Electromagnetic wave shielding film

By adjusting the Martens hardness ratio between the conductive adhesive layer and the insulating layer, the problem of the protrusions of the grounding member failing to fully penetrate the insulating layer is solved, and superior conductivity and stable connection between the grounding member and the shielding layer are achieved.

CN115004874BActive Publication Date: 2024-10-11TATSUTA ELECTRICWIRE & CABLE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180012283.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-02-25
Filing Date
2021-02-25
Publication Date
2024-10-11
Estimated Expiration
2041-02-25

AI Technical Summary

Technical Problem

In existing electromagnetic wave shielding films, the protrusions of the grounding member fail to fully penetrate the insulating layer, causing the conductive adhesive layer to deform and the conductive filler to detach, causing problems such as increased resistance and damaged connections.

Method used

By adjusting the Martens hardness ratio between the conductive adhesive layer and the insulating layer to be above 0.3, it is ensured that the protrusions of the grounding member can stably penetrate the insulating layer and contact the shielding layer, preventing deformation of the conductive adhesive layer.

Benefits of technology

It achieves superior conductivity and stable connection between the ground component and the shielding layer, avoiding the problems of rising resistance value and damaged connection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115004874B_ABST
    Figure CN115004874B_ABST
Patent Text Reader

Abstract

The present invention provides an electromagnetic wave shielding film that can easily exert excellent conductivity between a grounding member and a shielding layer when a grounding member is arranged on the electromagnetic wave shielding film. In the electromagnetic wave shielding film 1, a conductive adhesive layer 11, a shielding layer 12 and an insulating layer 13 are sequentially laminated, and the ratio of the Martens hardness of the conductive adhesive layer 11 based on ISO14577-1 to the Martens hardness of the insulating layer 13 based on ISO14577-1 [conductive adhesive layer / insulating layer] is 0.3 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an electromagnetic wave shielding film. More specifically, the present invention relates to an electromagnetic wave shielding film used in a printed wiring board. Background Art

[0002] Printed circuit boards are used to integrate circuits into the mechanisms of electronic devices such as mobile phones, cameras, and notebook personal computers. They are also used to connect movable parts such as print heads and control parts. Electromagnetic wave shielding measures are essential for these electronic devices, and shielded printed circuit boards with electromagnetic wave shielding measures are also used in the printed circuit boards used in the devices.

[0003] A general shielded printed circuit board is usually composed of the following: a base film, on which a printed circuit and an insulating film are arranged in sequence; an electromagnetic wave shielding film (hereinafter sometimes simply referred to as a "shielding film"), which is composed of an adhesive layer, a shielding layer stacked on the above-mentioned adhesive layer, and an insulating layer stacked on the above-mentioned shielding layer, and the electromagnetic wave shielding film is stacked on the above-mentioned base film in a manner that the above-mentioned adhesive layer is in contact with the above-mentioned base film.

[0004] The printed circuit includes a grounding circuit, which is electrically connected to the housing of the electronic device for grounding. In order to electrically connect the grounding circuit to the housing of the electronic device, it is necessary to open a hole in part of the insulating film and the shielding film in advance. This is the main reason that hinders the degree of freedom in designing printed circuits.

[0005] Patent document 1 discloses a shielding membrane, which forms an insulating layer (covering film) on one side of a separation membrane by coating, and a shielding layer composed of a metal film layer and an adhesive layer is arranged on the surface of the above-mentioned insulating layer. In addition, the shielding membrane contains a grounding component, one end side of the grounding component contains a protrusion and a conductive filler (connecting part) which is pressed against the above-mentioned insulating layer and penetrates the insulating layer to be connected to the above-mentioned shielding layer, and the other end side is exposed so that it can be connected to the grounding part nearby.

[0006] When manufacturing the shielding film described in Patent Document 1, the grounding member is pressed against the insulating layer so that the protrusion of the grounding member and the conductive filler penetrate the insulating layer. As a result, the grounding member is electrically connected to the shielding layer, so the grounding member can be arranged at any position of the shielding film. When such a grounding member is used to manufacture a shielded printed circuit board, the grounding circuit can be electrically connected to the housing of the electronic device at any position.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent document 1: Japanese Patent Application Laid-Open No. 2004-95566. Summary of the invention

[0010] Technical problem to be solved by the invention

[0011] However, sometimes the protrusion of the grounding member does not fully penetrate the insulating layer and fails to fully contact the shielding layer of the shielding film. In addition, even if the protrusion of the grounding member and the conductive filler (hereinafter referred to as "protrusion") fully penetrate the insulating layer, sometimes the protrusion of the grounding member and the shielding layer are squeezed into the conductive adhesive layer located on the back side of the shielding layer and deformed, so that the conductive filler in the conductive adhesive layer is squeezed by the protrusion, and the conductive filler moves and leaves the circuit. These situations will cause the resistance value to increase, and the connection between the grounding member, the shielding film and the circuit of the printed circuit board will be damaged.

