A control method for intermediate cooling of thick plates

By setting up sequential air cooling and water cooling processes in thick plate production, and adjusting the stroke rhythm according to the length of the rolled piece, the problem of long waiting time for the intermediate billet to be heated is solved, the rolling rhythm and production capacity are improved, and the difficulty of controlling the water cooling temperature drop is improved. The rolling efficiency is improved.

CN115069786BActive Publication Date: 2024-10-15BAOSHAN IRON & STEEL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202110276217.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-03-15
Publication Date
2024-10-15
Estimated Expiration
2041-03-15

AI Technical Summary

Technical Problem

In the production of thick plates, the long waiting time of the intermediate billet affects the production line productivity. In the existing technology, the air-cooling waiting time is long and the water cooling device is difficult to control the temperature drop at the head and tail of thick-sized steel plates, resulting in limited rolling rhythm and production capacity improvement.

Method used

Set up sequential air cooling and water cooling processes between rough rolling and finishing rolling, and establish a stroke rhythm according to the length of the rolled piece. The water cooling temperature drop and the roller speed are monitored and controlled in real time through the rough rolling exit thermometer and the finishing rolling entrance thermometer. , ensuring that each rolled piece reaches the target temperature when it reaches the finishing rolling entrance.

Benefits of technology

It shortens the waiting time of the intermediate billet, improves the rolling rhythm and hourly production capacity, avoids the head and tail blackhead phenomenon caused by separate multi-pass water cooling and the problem of too long waiting time for single air cooling, and realizes the rolling rhythm and rolling line production capacity. improvement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115069786B_ABST
    Figure CN115069786B_ABST
Patent Text Reader

Abstract

A control method for intermediate cooling and waiting for temperature of thick plates, an air cooling process and a water cooling process are sequentially arranged between the original rough rolling process and the finishing rolling process, by establishing sequential rough rolling, air cooling, water cooling, and finishing rolling processes, and establishing the travel rhythm of the front and rear rolled pieces according to the length of the rolled pieces, so that each rolled piece can form an orderly temperature control adapted to the target temperature when it reaches the finishing entrance. A control method for intermediate cooling and waiting for temperature of thick plates of the present invention, firstly, based on the original production line, a cooling waiting zone is arranged between rough rolling and finishing rolling, and the cooling waiting zone is composed of an air cooling zone and a water cooling zone arranged sequentially, and the rolling rhythm and hourly production capacity are improved by designing a waiting strategy of air cooling + water cooling, and at the same time, the cooling sequence of air cooling first and then water cooling can well improve the head and tail blackhead phenomenon caused by single multi-pass water cooling.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of slab rolling, and in particular relates to a method for controlling intermediate cooling and temperature treatment of thick plates. Background Art

[0002] Many types of steel in thick plate production require control of the start temperature of finishing rolling, so after the rough rolling is completed, the steel plate needs to be heated to a certain temperature before finishing rolling. Generally, the thicker the thickness, the longer the waiting time. Depending on the requirements, the waiting time of the intermediate billet is usually from a few minutes to tens of minutes, and for special steel types it can even reach more than 1 hour, which seriously affects the capacity improvement of the production line.

[0003] There are usually two ways to wait for thick plates to warm up: air cooling and water cooling. Air cooling waiting for warming is to swing the steel plate on the roller between rough rolling and finishing rolling for air cooling after rough rolling. The cooling speed is slow, which has a significant impact on the rolling rhythm. The finishing mill often needs to stop and wait for the air cooling process to complete. In order to alleviate the impact of the long air cooling waiting time, some steel mills adopt a production method of batch waiting for warming of multiple steel blocks when the distance between rough rolling and finishing rolling is long enough. The rolling rhythm has been improved, but the rhythm is still slow. For production lines with limited distance, the strategy of air cooling of multiple steel blocks cannot be effectively implemented. In order to shorten the waiting time, many thick plate mills have built intermediate water cooling devices on the rollers between rough rolling and finishing rolling, and use water cooling devices to achieve rapid cooling of the intermediate billet to improve production efficiency. However, for thick specifications, continuous water cooling for multiple passes will cause a significant temperature drop at the head and tail of the steel plate, making it difficult to control blackheads at the head and tail.

[0004] The invention application with application number: 200910104025.5 discloses "an intermediate billet cooling system and cooling control process". An aerosol cooling device body is arranged between a rough rolling mill and a finishing rolling mill. The aerosol cooling device body is composed of an upper cooling manifold and a lower cooling manifold. An aerosol nozzle and a compressed air pipe are installed on the cooling water pipes of the upper cooling manifold and the lower cooling manifold; the opening and closing control valves and flow control valves of the cooling water pipe and the compressed air pipe are connected to the control valve station. The cooling manifolds arranged near the rollers before and after the rolling mill control the aerosol cooling process of the intermediate billet by spraying water mist control technology on the cooling manifolds.

