A flexible capacitor and a method for preparing the same

By using magnesium perchlorate solution and high molecular polymer in flexible capacitors to prepare flexible quasi-solid hydrogel electrolytes, the problem of poor performance of capacitors in low-temperature environments is solved, and stable operation and high energy under extreme low-temperature conditions are achieved. Density to meet the energy supply needs of flexible electronic devices.

CN115116758BActive Publication Date: 2024-10-22ZINERGY SHENZHEN LTD

Patent Information

Application Number
CN202210809490.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-11
Publication Date
2024-10-22
Estimated Expiration
2042-07-11

AI Technical Summary

Technical Problem

Existing capacitors have poor performance in low-temperature environments, cannot work stably, and cannot meet the energy supply needs of flexible electronic devices under extreme low-temperature conditions.

Method used

A flexible quasi-solid hydrogel electrolyte is prepared by combining a magnesium perchlorate solution with a high molecular polymer, and is sandwiched between a flexible anode and a cathode to form a flexible capacitor, taking advantage of the low-temperature resistance and high conductivity of magnesium perchlorate. efficiency characteristics and avoid the use of harmful organic additives.

Benefits of technology

It has achieved the goal of maintaining good mechanical and electrochemical properties under low temperature conditions. It is a flexible capacitor with low temperature resistance, high energy density and good mechanical properties. It can work stably in the temperature range of -40-25℃, meeting the requirements of flexible electronic equipment. Energy supply demand.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115116758B_ABST
    Figure CN115116758B_ABST
Patent Text Reader

Abstract

The present invention discloses a flexible capacitor and a preparation method thereof, wherein the flexible capacitor comprises a flexible quasi-solid hydrogel electrolyte, a flexible anode and a flexible cathode, wherein the flexible quasi-solid hydrogel electrolyte is sandwiched between the flexible anode and the flexible cathode; the flexible quasi-solid hydrogel electrolyte comprises a magnesium perchlorate solution and a polymer; wherein the polymer comprises at least one of polyacrylamide, polyvinyl alcohol, polyvinylidene fluoride, polyethylene, polypropylene, polytetrafluoroethylene, polystyrene, polymethyl methacrylate, polyhydroxyethyl methacrylate and polyimide. The flexible capacitor disclosed in the present invention can solve the technical problem that the current capacitor has poor low temperature resistance and cannot normally supply energy to flexible electronic devices under low temperature conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of energy storage devices, and in particular relates to a flexible capacitor and a preparation method thereof. Background Art

[0002] With the rapid development of electronic technology, the development of flexible electronic devices such as electronic skin, foldable mobile phones and wearable devices has attracted widespread attention. As energy storage devices that provide energy for various flexible electronic devices, capacitors are naturally required to have higher performance in all aspects as flexible electronic devices are updated.

[0003] Current capacitors generally have the problem of poor low-temperature resistance. They cannot work stably in low-temperature environments, and thus cannot meet the needs of normal power supply for flexible electronic devices under extreme low-temperature conditions. Summary of the invention

[0004] In order to overcome the above-mentioned shortcomings of the prior art, the purpose of the present invention is to provide a flexible capacitor, aiming to solve the technical problem that the current capacitor has poor low-temperature resistance and cannot normally supply energy for flexible electronic devices under low temperature conditions.

[0005] In order to achieve the purpose, the technical solution adopted by the present invention is as follows:

[0006] A flexible capacitor, comprising a flexible quasi-solid hydrogel electrolyte, a flexible anode and a flexible cathode, wherein the flexible quasi-solid hydrogel electrolyte is sandwiched between the flexible anode and the flexible cathode;

[0007] The flexible quasi-solid hydrogel electrolyte comprises a magnesium perchlorate solution and a polymer; wherein the polymer comprises at least any one of polyacrylamide, polyvinyl alcohol, polyvinylidene fluoride, polyethylene, polypropylene, polytetrafluoroethylene, polystyrene, polymethyl methacrylate, polyhydroxyethyl methacrylate, and polyimide.