[0012] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide an electromagnetic wave shielding film that can easily exhibit excellent conductivity between a grounding member and a shielding layer when a grounding member is arranged on the electromagnetic wave shielding film.

[0013] Technical means to solve technical problems

[0014] The inventors of the present application have made careful studies to achieve the above-mentioned purpose and have found that by determining the relationship between the Martens hardness, which is an index indicating the hardness of a micro-region, between the insulating layer and the conductive adhesive layer in the shielding film, it is easy to achieve excellent conductivity between the grounding member and the shielding layer when the grounding member is arranged on the electromagnetic wave shielding film. The present invention is completed based on the above-mentioned findings.

[0015] That is, the present invention provides an electromagnetic wave shielding film, in which a conductive adhesive layer, a shielding layer and an insulating layer are stacked in sequence, and the ratio of the Martens hardness of the conductive adhesive layer based on ISO14577-1 to the Martens hardness of the insulating layer based on ISO14577-1 [conductive adhesive layer / insulating layer] is greater than 0.3.

[0016] In the above-mentioned electromagnetic wave shielding film, the above-mentioned Martens hardness ratio is 0.3 or more, which means that the Martens hardness of the conductive adhesive layer is larger than that of the insulating layer. When the protrusion of the grounding member is pressed to penetrate the insulating layer, pressure is locally applied from the protrusion to the laminated insulating layer, the shielding layer and the conductive adhesive layer. At this time, since the Martens hardness of the insulating layer is relatively low, the above-mentioned pressure is locally applied to the insulating layer, and the protrusion of the grounding member can easily penetrate the insulating layer. Then, when the protrusion of the grounding member penetrates the insulating layer and contacts the shielding layer, since the Martens hardness of the conductive adhesive layer located on the back side of the shielding layer is relatively high, it is difficult to deform the conductive adhesive layer by the pressure locally applied through the shielding layer, thereby making it difficult to damage the contact between the conductive particles in the conductive adhesive layer and the shielding layer, or the conductive particles and the printed circuit board. Therefore, in the electromagnetic shielding film having the above structure, the protrusion of the grounding member penetrating the insulating layer can stably contact the shielding layer, and when the grounding member is arranged on the electromagnetic shielding film, excellent conductivity can be easily exerted between the grounding member and the shielding layer.

[0017] The Martens hardness of the insulating layer based on ISO14577-1 is preferably 3 to 150 N / mm 2 In the electromagnetic wave shielding film having the above structure, the local hardness of the insulating layer is moderate, so the protrusion of the grounding member can easily penetrate the insulating layer.

[0018] The Martens hardness of the conductive adhesive layer based on ISO14577-1 is preferably 20 to 200 N / mm 2 In the electromagnetic wave shielding film containing the above structure, the local hardness of the conductive adhesive layer is moderate, so when the protrusion of the grounding member is squeezed into the shielding layer, the conductive adhesive layer is difficult to deform, or even if it is deformed, it is easy to restore, and the contact between the conductive particles in the conductive adhesive layer and the shielding layer, or the conductive particles and the printed circuit board is difficult to be damaged.

[0019] Effects of the Invention

[0020] The electromagnetic wave shielding film of the present invention can easily exhibit excellent conductivity between the grounding member and the shielding layer when the grounding member is disposed on the electromagnetic wave shielding film. BRIEF DESCRIPTION OF THE DRAWINGS

[0021]

Figure 1

[0022]

Figure 2

[0023] [Electromagnetic wave shielding film]

[0024] The electromagnetic wave shielding film of the present invention includes a conductive adhesive layer, a shielding layer which is a layer for shielding electromagnetic waves, and an insulating layer.

[0025] An embodiment of the electromagnetic wave shielding film of the present invention will be described below. Figure 1 It is a schematic cross-sectional view of one embodiment of the electromagnetic wave shielding film of the present invention.

[0026] Figure 1 The shielding film 1 shown contains a conductive adhesive layer 11, a shielding layer 12 formed on the surface of the conductive adhesive layer 11, and an insulating layer 13 formed on the surface of the shielding layer 12. That is, the conductive adhesive layer 11, the shielding layer 12, and the insulating layer 13 are sequentially stacked in the shielding film 1. In addition, it can be designed that the conductive adhesive layer 11 and the shielding layer 12, and the shielding layer 12 and the insulating layer 13 are not stacked in a contacting manner. That is, it can be designed that at least one arbitrary layer is set between the conductive adhesive layer and the shielding layer, or between the shielding layer and the insulating layer.