[0005] The invention application with application number: 201610361553.9 discloses "an inter-frame cooling equipment and hot rolling process". By arranging cooling equipment between the roughing mill and the finishing mill in the rolling process, it is beneficial to make the intermediate billet steel plate after roughing meet the finishing rolling temperature requirements as soon as possible, shorten the waiting time and the rolling cycle, and save energy and reduce consumption; the use of hot rolling is beneficial to improve the core toughness of the rolled steel plate, improve the core quality of the plate, thereby improving the steel plate flaw detection pass rate. It is characterized in that it includes a frame, a cooling manifold array is arranged on the frame, each cooling manifold is arranged on a nozzle array, the frame has a transverse crossing section of the cooling roller, the left end of the frame is the intermediate billet steel plate input end, and the right end of the frame is the intermediate billet steel plate output end.

[0006] The invention application with application number: 201010194568.3 discloses "a cooling method for intermediate billets in controlled rolling of medium and thick plates". The specific process is: the intermediate billets with a thickness range of 30 to 110 mm after rough rolling in the austenite recrystallization zone are rapidly cooled to 800 to 950°C by the transmission roller, and then enter the rolling mill for rolling in the non-recrystallization zone after short-term air cooling. The intermediate cooling process adopts high-density and ultra-density upper and lower headers to impact jet water cooling on the intermediate billets, and the specific process parameters are precisely controlled by computers.

[0007] The invention application with application number: 201110358731.X discloses "a device and rolling method for improving the hourly output of a single-stand medium plate rolling mill". The arrangement order of the process equipment of the single-stand rolling mill is: heating furnace, descaling box, intermediate billet waiting support, rolling mill, roller table, ACC; its rolling process steps are as follows: (1) the first intermediate billet enters the ACC for laminar cooling after the rolling mill, the second slab is opened in the rolling mill, and the third slab is taken out of the furnace; (2) the second intermediate billet is returned to the rolling mill and placed on the billet waiting support, the first intermediate billet is rolled into a finished product, and the third billet is sent to the descaling box for descaling; (3) the first steel plate is successfully rolled and leaves the rolling mill, the second intermediate billet is placed in the roller table and passes through the rolling mill to enter the ACC for laminar cooling, the third billet is opened, and the fourth billet is taken out of the furnace. Summary of the invention

[0008] In order to solve the above problems, the present invention provides a control method for intermediate cooling of thick plates, and the technical solution thereof is as follows:

[0009] A method for controlling intermediate cooling of thick plates, characterized in that:

[0010] An air cooling process and a water cooling process are sequentially set between the original rough rolling process and the finishing rolling process.

[0011] By establishing the rough rolling, air cooling, water cooling and finishing rolling processes in sequence, and establishing the travel rhythm of the front and rear rolled pieces according to the length of the rolled pieces, each rolled piece can form an orderly temperature control that is adapted to the target finishing rolling start temperature when it reaches the finishing rolling entrance.

[0012] A control method for intermediate cooling of thick plates according to the present invention is characterized in that:

[0013] The air cooling process and the water cooling process are sequentially arranged along the original roller table between the rough rolling process and the finishing rolling process;

[0014] The distance from the rough rolling outlet to the air cooling inlet is set to be greater than the longest intermediate billet length.

[0015] A control method for intermediate cooling of thick plates according to the present invention is characterized in that:

[0016] A rough rolling outlet temperature measuring instrument is arranged at the rough rolling outlet. The rough rolling, air cooling, water cooling, and finishing rolling processes are established in sequence, and the travel rhythm of the front and rear rolling pieces is established according to the length of the rolling pieces, so that each rolling piece can form an orderly temperature control adapted to the target finishing rolling start temperature when it arrives at the finishing rolling entrance. Specifically, the steps include:

[0017] S1: L2 reads the current rough rolling steel temperature value measured by the rough rolling outlet temperature measuring instrument from L1; L2 reads the corresponding rolled piece information from L3;

[0018] S2: L2 calculates the water cooling temperature drop and roller speed required for the rolled piece when the water flow density is the maximum according to the current rough rolling temperature value and the corresponding rolled piece information;

[0019] S3: comparing the calculated roller speed with the slowest speed of the water-cooled roller speed, and determining the number of water cooling passes required for the rolled piece according to the comparison result;

[0020] S4: L1 sends the water flow rate and water-cooling roller speed control instructions to the corresponding action execution end according to the water-cooling channel order calculated by L2.

[0021] A control method for intermediate cooling of thick plates according to the present invention is characterized in that:

[0022] A finishing rolling entrance temperature meter is set at the finishing rolling entrance. The temperature model of L2 is corrected by the real-time measurement value of the finishing rolling entrance temperature meter, and adaptive correction is established for subsequent rolled products based on this.