[0008] Correspondingly, the present invention also proposes a method for preparing a flexible capacitor, which is used to manufacture the flexible capacitor as described above. The method for preparing the flexible capacitor comprises the following steps:

[0009] Dissolving magnesium perchlorate powder in water to prepare a magnesium perchlorate solution;

[0010] Adding a high molecular polymer to the magnesium perchlorate solution and stirring the mixture to obtain a first mixed solution; wherein the high molecular polymer comprises at least one of polyacrylamide, polyvinyl alcohol, polyvinylidene fluoride, polyethylene, polyacrylic acid, polystyrene, polymethyl methacrylate, polyhydroxyethyl methacrylate, and polyimide;

[0011] Injecting the first mixed solution into a molding mold to form the flexible quasi-solid hydrogel electrolyte;

[0012] The flexible quasi-solid hydrogel electrolyte is sandwiched between the flexible anode and the flexible cathode.

[0013] Correspondingly, the present invention also proposes a method for preparing a flexible capacitor, which is used to manufacture the flexible capacitor as described above. The method for preparing the flexible capacitor comprises the following steps:

[0014] Dissolving magnesium perchlorate powder in water to prepare a magnesium perchlorate solution;

[0015] adding acrylamide, ammonium persulfate and N,N'-methylenebisacrylamide to the magnesium perchlorate solution and stirring to obtain the first mixed solution;

[0016] Injecting the first mixed solution into a molding mold, and heating the first mixed solution to cause the first mixed solution to undergo a polymerization reaction and form the flexible quasi-solid hydrogel electrolyte;

[0017] The flexible quasi-solid hydrogel electrolyte is sandwiched between the flexible anode and the flexible cathode.

[0018] Furthermore, the step of dissolving magnesium perchlorate powder in water to prepare a magnesium perchlorate solution comprises:

[0019] The magnesium perchlorate solution is prepared by dissolving magnesium perchlorate powder and manganese sulfate powder in water.

[0020] Furthermore, the concentration of the magnesium perchlorate solution is 0.5-8 mol / L.

[0021] Furthermore, the step of adding acrylamide, ammonium persulfate and N,N'-methylenebisacrylamide to the magnesium perchlorate solution and stirring to obtain the first mixed solution comprises:

[0022] Add acrylamide, ammonium persulfate and N,N'-methylenebisacrylamide to the magnesium perchlorate solution and stir for 0.25-2 hours to obtain the first mixed solution.

[0023] Furthermore, the mass ratio of the magnesium perchlorate solution, the acrylamide, the ammonium persulfate and the N,N'-methylenebisacrylamide is 31000:3000:15:2.

[0024] Furthermore, the step of heating the first mixed solution comprises:

[0025] The forming mold is placed in an oven to perform the heating operation on the first mixed solution; wherein the heating temperature of the heating operation is 60-90° C., and the heating time of the heating operation is 2-5 hours.

[0026] Furthermore, before the step of sandwiching the flexible quasi-solid hydrogel electrolyte between the flexible anode and the flexible cathode, the step includes:

[0027] Mixing activated carbon powder, conductive carbon black and polyvinylidene fluoride in N-methylpyrrolidone and stirring to prepare a second mixed solution;

[0028] Applying the second mixed solution on a first carbon cloth, and performing a first drying operation on the first carbon cloth to form the flexible anode;

[0029] Mixing manganese dioxide powder, conductive carbon black and polyvinylidene fluoride in N-methylpyrrolidone and stirring to prepare a third mixed solution;

[0030] The third mixed solution is coated on a second carbon cloth, and a second drying operation is performed on the second carbon cloth to form the flexible cathode.

[0031] Furthermore, before the step of mixing manganese dioxide powder, conductive carbon black and polyvinylidene fluoride in N-methylpyrrolidone and stirring to prepare a third mixed solution, the step includes:

[0032] Dissolving potassium permanganate and manganese sulfate powder in water and stirring to prepare a fourth mixed solution;

[0033] injecting the fourth mixed solution into a polytetrafluoroethylene reactor and performing a hydrothermal reaction to obtain a manganese dioxide precipitate;