[0027] The ratio of the Martens hardness of the conductive adhesive layer to the Martens hardness of the insulating layer [conductive adhesive layer / insulating layer] is 0.3 or more, preferably 0.5 or more, more preferably 0.6 or more, and even more preferably 1.0 or more. The Martens hardness is a value measured in accordance with ISO14577-1.

[0028] In the electromagnetic wave shielding film of the present invention, the above-mentioned Martens hardness ratio is 0.3 or more, which means that the Martens hardness of the conductive adhesive layer is larger than that of the insulating layer. When the protrusion of the grounding member is pressed to penetrate the insulating layer, pressure is locally applied from the protrusion to the laminated insulating layer, the shielding layer and the conductive adhesive layer. At this time, since the Martens hardness of the insulating layer is relatively low, the above-mentioned pressure is locally applied to the insulating layer, and the protrusion of the grounding member can easily penetrate the insulating layer. Then, when the protrusion of the grounding member penetrates the insulating layer and contacts the shielding layer, since the Martens hardness of the conductive adhesive layer located on the back side of the shielding layer is relatively high, it is difficult to deform the conductive adhesive layer by the pressure locally applied through the shielding layer, thereby making it difficult to damage the contact between the conductive particles in the conductive adhesive layer and the shielding layer, or the conductive particles and the printed circuit board. Therefore, in the electromagnetic shielding film having the above structure, the protrusion of the grounding member penetrating the insulating layer can stably contact the shielding layer, and when the grounding member is arranged on the electromagnetic shielding film, excellent conductivity can be easily exerted between the grounding member and the shielding layer.

[0029] The Martens hardness ratio [conductive adhesive layer / insulating layer] is, for example, 50.0 or less, preferably 10.0 or less, more preferably 5.0 or less, further preferably 3.0 or less, and particularly preferably 2.0 or less.

[0030] (Conductive adhesive layer)

[0031] The conductive adhesive layer 11 has bonding properties and conductivity for bonding the electromagnetic wave shielding film of the present invention to a printed circuit board. Preferably, the conductive adhesive layer is formed adjacent to the electromagnetic wave shielding layer. The conductive adhesive layer can be designed to be either a single layer or a multilayer.

[0032] Preferably, the conductive adhesive layer contains a binder component and conductive particles.

[0033] Examples of the binder component include thermoplastic resins, thermosetting resins, active energy ray-curable compounds, etc. The binder component may be used alone or in combination of two or more.

[0034] Examples of the thermoplastic resin include polystyrene resins, vinyl acetate resins, polyester resins, polyolefin resins (such as polyethylene resins, polypropylene resin compositions, etc.), polyimide resins, acrylic resins, etc. The thermoplastic resins may be used alone or in combination of two or more.

[0035] The thermosetting resin may include a thermosetting resin (thermosetting resin) and a resin obtained by curing the thermosetting resin. Examples of the thermosetting resin include phenolic resins, epoxy resins, polyurethane resins, melamine resins, alkyd resins, and the like. The thermosetting resin may be used alone or in combination of two or more.

[0036] Examples of the epoxy resin include bisphenol epoxy resins, spirocycle epoxy resins, naphthalene epoxy resins, biphenyl epoxy resins, terpene epoxy resins, glycidyl ether epoxy resins, glycidyl amine epoxy resins, and novolac epoxy resins.

[0037] Examples of the bisphenol epoxy resins include bisphenol A epoxy resins, bisphenol F epoxy resins, bisphenol S epoxy resins, and tetrabromobisphenol A epoxy resins. Examples of the glycidyl ether epoxy resins include tris(glycidyloxyphenyl)methane and tetra(glycidyloxyphenyl)ethane. Examples of the glycidylamine epoxy resins include tetraglycidyldiaminodiphenylmethane. Examples of the (linear) novolac epoxy resins include cresol (linear) novolac epoxy resins, phenol (linear) novolac epoxy resins, α-naphthol (linear) novolac epoxy resins, and brominated phenol (linear) novolac epoxy resins.

[0038] The epoxy resin may be an epoxy resin containing a self-reactive modified portion in addition to an epoxy group (modified epoxy resin), such as an epoxy resin containing a (meth)acryloyl group (acrylic modified epoxy resin), etc. When the modified epoxy resin is used, the Martens hardness of the conductive adhesive layer can be easily set within a suitable range by cross-linking.

[0039] The active energy ray curable compound may include compounds that can be cured by irradiation with active energy rays (active energy ray curable compounds) and compounds obtained by curing the active energy ray curable compounds. The active energy ray curable compound is not particularly limited, and examples thereof include polymerizable compounds containing one or more (preferably two or more) free radical reactive groups (such as (meth) acryloyl groups) in the molecule. The active energy ray curable compound may be used alone or in combination of two or more.

