Preparation method and application of high entropy perovskite fluoride electrode material
Preparing high-entropy perovskite fluoride nanoparticles through a solvothermal reaction method solves the problems of high cost and strict parameter control of high-energy ball milling, achieving efficient and low-cost preparation of high-entropy perovskite fluoride electrode materials with excellent electrochemical properties and potential supercapacitor applications.
Patent Information
- Application Number
- CN202210873033.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-22
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-07-22
AI Technical Summary
Existing preparation methods for high-entropy perovskite fluoride electrode materials mainly rely on high-energy ball milling, resulting in high preparation costs and strict parameter control, which limits the large-scale application of the materials.
Using the solvothermal reaction method, soluble divalent metal salts, fluoride ion salts and polyvinylpyrrolidone are stirred and ultrasonicated in ethylene glycol to form a uniform mixed solution. After centrifugation, drying and grinding, high-entropy perovskite fluorine is obtained. Chemical nanoparticles are mixed with conductive agents and adhesives for the preparation of supercapacitor cathode materials.
The low-cost and simple preparation of high-entropy perovskite fluoride electrode materials is achieved. It has high crystallinity and high purity, improves specific capacitance performance, and has potential application value in supercapacitors.
Smart Images

Figure CN115116765B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of supercapacitor electrode materials, and in particular relates to a preparation method and application of a high-entropy perovskite fluoride electrode material. Background Art
[0002] High-entropy nanomaterials have great potential in many aspects, but these potentials have not yet been realized due to the limitations of high-temperature synthesis routes and limited understanding of high-entropy materials. Therefore, exploring new preparation methods for high-entropy nanomaterials is of great significance for conducting research in new directions.
[0003] Among various types of high-entropy nanomaterials, high-entropy perovskite fluorides have excellent thermodynamic stability, cocktail effect and multi-metal ion combination, which make this type of material have excellent electrochemical properties and show great advantages in the field of energy storage and conversion. However, there are very few reports on perovskite fluorides, and the relevant synthesis methods are limited to high-energy ball milling (JOURNAL OF THE AMERICAN CHEMICAL SOCIETY 142.10 (2020) 4550-4554.), and the high-energy ball milling method is extremely dependent on expensive equipment such as high-energy ball mills, which also leads to the high cost of preparing such materials. The relevant parameters are extremely strict, which will greatly hinder the large-scale application of such materials. Therefore, exploring simple, practical and universal methods for preparing high-entropy perovskite fluorides will be of great significance to the research work in the field of high-entropy perovskite fluorides. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a preparation method and application of a high entropy perovskite fluoride electrode material to solve the technical problem that the current synthesis method of perovskite fluoride is limited to high-energy ball milling, the preparation cost is very high, the related parameter control is extremely strict and cannot be applied on a large scale.
[0005] A method for preparing a high entropy perovskite fluoride electrode material comprises the following steps, and the following steps are performed in sequence:
[0006] Step 1: dissolving a soluble divalent metal salt, a fluoride ion salt and polyvinylpyrrolidone (PVP) in an ethylene glycol solvent, stirring and ultrasonicating until a uniform mixed solution is formed;
[0007] Step 2: subjecting the mixed solution of step 1 to a solvothermal reaction in a reactor, and then sequentially subjecting the mixed solution to centrifugation, drying, and grinding to obtain high-entropy perovskite fluoride nanoparticles, which are high-entropy perovskite fluoride electrode materials.
[0008] The soluble divalent metal salt is at least one of zinc chloride, manganese chloride, cobalt chloride, nickel chloride, magnesium chloride, ferrous chloride, and aluminum chloride. The molar ratio of water to the divalent metal salt in the soluble divalent metal salt is 1:1.5, and the total amount of the metal salt is 2mmol to 3mmol.
[0009] The fluorine-containing ion salt is KF or LiF, and the usage amount of the fluorine-containing ion salt is 5 mmol to 6 mmol.
[0010] The usage amount of the polyvinyl pyrrolidone PVP is 0.2g-0.3g.
[0011] The usage amount of the ethylene glycol solvent is 30mL to 40mL.
[0012] The setting conditions of the reactor in step 2 are 150° C. to 180° C., and the reaction time is 5 h to 6 h.