[0023] A control method for intermediate cooling of thick plates according to the present invention is characterized in that:

[0024] Step S2 is specifically as follows:

[0025] When the current rolled piece is the 0# rolled piece, the required water cooling temperature drop is determined by the following formula:

[0026] ΔT WC =T R -T F ,

[0027] The roller speed is determined by the following two equations:

[0028]

[0029]

[0030] When the current rolled piece is not a 0# rolled piece, the required water cooling temperature drop is determined by the following formula:

[0031] ΔT WC =T R -T F -ΔT AC ,

[0032] The roller speed is determined by the following two equations:

[0033]

[0034] in,

[0035] ΔT WC : Required water cooling temperature drop, unit: °C;

[0036] T R : Rough rolling and polishing temperature, unit: ℃;

[0037] T F : Finish rolling start setting temperature, unit: °C;

[0038] v: roller speed, unit: m / s;

[0039] L WC : Length of water-cooled roller, unit: m;

[0040] t WC : Water cooling time, unit: S;

[0041] C: Specific heat of steel plate; J / (kg℃);

[0042] m: mass, unit: kg;

[0043] h: heat transfer coefficient;

[0044] S: Steel plate water cooling heat exchange surface area, unit: m 2 ;

[0045] T 水 : Water temperature, unit: ℃;

[0046] ΔT AC : The temperature drop of the rolled piece during air cooling, unit: °C;

[0047] T wc : The temperature of the workpiece at the time of the last pass of finishing rolling of the previous workpiece, unit: ℃.

[0048] A control method for intermediate cooling of thick plates according to the present invention is characterized in that:

[0049] Step S3 is specifically as follows:

[0050] When the roller speed is greater than the slowest speed of the water-cooled roller, the water-cooling pass of the rolled piece is determined to be one pass;

[0051] When the roller speed is less than the slowest speed of the water-cooled roller, the water-cooling pass of the rolled piece is determined based on the water-cooled roller speed.

[0052] A control method for intermediate cooling of thick plates according to the present invention is characterized in that:

[0053] The process of establishing the travel rhythm of the front and rear rolled pieces according to the length of the rolled pieces is specifically as follows:

[0054] SA1: When the workpiece i is being finished rolled in the finishing process stage, the i+1 workpiece is controlled to be in the air cooling zone; and the difference between the sum of the lengths of the i+2 workpiece and the i+1 workpiece and the set length of the air cooling zone is calculated;

[0055] If the sum of the two is greater than the set length of the air cooling zone, the i+2 piece is controlled to wait in the rough rolling zone;

[0056] If the sum of the two is less than the set length of the air cooling zone, the i+2nd rolled piece is controlled to wait in the air cooling zone;

[0057] SA2: When the i-th workpiece is rolled in the last pass of positive casting, the i+1 workpiece is driven to enter the water cooling zone, and the front end of the i+2 workpiece is driven to run to the end position of the air cooling zone. At the same time, the difference between the sum of the lengths of the i+2 workpiece and the i+3 workpiece and the set length of the air cooling zone is calculated;

[0058] If the sum of the two is greater than the set length of the air cooling zone, the i+3 piece is controlled to wait in the rough rolling zone;

[0059] If the sum of the two is less than the set length of the air cooling zone, the i+3 rolled piece is controlled to wait in the air cooling zone.

[0060] A control method for intermediate cooling of thick plates according to the present invention is characterized in that:

[0061] The h is determined by the following formula:

[0062] h=0.277×(1060-T WC )f 0.35 ×θ,

[0063] in,

[0064] h: heat transfer coefficient;

[0065] T wc : The temperature of the rolled piece at the time of the last pass of the finishing rolling forward casting of the previous rolled piece, unit: ℃;

[0066] f: water flow density, unit: L / (min·m 2 )

[0067] θ: Adaptive coefficient.

[0068] A control method for intermediate cooling of thick plates according to the present invention is characterized in that:

[0069] The ΔT AC Determined by the following formula:

[0070]

[0071] in,

[0072] ΔT AC : The temperature drop of the rolled piece during air cooling, unit: °C;

[0073] t AC : Air cooling time, unit: S;

[0074] A: Steel plate surface area, unit: m 2 ;

[0075] σ: Stefan-Bolzman constant;

[0076] ε: blackness coefficient;

[0077] T R : Rough rolling and polishing temperature, unit: ℃;

[0078] T ∞ : Ambient temperature, unit: ℃.

[0079] A control method for intermediate cooling of thick plates according to the present invention is characterized in that:

[0080] When the roller speed is less than the slowest speed of the water-cooled roller speed, the slowest speed of the water-cooled roller speed is set as the roller speed, and the water cooling pass of the rolled piece is determined accordingly, which is specifically determined by the following formula:

[0081]

[0082] in,

[0083] n: required cooling passes;

[0084] t WC : Water cooling time, unit: S;

[0085] v min : The slowest roller speed of the water-cooled roller, unit: m / s;

[0086] L WC : Length of water cooling section, unit: m.