[0040] Among them, thermosetting resin is preferred as the adhesive component. In this case, after the electromagnetic wave shielding film of the present invention is arranged on a printed wiring board for bonding with the printed wiring board, the adhesive component can be cured by pressurization and heating, thereby improving bonding with the printed wiring board.

[0041] When the binder component includes a thermosetting resin, a curing agent for promoting a thermosetting reaction may be included as a component constituting the binder component. The curing agent may be appropriately selected according to the type of the thermosetting resin. Only one type of curing agent may be used, or two or more types of curing agents may be used.

[0042] The content ratio of the binder component in the conductive adhesive layer is not particularly limited, and is preferably 5 to 60% by mass, more preferably 10 to 50% by mass, and further preferably 20 to 45% by mass relative to the total amount 100% by mass of the conductive adhesive layer. When the content ratio is 5% by mass or more, the close adhesion with the printed wiring board is more excellent. When the content ratio is 60% by mass or less, the conductive particles can be fully contained.

[0043] Examples of the conductive particles include metal particles, metal-coated resin particles, metal fibers, carbon-based fillers, carbon nanotubes, etc. The conductive particles may be used alone or in combination of two or more.

[0044] Examples of the metal constituting the coating of the metal particles and the metal-coated resin particles include gold, silver, copper, nickel, zinc, etc. The metals may be used alone or in combination of two or more.

[0045] Specifically, the metal particles include, for example, copper particles, silver particles, nickel particles, silver-coated copper particles, gold-coated copper particles, silver-coated nickel particles, gold-coated nickel particles, silver-coated alloy particles, etc. The silver-coated alloy particles include, for example, silver-coated copper alloy particles obtained by coating copper-containing alloy particles (for example, copper alloy particles composed of an alloy of copper, nickel and zinc), etc. The metal particles can be produced by electrolysis, atomization, reduction, etc.

[0046] Among them, silver particles, silver-coated copper particles, and silver-coated copper alloy particles are preferred as the above-mentioned metal particles. Silver-coated copper particles and silver-coated copper alloy particles are particularly preferred from the viewpoints of excellent conductivity, suppression of oxidation and coagulation of metal particles, and reduction of the cost of metal particles.

[0047] Examples of the conductive particles include spherical, flake (scale), dendritic, fibrous, and amorphous (polyhedral) shapes.

[0048] The median diameter (D50) of the conductive particles is preferably 1 to 50 μm, more preferably 3 to 40 μm. When the median diameter is 1 μm or more, the conductive particles have good dispersibility, thereby suppressing coagulation and being difficult to oxidize. When the average particle diameter is 50 μm or less, the conductivity is good. The median diameter can be measured by volume-based particle size distribution.

[0049] The conductive adhesive layer may have isotropic conductivity or anisotropic conductivity as required. In particular, the conductive adhesive layer preferably has anisotropic conductivity from the viewpoint of improving the transmission characteristics of high-frequency signals transmitted by the signal circuit of the printed wiring board.

[0050] The content ratio of the conductive particles in the conductive adhesive layer is not particularly limited, and is preferably 2 to 80% by mass, more preferably 5 to 60% by mass, and further preferably 10 to 40% by mass relative to the total amount 100% by mass of the conductive adhesive layer. When the content ratio is 2% by mass or more, the conductivity is better. When the content ratio is 80% by mass or less, the adhesive component can be fully contained, thereby making the close adhesion with the printed wiring board better.

[0051] The conductive adhesive layer preferably contains a filler (filler) other than the conductive particles. The Martens hardness of the conductive adhesive layer can be adjusted by mixing the filler. The filler may be used alone or in combination of two or more.

[0052] Inorganic fillers or organic fillers can be used as the fillers. From the viewpoint of increasing the Martens hardness of the conductive adhesive layer, inorganic fillers, organic fillers composed of crosslinkable resin particles, and organic phosphorus compounds are preferred. Examples of inorganic fillers include metal oxides such as silicon oxide, boron oxide, aluminum oxide, titanium oxide, and zirconium oxide; phosphorus compounds such as red phosphorus; metal carbides such as silicon carbide, boron carbide, and titanium carbide; metal nitrides such as aluminum nitride, boron nitride, and titanium nitride; metal hydroxides such as magnesium hydroxide and aluminum hydroxide; carbonates such as calcium carbonate and magnesium carbonate, and the like. Examples of crosslinked resin particles include polyolefins such as polyethylene, polypropylene, polystyrene, polyvinyl chloride, polyvinylidene chloride, polytetrafluoroethylene, polyisobutylene, and polybutadiene; acrylic resins such as polymethyl methacrylate and polymethacrylate; copolymer resins of acrylate and divinylbenzene, polyalkylene terephthalate, polysulfone, polycarbonate, polyamide, phenol formaldehyde resin, melamine formaldehyde resin, benzoguanidine formaldehyde resin, and urea formaldehyde resin. Examples of organic phosphorus compounds include phosphorus compounds such as phosphates and metal phosphinates. When the organic filler is a phosphorus compound such as a phosphate and a metal phosphinate, it also has the function of a flame retardant, so it can control the Martens hardness and also impart flame retardancy.