[0013] An application of a high entropy perovskite fluoride electrode material is applied to the preparation of a positive electrode material for a supercapacitor, and the preparation method thereof is as follows:
[0014] The high entropy perovskite fluoride electrode material, the conductive agent Super P conductive carbon black and the adhesive polyvinylidene fluoride are mixed, and N,N'-dimethylacetamide is added and ground to obtain a homogeneous black slurry. The black slurry is evenly spread on the current collector foam nickel, and after drying and pressing, a high entropy perovskite fluoride positive electrode material for supercapacitors is obtained.
[0015] The high entropy perovskite fluoride electrode material, the conductive agent Super P conductive carbon black and the adhesive polyvinylidene fluoride are mixed in a mass ratio of 8:1:1.
[0016] The amount of N,N'-dimethylacetamide added is 3 mL to 8 mL.
[0017] Through the above design scheme, the present invention can bring the following beneficial effects:
[0018] The present invention lays a foundation for the application of high-entropy perovskite fluoride. The prepared electrode material is high-entropy perovskite fluoride nanoparticles. Compared with the high-energy ball milling method, this method has the advantages of being simpler and having lower production costs. The prepared high-entropy perovskite fluoride has excellent physical phase characteristics of high crystallinity and high purity. The material prepared by the method of the present invention has high specific capacitance and has potential application value in aspects such as supercapacitor positive electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The present invention is further described below with reference to the accompanying drawings and specific embodiments:
[0020] Figure 1It is K(ZnMnCoNiMg) prepared in Example 1 of the present invention 1 / 5 X-ray diffraction pattern of F3;
[0021] Figure 2 It is K(ZnMnCoNiMg) prepared in Example 1 of the present invention 1 / 5 Scanning electron micrograph of F3;
[0022] Figure 3 It is K(ZnMnCoNiMg) prepared in Example 1 of the present invention 1 / 5 X-ray photoelectron spectrum of F3;
[0023] Figure 4 It is K(ZnMnCoNiMg) prepared in Example 1 of the present invention 1 / 5 A partial enlargement of the X-ray photoelectron spectrum of F3;
[0024] Figure 5 It is K(ZnMnCoNiMg) prepared in Example 1 of the present invention 1 / 5 A partial enlargement of the X-ray photoelectron spectrum of F3;
[0025] Figure 6 It is K(ZnMnCoNiMg) prepared in Example 1 of the present invention 1 / 5 A partial enlargement of the X-ray photoelectron spectrum of F3;
[0026] Figure 7 It is K(ZnMnCoNiMg) prepared in Example 1 of the present invention 1 / 5 A partial enlargement of the X-ray photoelectron spectrum of F3;
[0027] Figure 8 It is K(ZnMnCoNiMg) prepared in Example 1 of the present invention 1 / 5 A partial enlargement of the X-ray photoelectron spectrum of F3;
[0028] Fig. 9 It is K(ZnMnCoNiMg) prepared in Example 1 of the present invention 1 / 5 A partial enlargement of the X-ray photoelectron spectrum of F3;
[0029] Fig.10 It is K(ZnMnCoNiMg) prepared in Example 1 of the present invention 1 / 5 A partial enlargement of the X-ray photoelectron spectrum of F3;
[0030] Fig.11 It is K(ZnMnCoNiMgFe) prepared in Example 2 of the present invention 1 / 6 X-ray diffraction pattern of F3;
[0031] Fig.12 It is K(ZnMnCoNiMgFe) prepared in Example 2 of the present invention 1 / 6 Scanning electron micrograph of F3;
[0032] Fig.13 It is K(ZnMnCoNiMgFe) prepared in Example 2 of the present invention 1 / 6 X-ray photoelectron spectrum of F3;
[0033] Fig.14 It is K(ZnMnCoNiMgFe) prepared in Example 2 of the present invention 1 / 6 A partial enlargement of the X-ray photoelectron spectrum of F3;
[0034] Fig.15 It is K(ZnMnCoNiMgFe) prepared in Example 2 of the present invention 1 / 6 A partial enlargement of the X-ray photoelectron spectrum of F3;
[0035] Fig.16 It is K(ZnMnCoNiMgFe) prepared in Example 2 of the present invention 1 / 6 A partial enlargement of the X-ray photoelectron spectrum of F3;
[0036] Fig.17 It is K(ZnMnCoNiMgFe) prepared in Example 2 of the present invention 1 / 6 A partial enlargement of the X-ray photoelectron spectrum of F3;
[0037] Fig.18 It is K(ZnMnCoNiMgFe) prepared in Example 2 of the present invention 1 / 6 A partial enlargement of the X-ray photoelectron spectrum of F3;
[0038] Fig.19 It is K(ZnMnCoNiMgFe) prepared in Example 2 of the present invention 1 / 6 A partial enlargement of the X-ray photoelectron spectrum of F3;
[0039] Fig. 20 It is K(ZnMnCoNiMgFe) prepared in Example 2 of the present invention 1 / 6 A partial enlargement of the X-ray photoelectron spectrum of F3;
[0040] Fig.21 It is K(ZnMnCoNiMgFe) prepared in Example 2 of the present invention 1 / 6 A partial enlargement of the X-ray photoelectron spectrum of F3;
[0041] Fig. 22It is K(ZnMnCoNiMgFe) prepared in Example 2 of the present invention 1 / 6 Constant current charge and discharge curve of F3;
[0042] Fig.23 It is K(ZnMnCoNiMgFeAl) prepared in Example 3 of the present invention 1 / 7 X-ray diffraction pattern of F3;
[0043] Fig.24 It is K(ZnMnCoNiMgFeAl) prepared in Example 3 of the present invention 1 / 7 Scanning electron micrograph of F3.