[0087] The invention discloses a control method for intermediate cooling and waiting for temperature of thick plates. First, based on the original production line, a cooling waiting zone is set between rough rolling and finishing rolling. The cooling waiting zone is composed of an air cooling zone and a water cooling zone set in sequence. The waiting temperature strategy of air cooling + water cooling is designed to improve the rolling rhythm and hourly production capacity. At the same time, the cooling sequence of air cooling first and then water cooling can well improve the black head phenomenon at the head and tail caused by single multi-pass water cooling and the problem of too long waiting time for single air cooling. At the same time, since this scheme is developed based on the existing production line, and the space of the existing production line is limited, in order to first ensure that the rough rolling cast steel does not interfere with the rolled piece in the air cooling zone, the distance from the rough rolling outlet to the air cooling zone entrance must be set. The distance must be greater than the longest rolled piece length, and the length setting of the air cooling zone must be considered later. It can accommodate at least 1-2 rolled pieces for air cooling. In addition, the water cooling setting will inevitably cause the distance from the water cooling outlet to the finishing entrance to be less than the longest rolled piece, which may affect the finishing steel casting in the water cooling zone, which will inevitably bring about further problems in controlling the beat setting. The present invention further solves this problem well through the control of the beat, from the scheme concept to the practical operation of the scheme, shortening the waiting time of the intermediate billet and reducing the idling waiting time of the finishing mill have been put into practice, thereby achieving an improvement in the rolling rhythm and the rolling line capacity. BRIEF DESCRIPTION OF THE DRAWINGS

[0088] Figure 1 It is a schematic diagram of the production line layout of the present invention;

[0089] Figure 2 It is a schematic diagram of the temperature control steps of the rolled piece waiting for temperature in the present invention;

[0090] Figure 3 The present invention is a flow chart for establishing the travel cycle of the front and rear rolling pieces according to the length of the rolling piece. DETAILED DESCRIPTION

[0091] Next, a control method for intermediate cooling of thick plates according to the present invention will be further described in detail according to the accompanying drawings and specific implementation methods.

[0092] like Figure 1 A control method for intermediate cooling of thick plates is shown in FIG.

[0093] An air cooling process and a water cooling process are sequentially set between the original rough rolling process and the finishing rolling process.

[0094] By establishing the rough rolling, air cooling, water cooling and finishing rolling processes in sequence, and establishing the travel rhythm of the front and rear rolled pieces according to the length of the rolled pieces, each rolled piece can form an orderly temperature control that is adapted to the target finishing rolling start temperature when it reaches the finishing rolling entrance.

[0095] in,

[0096] The air cooling process and the water cooling process are sequentially arranged along the original roller table between the rough rolling process and the finishing rolling process;

[0097] The distance from the rough rolling outlet to the air cooling inlet is set to be greater than the longest intermediate billet length.

[0098] in,

[0099] A rough rolling outlet temperature measuring instrument is set at the rough rolling outlet. By establishing the rough rolling, air cooling, water cooling, and finishing rolling processes in sequence, and establishing the travel rhythm of the front and rear rolling pieces according to the length of the rolling pieces, each rolling piece can form an orderly temperature control adapted to the target finishing rolling start temperature when it reaches the finishing rolling entrance, such as Figure 2 As shown, the specific steps include:

[0100] S1: L2 reads the current rough rolling steel temperature value measured by the rough rolling outlet temperature measuring instrument from L1; L2 reads the corresponding rolled piece information from L3;

[0101] S2: L2 calculates the water cooling temperature drop and roller speed required for the rolled piece when the water flow density is the maximum according to the current rough rolling temperature value and the corresponding rolled piece information;

[0102] S3: comparing the calculated roller speed with the slowest speed of the water-cooled roller speed, and determining the number of water cooling passes required for the rolled piece according to the comparison result;

[0103] S4: L1 sends the water flow rate and water-cooling roller speed control instructions to the corresponding action execution end according to the water-cooling channel order calculated by L2.

[0104] in,

[0105] A finishing rolling entrance temperature meter is set at the finishing rolling entrance. The temperature model of L2 is corrected by the real-time measurement value of the finishing rolling entrance temperature meter, and adaptive correction is established for subsequent rolled products based on this.

[0106] in,

[0107] Step S2 is specifically as follows:

[0108] When the current rolled piece is the 0# rolled piece, the required water cooling temperature drop is determined by the following formula:

[0109] ΔT WC =T R -T F ,

[0110] The roller speed is determined by the following two equations:

[0111]

[0112]

[0113] When the current rolled piece is not a 0# rolled piece, the required water cooling temperature drop is determined by the following formula:

[0114] ΔT WC =T R -T F -ΔT AC ,

[0115] The roller speed is determined by the following two equations:

[0116]

[0117] in,

[0118] ΔT WC : Required water cooling temperature drop, unit: °C;

[0119] T R : Rough rolling and polishing temperature, unit: ℃;

[0120] T F : Finish rolling start setting temperature, unit: °C;

[0121] v: roller speed, unit: m / s;

[0122] L WC : Length of water-cooled roller, unit: m;

[0123] t WC : Water cooling time, unit: S;

[0124] C: Specific heat of steel plate; J / (kg℃);

[0125] m: mass, unit: kg;

[0126] h: heat transfer coefficient;

[0127] S: Steel plate water cooling heat exchange surface area, unit: m 2 ;

[0128] T 水 : Water temperature, unit: ℃;

[0129] ΔT AC: The temperature drop of the rolled piece during air cooling, unit: °C;

[0130] T wc : The temperature of the workpiece at the time of the last pass of finishing rolling of the previous workpiece, unit: ℃.