[0053] From the viewpoint of easily controlling the Martens hardness of the conductive adhesive layer, the median diameter (D50) of the filler is preferably 0.01 to 100 μm, more preferably 1 to 20 μm. The median diameter can be measured by volume-based particle size distribution.

[0054] The content ratio of the filler in the conductive adhesive layer is not particularly limited, and is preferably 1 to 70% by mass, more preferably 10 to 60% by mass, and further preferably 35 to 50% by mass relative to the total amount 100% by mass of the conductive adhesive layer. When the content ratio is within the above range, the conductivity and the close adhesion with the printed wiring board can be maintained, and the Martens hardness can be easily adjusted within an appropriate range.

[0055] The conductive adhesive layer may contain other ingredients in addition to the above-mentioned components within the scope of not impairing the technical effects of the present invention. The above-mentioned other ingredients may include well-known or even commonly used ingredients contained in adhesive layers. The above-mentioned other ingredients may include, for example, flame retardants, flame retardant aids, defoamers, viscosity modifiers, antioxidants, diluents, anti-settling agents, colorants, leveling agents, coupling agents, ultraviolet absorbers, tackifying resins, etc. that do not conform to the above-mentioned fillers. The above-mentioned other ingredients may be used alone or in combination of two or more.

[0056] The Martens hardness of the conductive adhesive layer is preferably 20 to 200 N / mm 2 , more preferably 30 to 180 N / mm 2, more preferably 50 to 170 N / mm 2 When the Martens hardness is within the above range, the local hardness of the conductive adhesive layer is moderate, so when the protrusion of the grounding member is squeezed into the shielding layer, the conductive adhesive layer is difficult to deform, or even if it is deformed, it is easy to restore, and the contact between the conductive adhesive layer and the shielding layer, or the conductive particles and the printed circuit board is difficult to be damaged. In addition, the Martens hardness is 200N / mm 2 When the hardness is less than 0.5, the adhesion to the printed wiring board is good. The Martens hardness of the conductive adhesive layer is a value measured in accordance with ISO14577-1 and is measured on the surface on the shielding layer side.

[0057] The thickness of the conductive adhesive layer is preferably 3 to 20 μm, more preferably 5 to 15 μm. When the thickness is 3 μm or more, the shielding film can provide a more adequate shielding performance for shielding high-frequency electromagnetic waves generated internally. When the thickness is 20 μm or less, the shielding film has excellent flexibility.

[0058] (Shielding layer)

[0059] The shielding layer 12 is formed on the surface of the conductive adhesive layer 11. A well-known or even commonly used shielding layer having electromagnetic wave shielding properties can be used as the shielding layer. Among them, it is preferred that the shielding layer includes a metal layer. The shielding layer may be a single layer or a multilayer.

[0060] Examples of the metal constituting the metal layer include gold, silver, copper, aluminum, nickel, tin, palladium, chromium, titanium, zinc, or alloys of the metals above. A metal plate or metal foil is preferably used as the metal layer. That is, a copper plate (copper foil) or a silver plate (silver foil) is preferably used as the metal layer.

[0061] The thickness of the shielding layer is preferably 0.01 to 10 μm. When the thickness is 0.01 μm or more, more sufficient shielding performance can be obtained. When the thickness is 10 μm or less, flexibility is better.

[0062] (Insulation layer)

[0063] The insulating layer 13 is formed on the surface of the shielding layer 12. The insulating layer 13 has insulating properties and has a function of protecting the conductive adhesive layer 11 and the shielding layer 12 in the electromagnetic wave shielding film 1 of the present invention. The insulating layer may be a single layer or a multilayer.

[0064] The insulating layer preferably contains a binder component. Examples of the binder component include thermoplastic resins, thermosetting resins, and active energy ray-curable compounds. Examples of the thermoplastic resins, thermosetting resins, and active energy ray-curable compounds include the examples of binder components that the conductive adhesive layer may contain as mentioned above. Only one type of binder component may be used, or two or more types may be used. Among them, it is preferred that the binder component includes a thermosetting resin and an active energy ray-curable compound.