[0044] Fig.25 It is K(ZnMnCoNiMgFeAl) prepared in Example 3 of the present invention 1 / 7 X-ray photoelectron spectrum of F3;
[0045] Fig.26 It is K(ZnMnCoNiMgFeAl) prepared in Example 3 of the present invention 1 / 7 A partial enlargement of the X-ray photoelectron spectrum of F3;
[0046] Fig. 27 It is K(ZnMnCoNiMgFeAl) prepared in Example 3 of the present invention 1 / 7 A partial enlargement of the X-ray photoelectron spectrum of F3;
[0047] Fig.28 It is K(ZnMnCoNiMgFeAl) prepared in Example 3 of the present invention 1 / 7 A partial enlargement of the X-ray photoelectron spectrum of F3;
[0048] Fig.29 It is K(ZnMnCoNiMgFeAl) prepared in Example 3 of the present invention 1 / 7 A partial enlargement of the X-ray photoelectron spectrum of F3;
[0049] Fig.30 It is K(ZnMnCoNiMgFeAl) prepared in Example 3 of the present invention 1 / 7 A partial enlargement of the X-ray photoelectron spectrum of F3;
[0050] Fig.31 It is K(ZnMnCoNiMgFeAl) prepared in Example 3 of the present invention 1 / 7 A partial enlargement of the X-ray photoelectron spectrum of F3;
[0051] Fig.32 It is K(ZnMnCoNiMgFeAl) prepared in Example 3 of the present invention1 / 7 A partial enlargement of the X-ray photoelectron spectrum of F3;
[0052] Fig.33 It is K(ZnMnCoNiMgFeAl) prepared in Example 3 of the present invention 1 / 7 A partial enlargement of the X-ray photoelectron spectrum of F3;
[0053] Fig.34 It is K(ZnMnCoNiMgFeAl) prepared in Example 3 of the present invention 1 / 7 A partial enlargement of the X-ray photoelectron spectrum of F3;
[0054] Fig.35 It is K(ZnMnCoNiMgFeAl) prepared in Example 3 of the present invention 1 / 7 Constant current charge and discharge curve of F3. DETAILED DESCRIPTION
[0055] A method for preparing a high entropy perovskite fluoride electrode material comprises the following steps:
[0056] (1) dissolving a soluble divalent metal salt, a fluoride ion salt and PVP in a solvent, stirring and ultrasonicating until a uniform mixed solution is formed;
[0057] (2) After subjecting the mixed solution of step (1) to a solvothermal reaction, the mixed solution is sequentially centrifuged, dried, and ground to obtain a high entropy perovskite fluoride electrode material.
[0058] In the present invention, the soluble divalent metal salt is selected from zinc chloride, manganese chloride, cobalt chloride, nickel chloride, magnesium chloride, ferrous chloride, aluminum chloride and the like.
[0059] In the present invention, the molar ratio of all soluble divalent metal salts is 1:1.5, and the total amount of the metal salts is 2 mmol to 3 mmol.
[0060] In the present invention, the fluorine-containing ion salt is preferably KF or LiF, more preferably KF.
[0061] In the present invention, the usage amount of the fluorine-containing ion salt is 5 mmol to 6 mmol.
[0062] In the present invention, the PVP is used in an amount of 0.2 g to 0.3 g.