[0034] The manganese dioxide precipitate is dried to obtain the manganese dioxide powder.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] The flexible capacitor proposed in the present invention makes full use of the characteristics of magnesium perchlorate such as good low-temperature resistance and high conductivity, and prepares a flexible quasi-solid hydrogel electrolyte by mixing a low-cost, low-concentration magnesium perchlorate solution with a high molecular polymer. There is no need to add organic additives that may cause harm to the human body and the environment. The flexible quasi-solid hydrogel electrolyte prepared in this way is safe and non-toxic and can maintain good mechanical and electrochemical properties under low temperature conditions. The flexible capacitor further prepared by combining the flexible quasi-solid hydrogel electrolyte with a flexible anode and a flexible cathode also has the advantages of low-temperature resistance, high energy density, good mechanical properties, etc., and can work stably under low temperature conditions, thereby meeting the demand for powering flexible electronic devices under low temperature climate conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0038] Figure 1 It is a schematic diagram of the process of the first embodiment of the method for preparing a flexible capacitor of the present invention;

[0039] Figure 2 It is a schematic flow chart of a second embodiment of a method for preparing a flexible capacitor of the present invention;

[0040] Figure 3 It is a schematic diagram of the conductivity variation characteristics of various substances used to make electrolytes with temperature;

[0041] Figure 4 Schematic diagram for comparing the specific capacities of the two electrolytes;

[0042] Figure 5 It is a schematic diagram of the process of the third embodiment of the method for preparing a flexible capacitor of the present invention;

[0043] Figure 6 It is a schematic diagram of the process of the fourth embodiment of the method for preparing a flexible capacitor of the present invention;

[0044] Figure 7 It is a structural schematic diagram of the flexible capacitor of the present invention.

[0045] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0046] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0047] It should be noted that if the embodiments of the present invention involve directional indications (such as up, down, left, right, front, back, etc.), the directional indications are only used to explain the relative position relationship, movement status, etc. between the components in a certain specific posture. If the specific posture changes, the directional indication will also change accordingly.

[0048] In addition, if there are descriptions involving "first", "second", etc. in the embodiments of the present invention, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features limited to "first" and "second" may explicitly or implicitly include at least one of the features. In addition, if "and / or" or "and / or" appears in the full text, its meaning includes three parallel solutions. Taking "A and / or B" as an example, it includes solution A, solution B, or solutions that satisfy both A and B. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in the field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0049] Reference Figure 1 , Figure 2 and Figure 7 , an embodiment of the present invention provides a flexible capacitor, the flexible capacitor comprises a flexible quasi-solid hydrogel electrolyte, a flexible anode and a flexible cathode, the flexible quasi-solid hydrogel electrolyte is sandwiched between the flexible anode and the flexible cathode;

[0050] The flexible quasi-solid hydrogel electrolyte comprises a magnesium perchlorate solution and a polymer; wherein the polymer comprises at least any one of polyacrylamide, polyvinyl alcohol, polyvinylidene fluoride, polyethylene, polypropylene, polytetrafluoroethylene, polystyrene, polymethyl methacrylate, polyhydroxyethyl methacrylate, and polyimide.

[0051] Current capacitors mainly consist of positive and negative electrodes and electrolytes. Studies have found that when placed in a low-temperature environment, the viscosity of the electrolyte increases and the ionic conductivity drops sharply, resulting in deterioration of the capacitor's performance. Therefore, the key to giving capacitors low-temperature resistance is to design an electrolyte that can maintain good ionic conductivity under low-temperature conditions.

[0052] For aqueous electrolytes (including aqueous solution electrolytes and hydrogel electrolytes), if you want to inhibit their freezing, the following two methods can be used: one is to use high-concentration salts (such as 22M KCF3SO3, saturated LiCl, etc.) to make electrolytes; the other is to use organic additives in the electrolyte (such as dimethyl sulfoxide, ethylene glycol, etc.). However, the use of high-concentration salts will greatly increase production costs, and salt precipitation will occur in low-temperature environments. In addition, high-concentration salts are not easy to use in flexible energy storage devices; and the use of organic additives may cause harm to human safety and the ecological environment due to their toxicity. On the other hand, it will cause the conductivity of the electrolyte to decrease, thereby reducing the performance of the energy storage device.