[0131] in,

[0132] Step S3 is specifically as follows:

[0133] When the roller speed is greater than the slowest speed of the water-cooled roller, the water-cooling pass of the rolled piece is determined to be one pass;

[0134] When the roller speed is less than the slowest speed of the water-cooled roller, the water-cooling pass of the rolled piece is determined based on the water-cooled roller speed.

[0135] in,

[0136] The travel rhythm of the front and rear rolled pieces is established according to the length of the rolled piece, such as Figure 3 As shown, specifically:

[0137] SA1: When the workpiece i is being finished rolled in the finishing process stage, the i+1 workpiece is controlled to be in the air cooling zone; and the difference between the sum of the lengths of the i+2 workpiece and the i+1 workpiece and the set length of the air cooling zone is calculated;

[0138] If the sum of the two is greater than the set length of the air cooling zone, the i+2 piece is controlled to wait in the rough rolling zone;

[0139] If the sum of the two is less than the set length of the air cooling zone, the i+2nd rolled piece is controlled to wait in the air cooling zone;

[0140] SA2: When the i-th workpiece is rolled in the last pass of positive casting, the i+1 workpiece is driven to enter the water cooling zone, and the front end of the i+2 workpiece is driven to run to the end position of the air cooling zone. At the same time, the difference between the sum of the lengths of the i+2 workpiece and the i+3 workpiece and the set length of the air cooling zone is calculated;

[0141] If the sum of the two is greater than the set length of the air cooling zone, the i+3 piece is controlled to wait in the rough rolling zone;

[0142] If the sum of the two is less than the set length of the air cooling zone, the i+3 rolled piece is controlled to wait in the air cooling zone.

[0143] in,

[0144] The h is determined by the following formula:

[0145] h=0.277×(1060-T WC )f 0.35 ×θ,

[0146] in,

[0147] h: heat transfer coefficient;

[0148] T wc : The temperature of the rolled piece at the time of the last pass of the finishing rolling forward casting of the previous rolled piece, unit: ℃;

[0149] f: water flow density, unit: L / (min·m 2 )

[0150] θ: Adaptive coefficient.

[0151] in,

[0152] The ΔT AC Determined by the following formula:

[0153]

[0154] in,

[0155] ΔT AC : The temperature drop of the rolled piece during air cooling, unit: °C;

[0156] t AC : Air cooling time, unit: S;

[0157] A: Steel plate surface area, unit: m 2 ;

[0158] σ: Stefan-Bolzman constant;

[0159] ε: blackness coefficient;

[0160] T R : Rough rolling and polishing temperature, unit: ℃;

[0161] T ∞ : Ambient temperature, unit: ℃.

[0162] in,

[0163] When the roller speed is less than the slowest speed of the water-cooled roller speed, the slowest speed of the water-cooled roller speed is set as the roller speed, and the water cooling pass of the rolled piece is determined accordingly, which is specifically determined by the following formula:

[0164]

[0165] in,

[0166] n: required cooling passes;

[0167] t WC : Water cooling time, unit: S;

[0168] v min: The slowest roller speed of the water-cooled roller, unit: m / s;

[0169] L WC : Length of water cooling section, unit: m.

[0170] Working process, principle and implementation example

[0171] like Figure 1 The production line layout shown in the figure: the roughing mill, the roughing mill outlet temperature measuring instrument, the air cooling waiting area, the water cooling device, the finishing mill inlet temperature measuring instrument and the finishing mill are arranged along the rolling direction of the rolling production line; the length of the air cooling waiting area is L ac ; The length of the water cooling device is L wc ; The total waiting length for air cooling + water cooling is LT = Lwc + Lac; The distance from the roughing mill outlet to the entrance of the air cooling waiting zone is L1; The distance from the water cooling outlet to the finishing mill is L2; ​​The temperature measuring instruments at the roughing mill outlet and the finishing mill entrance are used to detect the temperature of the steel plate before and after the waiting. Due to the length of the existing production line, the distance between roughing and finishing rolling is shorter during layout, and the distance from the roughing mill outlet to the entrance of the air cooling waiting zone is L1> the longest intermediate billet length, so as to ensure that the rough-rolled steel does not interfere with the intermediate billet in the air cooling waiting zone; The air cooling waiting distance is limited, and the number of steel plates waiting for heating varies according to the length of the steel plate, 1-2 pieces; The distance from the water cooling outlet to the entrance of the finishing mill is L2< the longest finished product length, that is, the finishing steel will occupy the water-cooled roller; The maximum water flow density of the water cooling device is f max , the slowest speed of water-cooled roller is v min .