[0063] In the present invention, the solvent is ethylene glycol.
[0064] In the present invention, the amount of ethylene glycol used is 30 mL to 40 mL.
[0065] In the present invention, the reaction kettle required for the solvothermal reaction is 40 or 50 mL.
[0066] In the present invention, the solvent thermal reaction conditions are: placing in a reaction kettle, reacting at 150° C. to 180° C. for 5 h to 6 h.
[0067] The present invention also protects a high entropy perovskite fluoride positive electrode material prepared using the high entropy perovskite fluoride electrode material.
[0068] Preferably, the method for preparing the high entropy perovskite fluoride positive electrode material comprises the following steps:
[0069] The high entropy perovskite fluoride electrode material, the conductive agent Super P conductive carbon black and the adhesive polyvinylidene fluoride are mixed, N,N'-dimethylacetamide is added and ground to obtain a homogeneous black slurry, the black slurry is evenly spread on the current collector nickel foam, and the high entropy perovskite fluoride positive electrode material is obtained after drying and pressing;
[0070] Among them, the mass ratio of high entropy perovskite fluoride electrode material, conductive agent Super P conductive carbon black and adhesive polyvinylidene fluoride is 8:1:1; the added amount of N,N'-dimethylacetamide is 3mL to 8mL.
[0071] The obtained high entropy perovskite fluoride positive electrode material is used to prepare supercapacitor positive electrode material.
[0072] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.
[0073] Example 1
[0074] Dissolve equal amounts of ZnCl2, MnCl2·4H2O, CoCl2·6H2O, NiCl2·6H2O, MgCl2·6H2O (2mmol in total), 5mmol of KF and 0.20g of PVP in 30mL of ethylene glycol, stir, and ultrasonicate to form a uniform solution. The uniform solution was placed in a 40mL reactor for a 160°C, 5-hour solvothermal reaction. The resulting precipitate was centrifuged, dried, and ground to obtain K(ZnMnCoNiMg) 1 / 5 F3.
[0075] Figure 1 K(ZnMnCoNiMg) prepared in Example 1 1 / 5 X-ray diffraction pattern of F3. It can be seen from the figure that all standard peaks are completely aligned with the standard card, proving that a single solid solution structure has been formed, proving that this method has been used to synthesize a five-element high-entropy perovskite fluoride K (ZnMnCoNiMg) with high crystallinity and pure phase. 1 / 5 F3;
[0076] Figure 2 K(ZnMnCoNiMg) prepared in Example 1 1 / 5 Scanning electron microscope image of F3, from which we can see that the five-element high entropy perovskite fluoride K (ZnMnCoNiMg) 1 / 5 F3 is a material composed of nanoparticles;
[0077] Figures 3 to 10 K(ZnMnCoNiMg) prepared in Example 1 1 / 5 The X-ray photoelectron spectrum of F3 shows that the sample has spectral peaks of seven elements, namely K, Zn, Mn, Co, Ni, Mg, and F, proving that the sample contains these seven elements and forms a multi-element high-entropy structure.
[0078] Example 2
[0079] Dissolve equal amounts of ZnCl2, MnCl2·4H2O, CoCl2·6H2O, NiCl2·6H2O, MgCl2·6H2O, FeCl2·4H2O (2.5 mmol in total), 5.5 mmol of KF and 0.25 g of PVP in 36 mL of ethylene glycol, stir, and sonicate to form a uniform solution. The uniform solution was placed in a 50 mL reactor for a 6-hour solvothermal reaction at 170°C. The resulting precipitate was centrifuged, dried, and ground to obtain K(ZnMnCoNiMgFe) 1 / 6 F3.
[0080] Fig.11 K(ZnMnCoNiMgFe) prepared in Example 2 1 / 6 X-ray diffraction pattern of F3. It can be seen from the figure that all standard peaks are completely aligned with the standard card, proving that a single solid solution structure has been formed, proving that this method has been used to synthesize a high-crystallinity and pure-phase hexavalent high-entropy perovskite fluoride K (ZnMnCoNiMgFe) 1 / 6 F3;
[0081] Fig.12 K(ZnMnCoNiMgFe) prepared in Example 2 1 / 6 Scanning electron microscope image of F3, from which we can see that the hexavalent high entropy perovskite fluoride K (ZnMnCoNiMgFe) 1 / 6 F3 is a material composed of nanoparticles;
[0082] Figures 13 to 21 K(ZnMnCoNiMgFe) prepared in Example 2 1 / 6The X-ray photoelectron spectrum of F3 shows that the sample has spectral peaks of eight elements, namely K, Zn, Mn, Co, Ni, Mg, Fe, and F, proving that the sample contains these eight elements and forms a multi-element high-entropy structure.