[0053] Based on the above problems, the present invention discloses the principle that magnesium perchlorate (Mg(ClO4)2) solution has low temperature resistance and high conductivity by means of physical characterization and theoretical simulation. Figure 3 The conductivity curves of magnesium perchlorate and other materials used to form electrolytes under different temperature conditions are shown. The unique advantages of magnesium perchlorate are: first, according to the Hofmeister sequence, perchlorate has a weaker ionic effect than other negative monovalent ions and can be better transferred in aqueous solution; second, a magnesium perchlorate molecule contains three ions, which is conducive to breaking the hydrogen bonds between water molecules and lowering the freezing point; in addition, magnesium ions have a higher reduction potential, so as a water-based supercapacitor, it will not be reduced to a metal form, which will lead to self-discharge and hydrogen evolution; finally, magnesium ions will not form weak base molecules with water.

[0054] Furthermore, the present invention prepares a flexible quasi-solid hydrogel electrolyte containing magnesium perchlorate salt based on the characteristic that low-concentration magnesium perchlorate solution has good low-temperature performance. Wherein, the high molecular polymer includes at least any one of polyacrylamide, polyvinyl alcohol, polyvinylidene fluoride, polyethylene, polypropylene, polytetrafluoroethylene, polystyrene, polymethyl methacrylate, polyhydroxyethyl methacrylate, and polyimide. The electrolyte used in the flexible capacitor is prepared by adding the above-mentioned high molecular polymer to the magnesium perchlorate solution. After the electrolyte is formed in the molding mold, it can eventually be solidified to form an electrolyte with a certain flexibility, and the formed flexible quasi-solid hydrogel electrolyte can be taken out of the molding mold for use. After the flexible quasi-solid hydrogel electrolyte is sandwiched between the positive and negative electrode bodies (i.e., the flexible anode and the flexible cathode), it can be formed as follows Figure 7 The flexible capacitor shown has high conductivity and excellent low temperature resistance, and can be used in flexible electronic devices. The high molecular polymer can be directly added to the magnesium perchlorate solution to dissolve, or the polymer monomer can be first added to the magnesium perchlorate solution, and then the high molecular polymer is formed by polymerization reaction, which is not limited here.

[0055] It can be seen that the flexible capacitor provided in this embodiment makes full use of the characteristics of magnesium perchlorate such as good low temperature resistance and high conductivity, and prepares the electrolyte by mixing a low-cost, low-concentration magnesium perchlorate solution with a high molecular polymer. There is no need to add organic additives that may cause harm to the human body and the environment. The flexible quasi-solid hydrogel electrolyte prepared in this way is safe and non-toxic and can maintain good mechanical and electrochemical properties under low temperature conditions. The flexible capacitor (specifically a flexible magnesium ion hybrid supercapacitor) further prepared by combining the flexible quasi-solid hydrogel electrolyte with a flexible anode and a flexible cathode also has the advantages of low temperature resistance (the normal operating temperature range is -40-25°C), high energy density (up to 103.9Wh / kg), good mechanical properties, etc., and can work stably under low temperature conditions, thereby meeting the demand for powering flexible electronic devices under low temperature climate conditions.

[0056] Correspondingly, refer to Figure 2 The embodiment of the present invention further provides a method for preparing a flexible capacitor, which is used to prepare the flexible capacitor in the above embodiment. The method for preparing the flexible capacitor comprises the following steps:

[0057] Dissolving magnesium perchlorate powder in water to prepare a magnesium perchlorate solution;

[0058] Adding a high molecular polymer to a magnesium perchlorate solution and stirring the mixture to obtain a first mixed solution; wherein the high molecular polymer comprises at least one of polyacrylamide, polyvinyl alcohol, polyvinylidene fluoride, polyethylene, polypropylene, polytetrafluoroethylene, polystyrene, polymethyl methacrylate, polyhydroxyethyl methacrylate, and polyimide;

[0059] Injecting the first mixed solution into a molding mold to form a flexible quasi-solid hydrogel electrolyte;

[0060] The flexible quasi-solid hydrogel electrolyte is sandwiched between the flexible anode and the flexible cathode.

[0061] In this embodiment, the electrolyte (ie, the first mixed solution) is prepared by directly adding the high molecular polymer into the magnesium perchlorate solution to dissolve it. This makes the production process simpler and can reduce material and labor costs accordingly.

