a 2kHz, 60-150V sinusoidal AC voltage. 2 The luminous intensity is high, and it can still work stably after washing and bending. The luminous fiber has good flexibility and can be further woven into luminous fabrics, which has great application prospects in the field of smart wearable electronic devices.

[0066] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing an electroluminescent fiber by melt coating, characterized in that: The method comprises the following steps: (1) Loading the luminescent active layer: physically blending the thermoplastic elastomer polymer and the electroluminescent active material in a melt coating device, then melt coating the polymer on the conductive fiber substrate, and then cooling and solidifying the conductive fiber online to obtain the conductive fiber coated with the electroluminescent active layer; (2) Loading the fiber external electrode: Loading the external electrode on the conductive fiber coated with the electroluminescent active layer in a twisted or twisted manner to obtain the electroluminescent fiber; (3) Insulation packaging: melt-coating a transparent insulating polymer on the outside of the electroluminescent fiber to obtain the electroluminescent fiber; The conductive fibers include one or more of metal conductive fibers, metal-particle-plated chemical fibers, ion gel fibers, and conductive polymer composite fibers; The diameter of the conductive fiber is 50-300 μm; the conductivity of the conductive fiber is 10 -4 -10 4 S / cm; The thermoplastic elastomer polymer is a solid resin, including fluororesin, cyanoresin, polystyrene, ABS, polytetrafluoroethylene, polyarylate, polyurethane resin or polyamide; the thermoplastic elastomer polymer accounts for 20-80wt% in the electroluminescent active layer; The electroluminescent active material is an inorganic electroluminescent material, including CaS, SrS, ZnS, CaGa2S4, SrGa2S4, SiO2:Ge, SiO2:Er, GaN or Zn2SiO4; The particle size of the electroluminescent active material is 10-50 μm, and the proportion of the electroluminescent active material in the electroluminescent active layer is 20-80 wt%; The coating process of step (3) includes melt extrusion, air cooling and winding, wherein the melting temperature is 50-180° C., the air cooling temperature is 5-30° C., the air cooling speed is 1-20 L / min; and the winding speed is 3-15 m / min; The twisting or twisting pitch in step (2) is 0.1-1.5 mm, and the speed is 3-10 m / min; the loading process in step (1) includes melt blending extrusion, air cooling and winding, the melt blending temperature is 200-500° C., and the time is 10-30 min; the air cooling temperature is 5-30° C., the air cooling speed is 1-20 L / min; the winding speed is 3-15 m / min; The outer electrode is a metal wire, including copper wire, steel wire, titanium wire or tungsten wire; the diameter of the metal wire is 10-100 μm, and the conductivity is 10 -4 -10 4 S / cm; The transparent insulating polymer is a solid transparent resin selected from SBS, epoxy resin, acrylate resin, polyurethane resin, polytetrafluoroethylene resin or silicone resin, and the weight average molecular weight of the solid transparent resin is 20,000-100,000; The thickness of the electroluminescent active layer is 20-150 μm, and the thickness of the coated transparent insulating polymer is 10-80 μm.

2. An electroluminescent fiber prepared by the method of claim 1, the luminescent fiber comprising from inside to outside: Conductive fibers, luminescent active layer, external electrodes and transparent encapsulation layer.

Citation Information

Patent Citations

  • Superfine electroluminescent fiber and preparation method and application thereof

    CN113981674A

  • Manufacturing a luminent composite fibre of goodstrength and abrasion-resistence

    KR1020000063795A

Cited By

  • High-performance luminescent fiber driven by safe voltage and preparation method of high-performance luminescent fiber

    CN120465167A

  • A high performance light emitting fiber driven by a safe voltage and a preparation method thereof

    CN120465167B

  • Solution-coated twist-set outer electrode light emitting fiber and method of making same

    CN122669530A