Carbon-interval nano-AlF3 catalyst rich in unsaturated coordination prepared by silicon-aluminum molecular sieve, preparation method and application thereof

The carbon-spaced nano-AlF3 catalyst prepared with silica-aluminum molecular sieve as the precursor solves the problem of carbon deposition and sintering of the aluminum fluoride catalyst during the reaction, improves the catalytic activity and stability, and achieves efficient fluorine-containing alkanes removal HF reaction.

CN115138378BActive Publication Date: 2024-10-01ZHEJIANG UNIV OF TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202210683849.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-17
Publication Date
2024-10-01
Estimated Expiration
2042-06-17

AI Technical Summary

Technical Problem

Existing aluminum fluoride catalysts are prone to carbon deposition and sintering during the cracking and dehydrogenation reactions of fluorinated alkanes, leading to catalyst deactivation, and the low specific surface area of ​​metal fluoride limits catalytic activity.

Method used

A carbon-spaced, unsaturated coordination-rich nano-AlF3 catalyst prepared with silicon-aluminum molecular sieves as a precursor is used, and is calcined in an N2 or argon atmosphere and fluorinated under the action of a fluorine source to form a catalyst with high catalytic activity and stability. catalyst.

Benefits of technology

The activity and stability of the catalyst are improved. The catalytic activity is 20-25% higher than that of ordinary AlF3 catalysts, and it maintains 60% activity during long-term reactions, extending the service life of the catalyst and reducing sintering deactivation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115138378B_ABST
    Figure CN115138378B_ABST
Patent Text Reader

Abstract

The present invention discloses a carbon-interval nano AlF3 catalyst rich in unsaturated coordination prepared by using silicon-aluminum molecular sieve, and a preparation method and application thereof. The preparation of the catalyst comprises the following process: using silicon-aluminum molecular sieve containing an organic template as a precursor, calcining the silicon-aluminum molecular sieve in an N2 atmosphere or an argon atmosphere, retaining the organic template in the form of carbon intervals in the pores of the silicon-aluminum molecular sieve to obtain a catalyst precursor, and then fluorinating the calcined catalyst precursor under the action of a fluorine source to obtain a carbon-interval nano AlF3 catalyst rich in unsaturated coordination. The carbon-interval nano AlF3 catalyst obtained by the present invention has excellent catalytic activity and selectivity in the reaction of preparing fluorinated olefins by removing HF from fluorinated alkanes in the gas phase, and the catalyst is not easily deactivated during the reaction, thereby increasing the service life of the catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of heterogeneous thermal catalysts and specifically relates to a carbon-interval-rich unsaturated coordination nano-AlF prepared using a silicon-aluminum molecular sieve as a precursor. 3 Catalyst, preparation method and application thereof. Background Art

[0002] Hydrofluorocarbons (HFCs) are a class of non-CO2 gases with long atmospheric lifetimes and strong greenhouse effects. 2 Greenhouse gas. Fluorinated alkanes can be converted into fluorinated olefins (HFOs) with less environmental impact through resource conversion, and can be widely used in refrigerants, foaming agents, aerosols and other fields, with high economic benefits. Therefore, converting fluorinated alkanes into fluorinated intermediates and fluorinated olefins with economic value can achieve the effective utilization of fluorine resources.

[0003] In the prior art, the most commonly used catalyst for the reaction of fluorinated alkanes to produce fluorinated olefins by dehydrofluorination of fluorinated alkanes is aluminum fluoride (AlF 3 ), but the low specific surface area of ​​metal fluorides limits the activity of the catalyst. 3 ) Catalysts are prone to carbon deposition and sintering during the catalytic reaction, which can lead to catalyst deactivation. Therefore, it is of great significance to develop a highly stable catalyst.