[0062] Correspondingly, refer to Figure 1 The embodiment of the present invention further provides a method for preparing a flexible capacitor, which is used to prepare the flexible capacitor in the above embodiment. The method for preparing the flexible capacitor comprises the following steps:

[0063] Dissolving magnesium perchlorate powder in water to prepare a magnesium perchlorate solution;

[0064] Adding acrylamide, ammonium persulfate and N,N'-methylenebisacrylamide to the magnesium perchlorate solution and stirring to obtain a first mixed solution;

[0065] Injecting the first mixed solution into a molding mold, and heating the first mixed solution to cause the first mixed solution to undergo a polymerization reaction and form a flexible quasi-solid hydrogel electrolyte;

[0066] The flexible quasi-solid hydrogel electrolyte is sandwiched between the flexible anode and the flexible cathode.

[0067] This embodiment adopts the method of first adding polymer monomers to the magnesium perchlorate solution, and then forming a high molecular polymer through a polymerization reaction to prepare an electrolyte (i.e., the first mixed solution), which can make the solute in the electrolyte evenly dispersed, thereby ensuring the consistency of mechanical properties and electrochemical properties of various parts of the flexible quasi-solid hydrogel electrolyte prepared subsequently. Specifically, acrylamide is used as a polymer long chain, and N, N'-methylenebisacrylamide is used as a polymer cross-point, which is conducive to the formation of a magnesium perchlorate-polyacrylamide-water molecule ternary network structure in the solution; ammonium persulfate is used as a strong oxidant, which not only catalyzes monomer polymerization, but also stabilizes perchloric acid molecules. In this way, on the basis of having good low temperature resistance, the flexible quasi-solid hydrogel electrolyte can further have good mechanical properties under low temperature conditions.

[0068] Optionally, the concentration of the magnesium perchlorate solution is 0.5-8 mol / L.

[0069] The concentration of the magnesium perchlorate solution is preferably 4 mol / L. Specifically, the magnesium perchlorate solution can be proportioned as follows:

[0070] 26.504 g of magnesium perchlorate (Mg(ClO4)2) powder was dissolved in 20 mL of distilled water to obtain a 4 mol / L magnesium perchlorate solution.

[0071] Further, in an exemplary embodiment, the step of dissolving magnesium perchlorate powder in water to prepare a magnesium perchlorate solution comprises:

[0072] Dissolve magnesium perchlorate powder and manganese sulfate powder in water to prepare a magnesium perchlorate solution.

[0073] like Figure 4As shown, the solution obtained by mixing manganese sulfate (MnSO4) and magnesium perchlorate (Mg(ClO4)2) has a specific capacity (i.e., the amount of electricity that can be released by a battery or active material per unit mass / volume) significantly higher than that of a solution containing only magnesium perchlorate (Mg(ClO4)2). Based on this, this embodiment adopts a method of mixing magnesium perchlorate powder and manganese sulfate powder to finally prepare a flexible quasi-solid hydrogel electrolyte, which can make the power supply effect of the flexible capacitor better.

[0074] Wherein, when the concentration of magnesium perchlorate in the magnesium perchlorate solution is 4 mol / L, the concentration of manganese sulfate in the magnesium perchlorate solution is preferably 0.1 mol / L.

[0075] Optionally, refer to Figure 1 , adding acrylamide, ammonium persulfate and N,N'-methylenebisacrylamide to a magnesium perchlorate solution and stirring to obtain a first mixed solution, comprising:

[0076] Add acrylamide, ammonium persulfate and N,N'-methylenebisacrylamide to the magnesium perchlorate solution and stir for 0.25-2 hours to obtain a first mixed solution; preferably, the stirring time is 30 minutes.

[0077] Optionally, refer to Figure 1 The mass ratio of magnesium perchlorate solution, acrylamide, ammonium persulfate and N,N'-methylenebisacrylamide is 31000:3000:15:2.

[0078] Specifically, the first mixed solution can be proportioned as follows:

[0079] 26.504 g of magnesium perchlorate (Mg(ClO4)2) powder was dissolved in 20 mL of distilled water to form a 4 mol / L magnesium perchlorate solution, and 4.5 g of acrylamide (C3H5NO), 22.5 mg of ammonium persulfate ((NH4)2S2O8) and 3 mg of N,N'-methylenebisacrylamide (C7H 10 N2O2) and stirred for 30 min.