[0065] The insulating layer may contain other components other than the binder component within the scope that the technical effect of the present invention is not impaired. The other components may include, for example, flame retardants, flame retardant aids, defoamers, viscosity modifiers, antioxidants, diluents, anti-settling agents, fillers, colorants, levelers, coupling agents, ultraviolet absorbers, tackifying resins, etc. The other components may be used alone or in combination of two or more.

[0066] The Martens hardness of the insulating layer is preferably 3 to 200 N / mm 2 , more preferably 30 to 150 N / mm 2 , more preferably 50 to 140 N / mm 2 , particularly preferably 70 to 130 N / mm 2 When the Martens hardness is within the above range, the local hardness of the insulating layer is moderate, so the protrusion of the grounding member can easily penetrate the insulating layer. The Martens hardness is 3N / mm 2 When the insulating layer surface is moderately hard, the protrusion of the grounding member can easily penetrate the protective layer. The above Martens hardness is 200N / mm 2 When the surface of the insulating layer is moderately soft, the protrusion of the grounding member can easily penetrate the insulating layer. The Martens hardness of the insulating layer can be adjusted by designing, for example, the degree of curing of the thermosetting component constituting the insulating layer, the type of curing agent, or the type of adhesive component. The Martens hardness of the insulating layer is a value measured based on ISO14577-1 and is measured on the surface of the insulating layer opposite to the shielding layer side.

[0067] The thickness of the insulating layer is preferably 1 to 15 μm, more preferably 3 to 10 μm. When the thickness is 1 μm or more, the shielding layer and the conductive adhesive layer can be more adequately protected. When the thickness is 15 μm or less, the flexibility is excellent and it is more economically advantageous.

[0068] The electromagnetic wave shielding film of the present invention may contain other layers in addition to the above layers. For example, the other layers may include an adhesion promoter coating provided between the insulating layer and the shielding layer. When the adhesion promoter coating is included, the insulating layer and the shielding layer have better adhesion.

[0069] Materials for forming the above-mentioned adhesion coating layer include polyurethane resins, acrylic resins, core-shell composite resins with polyurethane resin as shell and acrylic resin as core, epoxy resins, polyimide resins, polyamide resins, melamine resins, phenol resins, urea-formaldehyde resins, blocked isocyanates obtained by reacting blocking agents such as phenol with polyisocyanates, polyvinyl alcohol, polyvinyl pyrrolidone, etc. The above-mentioned materials may be used alone or in combination of two or more.

[0070] The electromagnetic wave shielding film of the present invention may have a separator (peeling film) on the insulating layer side and / or the conductive adhesive layer side. The separator is laminated in a manner that allows it to be peeled off from the electromagnetic wave shielding film of the present invention. The separator is an element for covering and protecting the above-mentioned insulating layer and the above-mentioned conductive adhesive layer, and is peeled off when using the electromagnetic wave shielding film of the present invention.

[0071] Examples of the separator include polyethylene terephthalate (PET) films, polyethylene films, polypropylene films, plastic films coated with a release agent such as a fluorine-based release agent or a long-chain alkyl acrylate-based release agent, and paper.

[0072] The thickness of the separator is preferably 10 to 200 μm, more preferably 15 to 150 μm. When the thickness is 10 μm or more, the protective performance is more excellent. When the thickness is 200 μm or less, the separator is easy to peel off during use.

[0073] The electromagnetic wave shielding film of the present invention is preferably used for a printed wiring board, and is particularly preferably used for a flexible printed wiring board (FPC). The electromagnetic wave shielding film of the present invention can be preferably used as an electromagnetic wave shielding film for a flexible printed wiring board.

[0074] [Shielded printed circuit board]

[0075] Figure 2 An embodiment of a shielded printed wiring board including the shielding film 1 which is the electromagnetic wave shielding film of the present invention is shown. Figure 2 The shielded printed wiring board X shown includes a printed wiring board 2, a shielding film 1, and a grounding member 3. Furthermore, an electronic component 4 is connected to a mounting portion provided on the lower side of the printed wiring board 2. In addition, the shielding film 1 is provided on the printed wiring board 2 and is arranged in a region facing the mounting portion to which the electronic component 4 is connected. Thus, noise such as electromagnetic waves from the outside relative to the mounting portion of the electronic component 4 is shielded by the shielding film 1.