[0172] When specific control:

[0173] For the first steel of the rolling line, after the billet is rough rolled into 0# intermediate billet, the L2 process control system sets the finishing mill rolling temperature T according to the received information of the intermediate billet (specifications, F , actual steel polishing temperature T R etc.) Calculate the temperature drop ΔT to be achieved: ΔT = T R -T F

[0174] Calculate the maximum water flow density f max The cooling roller speed v required to achieve the ΔT temperature drop of 0# billet under the following conditions.

[0175] If v>v min Then the water cooling pass n = 1, water cooling continues; if v <v min , then the roller speed is v min , calculate the maximum water flow density f max , slowest roller speed v min Required number of cooling passes n.

[0176] The control model sends the roller speed v, cooling pass number n and water flow density f to the first-stage machine. max, the water cooling device opens the switch valve and the regulating valve, adjusts the water flow density to the target value, and the 0# intermediate billet enters the water cooling device at a speed v to start water cooling for n passes, and then enters the finishing mill for rolling;

[0177] The rough rolled 1# intermediate billet is sent to the air cooling waiting area for heating. Since the reverse casting of the 0# billet in the finishing rolling stage will occupy the water cooling area, the water cooling area is vacant during the 0# billet finishing rolling process, and the 1# billet does not enter the water cooling area.

[0178] When the 0# billet is rolled in the last pass, calculate the air cooling temperature drop ΔT of the 1# billet. AC and the temperature T at that moment WC . Just use the common radiation heat transfer formula.

[0179] Calculate the water flow density to the maximum value f max When the temperature of billet 1# is lowered to the finishing rolling start temperature TF, the water cooling temperature drop ΔT WC and roller speed v;

[0180] If v>v min Then the water cooling pass n = 1, water cooling continues, and 1# enters the water cooling area while 2# billet moves to the front station; if v <v min , then the roller speed is v min , calculate the maximum water flow density f max , slowest roller speed v min Required number of cooling passes n.

[0181] The control model sends the roller speed and water flow density of the water cooling device to the first-stage machine. The water cooling device opens the switch valve and the regulating valve. After adjusting the water flow density to the target value, the 1# intermediate billet enters the water cooling device at a speed of v and starts water cooling for n passes. The subsequent 2# intermediate billet stays in the original air-cooled roller area to wait for temperature, avoiding the forward movement affecting the multi-pass water cooling of the 1# billet.

[0182] After water cooling, the 1# intermediate billet enters the finishing mill for rolling. The temperature measuring instrument at the entrance of the finishing mill is used to determine whether the temperature of the intermediate billet meets the target temperature after being heated, and the calculation model is corrected according to the temperature deviation. The control method of the subsequent intermediate billet is the same as that of the 1# billet.

[0183] After the rough rolling of 3# billet is completed, if there is vacancy in the air cooling waiting zone and the length of the vacancy is greater than the length of 3# billet, 3# billet will enter the air cooling waiting zone, otherwise it will continue to wait in the rough rolling mill area until the space in the air cooling waiting zone meets the requirements.

[0184] For example:

[0185] Air cooling waiting area length L ac =22m, the length of the water cooling device is L wc =12m;

[0186] 0# billet length 8m (thickness 100mm, width 3200mm), 1# billet length 8m (thickness 80mm, width 2800mm), 2# billet length 12m (thickness 100mm, width 3000mm);

[0187] The distance from the roughing mill outlet to the air cooling waiting zone entrance is L1 = 18m, and the distance from the water cooling outlet to the finishing mill is L2 = 32m;

[0188] Rough rolling temperature T R =950℃, finishing rolling start temperature T F =880℃;

[0189] Specific heat of steel plate c = 490 J / (kg℃); ambient temperature is 25℃;

[0190] According to the above method, we can calculate:

[0191] 1) The temperature drop of the 0# intermediate billet should be ΔT = T R -T F =950-880=70℃;

[0192] 2) Calculate the maximum water flow density f max The roller speed v of the 0# billet water cooling under the conditions.

[0193] Intermediate billet water cooling process, Q = c × m × ΔT WC =(T WC -T 水 )·t WC ·S·h

[0194] Where T WC =T R -ΔT AC , represents the temperature of the intermediate billet at the start of water cooling, ℃, for 0# billet, T WC =T R ; S is the water-cooled heat exchange surface area of ​​the steel plate, m 2 ; The heat transfer coefficient h can be obtained by using an empirical formula (the method of the present invention is explained by the following empirical formula):

[0195] h=0.277×(1060-T WC )f 0.35 ×θ

[0196] In summary, water cooling time

[0197]

[0198] Roller speed

[0199] Where T 水 is water temperature, 30℃; tWC is the water cooling time, s, unknown quantity; f is the water flow density, 600L / (min·m 2 ), θ is the adaptive coefficient 1.182.