[0080] Optionally, refer to Figure 1 , the step of heating the first mixed solution comprises:

[0081] The forming mold is placed in an oven to heat the first mixed solution; wherein the heating temperature of the heating operation is 60-90° C., and the heating time of the heating operation is 2-5 hours.

[0082] The heating temperature of the heating operation in the above polymerization reaction is preferably 70° C., and the heating time is preferably 3 hours.

[0083] Further, refer to Figure 5 and Figure 6 In an exemplary embodiment, before the step of sandwiching the flexible quasi-solid hydrogel electrolyte between the flexible anode and the flexible cathode, the method comprises:

[0084] Mixing activated carbon powder, conductive carbon black (Super P) and polyvinylidene fluoride (PVDF) in N-methylpyrrolidone (NMP) and stirring to prepare a second mixed solution;

[0085] Applying the second mixed solution on the first carbon cloth, and performing a first drying operation on the first carbon cloth to form a flexible anode;

[0086] Mixing manganese dioxide (MnO2) powder, conductive carbon black (Super P) and polyvinylidene fluoride (PVDF) in N-methylpyrrolidone (NMP) and stirring to prepare a third mixed solution;

[0087] The third mixed solution is coated on the second carbon cloth, and the second carbon cloth is subjected to a second drying operation to form a flexible cathode.

[0088] Optionally, refer to Figure 5 The step of mixing activated carbon powder, conductive carbon black and polyvinylidene fluoride in N-methylpyrrolidone and stirring comprises:

[0089] Activated carbon powder, conductive carbon black and polyvinylidene fluoride are mixed in N-methylpyrrolidone at a mass ratio of 7:2:1 and stirred for 4-8 hours. Preferably, the stirring time is 6 hours.

[0090] Optionally, refer to Figure 5 , the step of performing a first drying operation on the first carbon cloth comprises:

[0091] The first carbon is placed in an environment with a temperature of 60-120°C for a first drying operation, wherein the drying time of the first drying operation is 6-12 hours. Preferably, the environment temperature for the first drying operation is 80°C, and the drying time of the first drying operation is 8 hours.

[0092] Optionally, refer to Figure 6 The step of mixing manganese dioxide powder, conductive carbon black and polyvinylidene fluoride in N-methylpyrrolidone and stirring comprises:

[0093] Manganese dioxide powder, conductive carbon black and polyvinylidene fluoride are mixed in N-methylpyrrolidone at a mass ratio of 7:2:1 and stirred for 4-8 hours. Preferably, the stirring time is 6 hours.

[0094] Optionally, refer to Figure 6 The step of performing a second drying operation on the second carbon cloth comprises:

[0095] The second carbon is placed in an environment with a temperature of 60-120°C for a second drying operation, wherein the drying time of the second drying operation is 6-12 hours. Preferably, the environment temperature for the second drying operation is 80°C, and the drying time of the second drying operation is 8 hours.

[0096] In order to better cooperate with the flexible quasi-solid hydrogel electrolyte having a ternary network structure of magnesium perchlorate-polyacrylamide-water molecules, the present embodiment makes corresponding adjustments to the composition and preparation method of the existing flexible anode and flexible cathode (the traditional flexible anode is made of zinc, and the traditional flexible cathode is made of activated carbon). Specifically, activated carbon powder, conductive carbon black (Super P), polyvinylidene fluoride (PVDF) and N-methylpyrrolidone (NMP) are mixed and stirred by a magnetic stirrer to prepare a second mixed solution; manganese dioxide (MnO2) powder, conductive carbon black (Super P), polyvinylidene fluoride (PVDF) and N-methylpyrrolidone (NMP) are mixed and stirred by a magnetic stirrer to prepare a third mixed solution.

[0097] The mass loading of the active material of the flexible anode prepared by the above method is about 4.5-6 mg / cm 2 The mass loading of manganese dioxide in the flexible cathode prepared by the above method is about 1.5-2 mg / cm 2 .