[0076] The grounding member 3 is provided on the shielding film 1 and is arranged to face a mounting portion to which the electronic component 4 is connected. Figure 2In the present invention, the grounding member 3 is composed of a conductive substrate 31 and a conductive adhesive 32, and is adhered to the insulating layer 13 of the shielding film 1 by the adhesive 3a of the conductive adhesive 32. The conductive particles 3b contained in the conductive adhesive 32 protrude from the adhesive 3a contained in the conductive adhesive 32. Then, the conductive substrate 31 joined via the conductive adhesive 32 is in contact with the conductive particles 3b. On the other hand, the conductive particles 3b protruding from the lower side of the conductive adhesive 32 as protrusions included in the grounding member 3 penetrate the insulating layer 13 of the shielding film 1 and contact the shielding layer 12 thereunder. As a result, the conductive substrate 31 and the shielding layer 12 of the shielding film 1 become conductive via the conductive particles 3b of the conductive adhesive 32, so that the conductive grounding member 3 and the shielding layer 12 can have the same potential. Therefore, the conductive grounding member 3 can have a shielding effect. Therefore, the grounding member 3 is in contact with the shielding layer 12 so that the grounding member 3 can have at least the following two functions: strengthening the mounting position of the electronic component 4; shielding noise such as electromagnetic waves from the outside relative to the mounting position of the electronic component 4.

[0077] In addition, the state in which the protrusion of the grounding member 3 penetrates the insulating layer 13 of the shielding film 1 and contacts the shielding layer 12 is not limited to Figure 2 The form shown is a form in which the conductive particles 3b of the conductive adhesive 32 function as protrusions. For example, the following forms can be cited: a grounding member is formed by bending a conductive substrate 31 such as a metal foil, and then the grounding member is stacked on the insulating layer 13 without the conductive adhesive 32, and the mountain-shaped bent portion of the conductive substrate 31 functions as a protrusion of the grounding portion, penetrating the insulating layer 13 and contacting the shielding layer 12. The following forms can also be cited as other forms: the grounding member is formed by a conductive layer such as a metal foil, and one side of the conductive layer is provided with a conductive protrusion of a metal or the like integrally or non-integrally, and it is stacked on the insulating layer 13 without the conductive adhesive 32, and the conductive protrusion functions as a protrusion of the grounding portion, penetrating the insulating layer 13 and contacting the shielding layer 12. The shape of the conductive protrusion can be a columnar shape such as a cylinder or a prism, or a cone shape such as a cone or a pyramid.

[0078] The printed wiring board 2 includes a base member 21, a circuit pattern 23 partially provided on the surface of the base member 21, an insulating protective layer (cover film) 24 covering the circuit pattern 23 and insulating and protecting it, and an adhesive layer 22 for covering the circuit pattern 23 and bonding the circuit pattern 23 and the base member 21 to the insulating protective layer 24. The circuit pattern 23 includes a plurality of signal circuits 23a and a ground circuit 23b. In order to ensure conduction with the conductive adhesive layer 11 of the shielding film 1, a through hole 25 is formed in the adhesive layer 22 and the insulating protective layer 24 on the ground circuit 23b.

[0079] After the grounding member 3 is placed on the shielding film 1, the grounding member 3 can be formed by heat pressing. Figure 2 The shielded printed circuit board X shown in the figure. The above-mentioned hot pressing is generally carried out under the conditions of a temperature of about 150 to 190°C, a pressure of about 1 to 3 MPa, and a time of about 1 to 60 minutes. In addition, in order to promote curing, post-curing is sometimes carried out at 150 to 190°C for 30 to 90 minutes after hot pressing. Example

[0080] The present invention will be described in further detail below based on examples, but the present invention is not limited to these examples. In addition, the blending amounts described in the tables are relative blending amounts of each component, and are expressed in "parts by mass" unless otherwise specified.

[0081] Example 1

[0082] (1) Formation of insulating layer

[0083] On the release-treated surface of the substrate, i.e., the separation membrane, a resin composition composed of an acrylic-modified epoxy resin and an acrylic resin is prepared in the ratio shown in Table 1, and the resin composition is applied so that the thickness of the formed insulating layer is 3 μm, and heated at 100° C. for 120 seconds to form an insulating layer.

[0084] (2) Formation of shielding layer

[0085] A silver layer having a thickness of 0.1 μm was formed on the insulating layer obtained by the above steps by an evaporation method.

[0086] (3) Formation of conductive adhesive layer and electromagnetic wave shielding film

[0087] Silver-coated copper powder is added to a composition containing a phosphorus flame retardant and an acrylic modified epoxy resin so that the content ratio in the conductive adhesive layer is 20 mass %, thereby preparing an adhesive composition. Then, the above-mentioned adhesive composition is applied to the shielding layer obtained by the above steps so that the thickness is 15 μm to form a coating film. The coating method adopts a lip coating method. Then, a heat treatment is performed at 100° C. for 30 seconds to volatilize the solvent component of the above-mentioned coating film to form a conductive adhesive layer.

[0088] As described above, an electromagnetic wave shielding film having a structure of conductive adhesive layer / shielding layer / insulating layer was produced.

[0089] Examples 2 to 7 and Comparative Example 1

[0090] Except that the components constituting the insulating layer and the conductive adhesive layer were changed as shown in Table 1, the same procedure as in Example 1 was carried out to produce an electromagnetic wave shielding film.