[0083] Fig. 22 K(ZnMnCoNiMgFe) prepared in Example 2 1 / 6 The constant current charge and discharge curve of F3 shows that through calculation, the material has a specific capacitance of 133F / g at a current density of 1A / g, indicating that it has high capacitor performance and also proves that this material has good electrochemical properties.
[0084] Example 3
[0085] Dissolve equal amounts of ZnCl2, MnCl2·4H2O, CoCl2·6H2O, NiCl2·6H2O, MgCl2·6H2O, FeCl2·4H2O, AlCl3 (3 mmol in total), 6 mmol of KF and 0.3 g of PVP in 40 mL of ethylene glycol, stir, and sonicate to form a uniform solution. The uniform solution was placed in a 50 mL reactor for a 6-hour solvothermal reaction at 180°C. The resulting precipitate was centrifuged, dried, and ground to obtain K(ZnMnCoNiMgFeAl) 1 / 7 F3.
[0086] Fig.23 K(ZnMnCoNiMgFeAl) prepared in Example 3 1 / 7 X-ray diffraction pattern of F3. It can be seen from the figure that all standard peaks are completely aligned with the standard card, proving that a single solid solution structure has been formed, proving that this method has been used to synthesize a seven-element high-entropy perovskite fluoride K (ZnMnCoNiMgFeAl) with high crystallinity and pure phase. 1 / 7 F3;
[0087] Fig.24 K(ZnMnCoNiMgFeAl) prepared in Example 3 1 / 7 Scanning electron microscope image of F3, from which we can see that the seven-element high entropy perovskite fluoride K (ZnMnCoNiMgFeAl) 1 / 7 F3 is a material composed of nanoparticles;
[0088] Figures 25 to 34 K(ZnMnCoNiMgFeAl) prepared in Example 3 1 / 7 The X-ray photoelectron spectrum of F3 shows that the sample has spectral peaks of nine elements, namely K, Zn, Mn, Co, Ni, Mg, Fe, Al, and F, proving that the sample contains these nine elements and forms a multi-element high-entropy structure.
[0089] Fig.35 K(ZnMnCoNiMgFeAl) prepared in Example 3 1 / 7 Constant current charge and discharge curve of F3. Through calculation, it can be known that the material has a specific capacitance of 210F / g at a current density of 1A / g, indicating that it has high capacitor performance and also proves that this material has good electrochemical properties.
Claims
1. A method for preparing a high entropy perovskite fluoride electrode material, characterized in that: The process includes the following steps, which are performed in sequence: Step 1: dissolving a soluble divalent metal salt, a fluoride ion salt and polyvinylpyrrolidone (PVP) in an ethylene glycol solvent, stirring, and ultrasonicating to form a mixed solution; The soluble divalent metal salt is at least one of zinc chloride, manganese chloride, cobalt chloride, nickel chloride, magnesium chloride, ferrous chloride, and aluminum chloride, the molar ratio of water to the divalent metal salt in the soluble divalent metal salt is 1:1.5, and the total amount of the metal salt is 2 mmol to 3 mmol; The fluorine-containing ion salt is KF or LiF, and the amount of the fluorine-containing ion salt used is 5 mmol to 6 mmol; The usage amount of the polyvinyl pyrrolidone PVP is 0.2g to 0.3g; Step 2: subjecting the mixed solution of step 1 to a solvothermal reaction in a reactor, and then sequentially subjecting the mixed solution to centrifugation, drying, and grinding to obtain high-entropy perovskite fluoride nanoparticles, which are high-entropy perovskite fluoride electrode materials; The setting conditions of the reactor are 150° C. to 180° C., and the reaction time is 5 h to 6 h.
2. The method for preparing a high entropy perovskite fluoride electrode material according to claim 1, characterized in that: The usage amount of the ethylene glycol solvent is 30mL to 40mL.
3. An application of a high entropy perovskite fluoride electrode material, characterized in that: Preparation of positive electrode materials for supercapacitors.
Citation Information
Patent Citations
Preparation method of lithium ion battery electrode material
CN108461707A
NiO woolen yarn spherical electrode material and preparation method and application thereof
CN114188163A