[0098] Further, refer to Figure 6 In an exemplary embodiment, before the step of mixing manganese dioxide powder, conductive carbon black and polyvinylidene fluoride in N-methylpyrrolidone and stirring to prepare a third mixed solution, the step includes:

[0099] Dissolving potassium permanganate and manganese sulfate powder in water and stirring to prepare a fourth mixed solution;

[0100] injecting the fourth mixed solution into a polytetrafluoroethylene reactor and performing a hydrothermal reaction to obtain a manganese dioxide precipitate;

[0101] The manganese dioxide precipitate is dried to obtain the manganese dioxide powder.

[0102] Optionally, refer to Figure 6 In the step of dissolving potassium permanganate and manganese sulfate powder in water and stirring to prepare a fourth mixed solution, the stirring time may be 0.25-1 hour, preferably 0.5 hour.

[0103] Optionally, refer to Figure 6 , the mass ratio of potassium permanganate and manganese sulfate powder is 10:1.27; the concentration of the fourth mixed solution is 3.5-3.6 mg / mL.

[0104] Optionally, refer to Figure 6 The reaction temperature of the hydrothermal reaction is 100-130°C, and the reaction time of the hydrothermal reaction is 10-14 hours. Preferably, the reaction temperature of the hydrothermal reaction is 120°C, and the reaction time of the hydrothermal reaction is 12 hours.

[0105] Optionally, refer to Figure 6 The step of drying the manganese dioxide precipitate comprises:

[0106] The manganese dioxide precipitate is placed in a vacuum environment for drying, wherein the drying temperature of the drying operation is 60-90°C, and the drying time of the drying operation is 6-10 hours. Preferably, the drying temperature of the drying operation is 80°C, and the drying time of the drying operation is 8 hours.

[0107] This embodiment discloses a method for preparing manganese dioxide (MnO2) powder. Specifically, the fourth mixed solution can be proportioned and subsequently processed as follows:

[0108] 0.2528 g of potassium permanganate (KMnO4) powder and 0.0321 g of manganese sulfate (MnSO4) powder were dissolved in 80 mL of water and stirred for 30 minutes. The prepared fourth mixed solution was then transferred to a 100 mL polytetrafluoroethylene reactor liner, and a sufficient amount of distilled water was injected into the polytetrafluoroethylene reactor liner, so that the fourth mixed solution could produce a hydrothermal reaction and obtain a manganese dioxide precipitate.

[0109] It should be noted that other contents of the flexible capacitor and the preparation method thereof disclosed in the present invention can be found in the prior art and will not be described in detail here.

[0110] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A flexible capacitor for powering flexible electronic devices under low temperature conditions, characterized in that: The flexible capacitor comprises a flexible quasi-solid hydrogel electrolyte, a flexible anode and a flexible cathode, wherein the flexible quasi-solid hydrogel electrolyte is sandwiched between the flexible anode and the flexible cathode; The flexible quasi-solid hydrogel electrolyte comprises a magnesium perchlorate solution and a polymer; wherein the polymer comprises at least any one of polyacrylamide, polyvinyl alcohol, polyvinylidene fluoride, polyethylene, polypropylene, polytetrafluoroethylene, polystyrene, polymethyl methacrylate, polyhydroxyethyl methacrylate, and polyimide; the magnesium perchlorate solution comprises magnesium perchlorate with a concentration of 4 mol / L and manganese sulfate with a concentration of 0.1 mol / L, the magnesium perchlorate molecules in the magnesium perchlorate solution contain three ions for breaking the hydrogen bonding between water molecules and lowering the freezing point, the magnesium ions in the magnesium perchlorate solution do not form weak base molecules with water and will not be reduced to a metal form to cause self-discharge hydrogen evolution; The flexible anode comprises activated carbon, and the flexible cathode comprises manganese dioxide.