[0200] 3) The slowest roller speed is 0.5m / s, so the slowest roller speed v min = 0.5 required cooling passes

[0201]

[0202] 4) Open the switch valve and regulating valve, and adjust the water flow density to 600L / (min·m 2 ), the 0# intermediate billet begins to be water-cooled and then enters the finishing mill for rolling;

[0203] 5) The rough rolled 1# intermediate billet is sent to the air cooling waiting area to wait for temperature.

[0204] 6) When the 0# billet is rolled in the last pass, the 1# billet has been air-cooled for a period of time t AC = 146s, then the air cooling temperature drop of 1# billet is ΔT AC and the temperature T at that moment WC as follows:

[0205]

[0206]

[0207] Where, c is the specific heat of the steel plate, 490 J / (kg℃); m is the mass, kg; T R is the rough rolling temperature of 950℃, i.e. the starting temperature of the waiting temperature, ℃; A is the surface area of ​​the steel plate; T ∞ is the ambient temperature; Stefan-Bolzman constant σ=5.768×10 -8 ,J / (m 2 s℃ 4 );ε is the blackness coefficient, which is usually between 0.6 and 0.9 in the air-cooled state of hot-rolled steel plates.

[0208] 7) Calculate the water cooling temperature drop ΔT required for billet 1 WC and roller speed v;

[0209] Total temperature drop ΔT = T R -T F =ΔT AC +ΔT WC

[0210] Water cooling temperature drop

[0211] Water cooling time

[0212] Roller speed

[0213] 8) Roller speed 0.97m / s> slowest roller speed, one cooling pass is enough. When 1# enters the water cooling area, 2# billet moves to the next station;

[0214] Open the switch valve and regulating valve of the water cooling device and adjust the water flow density to 600L / (min·m 2 ) After that, the 1# intermediate billet is water cooled once. The control method of the subsequent intermediate billet is the same as that of the 1# billet.

[0215] The invention discloses a control method for intermediate cooling and waiting for temperature of thick plates. First, based on the original production line, a cooling waiting zone is set between rough rolling and finishing rolling. The cooling waiting zone is composed of an air cooling zone and a water cooling zone set in sequence. The waiting temperature strategy of air cooling + water cooling is designed to improve the rolling rhythm and hourly production capacity. At the same time, the cooling sequence of air cooling first and then water cooling can well improve the black head phenomenon at the head and tail caused by single multi-pass water cooling and the problem of too long waiting time for single air cooling. At the same time, since this scheme is developed based on the existing production line, and the space of the existing production line is limited, in order to first ensure that the rough rolling cast steel does not interfere with the rolled piece in the air cooling zone, the distance from the rough rolling outlet to the air cooling zone entrance must be set. The distance must be greater than the longest rolled piece length, and the length setting of the air cooling zone must be considered later. It can accommodate at least 1-2 rolled pieces for air cooling. In addition, the water cooling setting will inevitably cause the distance from the water cooling outlet to the finishing entrance to be less than the longest rolled piece, which may affect the finishing steel casting in the water cooling zone, which will inevitably bring about further problems in controlling the beat setting. The present invention further solves this problem well through the control of the beat, from the scheme concept to the practical operation of the scheme, shortening the waiting time of the intermediate billet and reducing the idling waiting time of the finishing mill have been put into practice, thereby achieving an improvement in the rolling rhythm and the rolling line capacity.

Claims

1. A method for controlling the intermediate cooling of thick plates, characterized in that: An air cooling process and a water cooling process are sequentially set between the original rough rolling process and the finishing rolling process. By establishing the rough rolling, air cooling, water cooling, and finishing rolling processes in sequence, and establishing the travel rhythm of the front and rear rolled pieces according to the length of the rolled pieces, each rolled piece can form an orderly temperature control that is adapted to the target finishing rolling start temperature when it reaches the finishing rolling entrance. The air cooling process and the water cooling process are sequentially arranged along the original roller table between the rough rolling process and the finishing rolling process; The distance from the rough rolling outlet to the air cooling inlet is set to be greater than the longest intermediate billet length. A rough rolling outlet temperature measuring instrument is arranged at the rough rolling outlet. The rough rolling, air cooling, water cooling, and finishing rolling processes are established in sequence, and the travel rhythm of the front and rear rolling pieces is established according to the length of the rolling pieces, so that each rolling piece can form an orderly temperature control adapted to the target finishing rolling start temperature when it arrives at the finishing rolling entrance. Specifically, the steps include: S1: L2 reads the current rough rolling steel temperature value measured by the rough rolling outlet temperature measuring instrument from L1; L2 reads the corresponding rolled piece information from L3; S2: L2 calculates the water cooling temperature drop and roller speed required for the rolled piece when the water flow density is the maximum according to the current rough rolling temperature value and the corresponding rolled piece information; S3: comparing the calculated roller speed with the slowest speed of the water-cooled roller speed, and determining the number of water cooling passes required for the rolled piece according to the comparison result; S4: L1 sends the water flow rate and water-cooling roller speed control instructions to the corresponding action execution end according to the water-cooling pass number calculated by L2; The process of establishing the travel rhythm of the front and rear rolled pieces according to the length of the rolled pieces is specifically as follows: SA1: When the workpiece i is being finished rolled in the finishing process stage, the i+1 workpiece is controlled to be in the air cooling zone; and the difference between the sum of the lengths of the i+2 workpiece and the i+1 workpiece and the set length of the air cooling zone is calculated; If the sum of the two is greater than the set length of the air cooling zone, the i+2 piece is controlled to wait in the rough rolling zone; If the sum of the two is less than the set length of the air cooling zone, the i+2nd rolled piece is controlled to wait in the air cooling zone; SA2: When the i-th workpiece is rolled in the last pass of positive casting, the i+1 workpiece is driven to enter the water cooling zone, and the front end of the i+2 workpiece is driven to run to the end position of the air cooling zone. At the same time, the difference between the sum of the lengths of the i+2 workpiece and the i+3 workpiece and the set length of the air cooling zone is calculated; If the sum of the two is greater than the set length of the air cooling zone, the i+3 piece is controlled to wait in the rough rolling zone; If the sum of the two is less than the set length of the air cooling zone, the i+3 rolled piece is controlled to wait in the air cooling zone.