[0091] (evaluate)

[0092] The electromagnetic wave shielding films obtained in the examples and comparative examples were evaluated below. The evaluation results are shown in Table 1.

[0093] (1) Martens hardness of the insulation layer

[0094] Each electromagnetic wave shielding film obtained in the examples and comparative examples was cut into a 1 mm square test sample, the separator on the insulating layer was peeled off, and the Martens hardness of the insulating layer surface was measured under the following conditions using a dynamic microhardness tester (trade name "DUH-211", manufactured by Shimadzu Corporation).

[0095] Indenter shape: triangular pyramid (115°)

[0096] Measurement method: Single extrusion measurement

[0097] Measurement temperature: 23°C

[0098] Load: 0.10mN

[0099] Loading speed: 0.0060mN / s

[0100] Loading hold time: 2s

[0101] Uninstall hold time: 0s.

[0102] (2) Martens hardness of the conductive adhesive layer

[0103] The Martens hardness of each conductive adhesive layer produced in each of Examples and Comparative Examples was measured in the same manner as the Martens hardness of the insulating layer.

[0104] (3) Connection resistance value

[0105] i) Fabrication of grounding components

[0106] Silver-coated nickel powder (average particle size 28 μm) was added to the epoxy resin composition so that the content ratio in the conductive adhesive layer was 35% by mass, thereby preparing an adhesive composition. Then, the adhesive composition was applied to a SUS sheet having a thickness of 0.2 mm so that the thickness of the formed conductive adhesive layer was 30 μm. Then, a heat treatment was performed at 100° C. for 30 seconds to volatilize the solvent component of the coating film and form a conductive adhesive layer. A grounding member consisting of a SUS sheet / conductive adhesive layer was prepared as above.

[0107] ii) Connection resistance value measurement

[0108] The grounding member obtained by the above steps was cut into a 10 mm square test sample, and it was placed on the surface of the insulating layer of each electromagnetic wave shielding film obtained in the embodiment and the comparative example at intervals of 10 mm, and joined by hot pressing to prepare a sample for measurement. The hot pressing was performed under the conditions of a temperature of 170°C, a pressure of 3 MPa, and a time of 30 minutes, and then post-cured at 150°C for 30 minutes. Then, the connection resistance value between adjacent grounding members was measured through the shielding layer of the electromagnetic wave shielding film.

[0109] [Table 1]

[0110]

[0111] It was determined that in the electromagnetic wave shielding film (Example) of the present invention, the connection resistance between adjacent grounding members was low, and excellent conductivity was exhibited between the grounding member and the shielding layer. On the other hand, when the ratio of the Martens hardness of the conductive adhesive layer to the Martens hardness of the insulating layer was less than 0.3 (Comparative Example 1), the connection resistance between adjacent grounding members exceeded the measurement limit.

[0112] Number Description

[0113] 1Electromagnetic wave shielding film

[0114] 11Conductive adhesive layer

[0115] 12 shielding layers

[0116] 13 Insulation layer

[0117] X-shielded printed circuit board

[0118] 2Printed circuit board

[0119] 21 Basic components

[0120] 22 Adhesive layer

[0121] 23 Circuit graphics

[0122] 23a signal circuit

[0123] 23b Grounding Circuit

[0124] 24 Insulation protection layer (covering film)

[0125] 25 through holes

[0126] 3 Grounding components

[0127] 31Conductive substrate

[0128] 32 Conductive adhesive

[0129] 3a Adhesive

[0130] 3b Conductive particles

[0131] 4 Electronic components

Claims

1. An electromagnetic wave shielding film, characterized in that: A conductive adhesive layer, a shielding layer and an insulating layer are sequentially stacked; The ratio of the Martens hardness of the conductive adhesive layer in accordance with ISO 14577-1 to the Martens hardness of the insulating layer in accordance with ISO 14577-1 [conductive adhesive layer / insulating layer] is 0.3 or more.

2. The electromagnetic wave shielding film according to claim 1, characterized in that: The Martens hardness of the insulating layer based on ISO14577-1 is 3 to 150 N / mm 2 .

3. The electromagnetic wave shielding film according to claim 1 or 2, characterized in that: The Martens hardness of the conductive adhesive layer according to ISO14577-1 is 20 to 200 N / mm 2 .

4. The electromagnetic wave shielding film according to claim 2, characterized in that: The Martens hardness of the insulating layer based on ISO14577-1 is 30 to 150 N / mm 2 .

5. The electromagnetic wave shielding film according to claim 3, characterized in that: The Martens hardness of the conductive adhesive layer according to ISO14577-1 is 50 to 170 N / mm 2 .