2. A method for preparing a flexible capacitor, used to prepare the flexible capacitor as claimed in claim 1, characterized in that: The method for preparing the flexible capacitor comprises the following steps: Dissolving magnesium perchlorate powder and manganese sulfate powder in water to prepare a magnesium perchlorate solution; Adding a high molecular polymer to the magnesium perchlorate solution and stirring the mixture to obtain a first mixed solution; wherein the high molecular polymer comprises at least one of polyacrylamide, polyvinyl alcohol, polyvinylidene fluoride, polyethylene, polyacrylic acid, polystyrene, polymethyl methacrylate, polyhydroxyethyl methacrylate, and polyimide; Injecting the first mixed solution into a molding mold to form the flexible quasi-solid hydrogel electrolyte; The flexible quasi-solid hydrogel electrolyte is sandwiched between the flexible anode and the flexible cathode.

3. A method for preparing a flexible capacitor, used to prepare the flexible capacitor as claimed in claim 1, characterized in that: The method for preparing the flexible capacitor comprises the following steps: Dissolving magnesium perchlorate powder and manganese sulfate powder in water to prepare a magnesium perchlorate solution; Adding acrylamide, ammonium persulfate and N,N'-methylenebisacrylamide to the magnesium perchlorate solution and stirring to obtain a first mixed solution; Injecting the first mixed solution into a molding mold, and heating the first mixed solution to cause the first mixed solution to undergo a polymerization reaction and form the flexible quasi-solid hydrogel electrolyte; The flexible quasi-solid hydrogel electrolyte is sandwiched between the flexible anode and the flexible cathode.

4. The method for preparing a flexible capacitor according to claim 3, characterized in that: The step of adding acrylamide, ammonium persulfate and N,N'-methylenebisacrylamide to the magnesium perchlorate solution and stirring to obtain the first mixed solution comprises: Add acrylamide, ammonium persulfate and N,N'-methylenebisacrylamide to the magnesium perchlorate solution and stir for 0.25-2 hours to obtain the first mixed solution.

5. The method for preparing a flexible capacitor according to claim 3, characterized in that: The mass ratio of the magnesium perchlorate solution, the acrylamide, the ammonium persulfate and the N,N'-methylenebisacrylamide is 31000:3000:15:

2.

6. The method for preparing a flexible capacitor according to claim 3, characterized in that: The step of heating the first mixed solution comprises: The forming mold is placed in an oven to perform the heating operation on the first mixed solution; wherein the heating temperature of the heating operation is 60-90° C., and the heating time of the heating operation is 2-5 hours.

7. The method for preparing a flexible capacitor according to claim 2 or claim 3, characterized in that: Before the step of sandwiching the flexible quasi-solid hydrogel electrolyte between the flexible anode and the flexible cathode, the method comprises: Mixing activated carbon powder, conductive carbon black and polyvinylidene fluoride in N-methylpyrrolidone and stirring to prepare a second mixed solution; Applying the second mixed solution on a first carbon cloth, and performing a first drying operation on the first carbon cloth to form the flexible anode; Mixing manganese dioxide powder, conductive carbon black and polyvinylidene fluoride in N-methylpyrrolidone and stirring to prepare a third mixed solution; The third mixed solution is coated on a second carbon cloth, and a second drying operation is performed on the second carbon cloth to form the flexible cathode.

8. The method for preparing a flexible capacitor according to claim 7, characterized in that: Before the step of mixing manganese dioxide powder, conductive carbon black and polyvinylidene fluoride in N-methylpyrrolidone and stirring to prepare a third mixed solution, the method comprises: Dissolving potassium permanganate and manganese sulfate powder in water and stirring to prepare a fourth mixed solution; injecting the fourth mixed solution into a polytetrafluoroethylene reactor and performing a hydrothermal reaction to obtain a manganese dioxide precipitate; The manganese dioxide precipitate is dried to obtain the manganese dioxide powder.

Citation Information

Patent Citations

  • Lithium battery flexible negative electrode material for wearable electronic equipment and preparation method

    CN111180715A

  • Low-temperature aqueous ion battery electrolyte and application thereof in aqueous ion battery

    CN114695974A

  • Electrochemical element

    JP1999204116A

  • Solid electrolyte, electrochemical element containing the same, and forming method of solid electrolyte

    JP2006196464A

  • Method for producing organic inorganic composite gel coating film

    JP2012236156A

Cited By

  • Low-temperature-resistant flexible stretchable all-polyampholyte hydrogel supercapacitor and preparation method thereof

    CN116825550A