2. A method for controlling intermediate cooling of thick plates according to claim 1, characterized in that: A finishing rolling entrance temperature meter is set at the finishing rolling entrance. The temperature model of L2 is corrected by the real-time measurement value of the finishing rolling entrance temperature meter, and adaptive correction is established for subsequent rolled products based on this.

3. A method for controlling intermediate cooling of thick plates according to claim 1, characterized in that: Step S2 is specifically as follows: When the current rolled piece is the 0# rolled piece, the required water cooling temperature drop is determined by the following formula: ΔT WC =T R -T F , The roller speed is determined by the following two equations: When the current rolled piece is not a 0# rolled piece, the required water cooling temperature drop is determined by the following formula: ΔT WC =T R -T F -ΔT AC , The roller speed is determined by the following two equations: in, ΔT WC : Required water cooling temperature drop, unit: °C; T R : Rough rolling and polishing temperature, unit: ℃; T F : Finish rolling start setting temperature, unit: °C; v: roller speed, unit: m / s; L WC : Length of water-cooled roller, unit: m; t WC : Water cooling time, unit: S; C: Specific heat of steel plate; J / (kg℃); m: mass, unit: kg; h: heat transfer coefficient; S: Steel plate water cooling heat exchange surface area, unit: m 2 ; T 水 : Water temperature, unit: ℃; ΔT AC : The temperature drop of the rolled piece during air cooling, unit: °C; T wc : The temperature of the workpiece at the time of the last pass of finishing rolling of the previous workpiece, unit: ℃.

4. A method for controlling intermediate cooling of thick plates according to claim 1, characterized in that: Step S3 is specifically as follows: When the roller speed is greater than the slowest speed of the water-cooled roller, the water-cooling pass of the rolled piece is determined to be one pass; When the roller speed is less than the slowest speed of the water-cooled roller, the water-cooling pass of the rolled piece is determined based on the water-cooled roller speed.

5. A method for controlling intermediate cooling of thick plates according to claim 3, characterized in that: The h is determined by the following formula: h=0.277×(1060-T WC )f 0.35 ×θ, in, h: heat transfer coefficient; T wc : The temperature of the rolled piece at the time of the last pass of the finishing rolling forward casting of the previous rolled piece, unit: ℃; f: water flow density, unit: L / (min·m 2 ) θ: Adaptive coefficient.

6. A method for controlling intermediate cooling of thick plates according to claim 3, characterized in that: The ΔT AC Determined by the following formula: in, ΔT AC : The temperature drop of the rolled piece during air cooling, unit: °C; t AC : Air cooling time, unit: S; A: Steel plate surface area, unit: m 2 ; σ: Stefan-Bolzman constant; ε: blackness coefficient; T R : Rough rolling and polishing temperature, unit: ℃; T ∞ : Ambient temperature, unit: ℃.

7. A method for controlling intermediate cooling of thick plates according to claim 4, characterized in that: When the roller speed is less than the slowest speed of the water-cooled roller speed, the slowest speed of the water-cooled roller speed is set as the roller speed, and the water cooling pass of the rolled piece is determined accordingly, which is specifically determined by the following formula: in, n: required cooling passes; t WC : Water cooling time, unit: S; v min : The slowest roller speed of the water-cooled roller, unit: m / s; L WC : Length of water cooling section, unit: m.

Citation Information

Patent Citations

  • Intermediate blank cooling system and cooling control technology

    CN101642780A

  • Cooling method of heavy and medium plate controlled rolling intermediate blank

    CN101829688A

  • Device for improving hourly yield of single-chassis medium plate mill and rolling method thereof

    CN102430569A

  • Cooling equipment between racks and hot core rolling technology

    CN105855305A

  • Method for cooling intermediate billet of medium-thickness plate by using equipment for cooling after rolling

    CN102513384A