[0004] Silica-alumina molecular sieves have abundant acid sites, good hydrothermal stability and thermal stability. In the fields of petrochemicals and fine chemicals, many reactions use acid centers as active sites. The different acidity of molecular sieves can directly affect the activity and selectivity of acid-catalyzed reactions. Since the silicon-aluminum ratio of silica-alumina molecular sieves can be adjusted in a wide range (Si / Al ratio is 1 to all silicon), the acid properties of silica-alumina molecular sieves are easier to control. At the same time, silica-alumina molecular sieves have good thermal stability and hydrothermal stability and can be prepared in batches, so they have good application prospects in the field of industrial catalysis. Summary of the invention

[0005] In view of the conventional AlF 3 The problem of catalyst deactivation caused by carbon deposition and sintering in the catalytic dehydrofluorination reaction of fluorinated alkanes is that the present invention aims to provide a carbon-interval nano AlF3 catalyst rich in unsaturated coordination prepared by using silicon-aluminum molecular sieve as a precursor, and its preparation method and application. 3 The preparation method of the catalyst has the characteristics of simple preparation and easy control of the silicon-aluminum ratio. The catalyst synthesized by the invention has high catalytic activity and stability in the reaction of removing HF from fluorinated alkanes (HFCs) to prepare fluorinated olefins (HFOs), and has high practicality.

[0006] The technical solution adopted by the present invention is as follows:

[0007] The method of using silicon aluminum molecular sieve as a precursor to prepare carbon-interval-rich unsaturated coordination nano AlF 3 The method for preparing the catalyst is characterized by comprising the following steps: using a silicon-aluminum molecular sieve containing an organic template as a precursor, 2 The silicon-aluminum molecular sieve is calcined in an atmosphere or an argon atmosphere, and the organic template is retained in the pores of the silicon-aluminum molecular sieve in the form of a carbon interval to obtain a catalyst precursor, and then the calcined catalyst precursor is fluorinated under the action of a fluorine source to obtain a carbon-interval-rich unsaturated coordination nano-AlF 3 catalyst.

[0008] The method of using silicon aluminum molecular sieve as a precursor to prepare carbon-interval-rich unsaturated coordination nano AlF 3 The method is characterized in that the organic template is triethylamine, tetramethylammonium hydroxide or hexamethylenediamine, and the preparation method of the silica-alumina molecular sieve containing the organic template is to mix the aluminum source, the organic template, the silicon source and deionized water, stir them thoroughly to form a uniform gel, and after the gel is crystallized at 160-200°C for 40-60h, the product is cooled to room temperature, the product is filtered, washed with deionized water, and dried at 100-110°C to obtain the silica-alumina molecular sieve containing the organic template; the aluminum source of the raw material for preparing the silica-alumina molecular sieve is Al 2 O 3 The molar ratio of the organic template to the organic template is 1:0.7 to 1. That is, the silica-alumina molecular sieve raw materials containing the organic template used in the present invention have not been subjected to calcination treatment to remove the template.

[0009] The method for preparing a carbon-intervaled unsaturated coordinated nano AlF3 catalyst using a silicon-aluminum molecular sieve as a precursor is characterized in that the silicon-aluminum molecular sieve is a low-silicon molecular sieve with a Si / Al molar ratio of 1 to 1.5, a Y-type molecular sieve with a Si / Al molar ratio of 1.5 to 3.0, or a silicon-rich molecular sieve with a Si / Al molar ratio of 3 to 100.

[0010] The method of using silicon aluminum molecular sieve as a precursor to prepare carbon-interval-rich unsaturated coordination nano AlF 3 The method is characterized in that the N 2 The specific process of calcining the silicon-aluminum molecular sieve in an atmosphere or argon atmosphere is as follows: placing the silicon-aluminum molecular sieve in a tube furnace and introducing N 2 or argon, and calcine at a calcination temperature of 250-550° C. for 1-10 hours, and then naturally cool to room temperature after the calcination. The calcination temperature is preferably 350-550° C., and the calcination time is preferably 2-8 hours.

[0011] The method for preparing a carbon-interval nano-AlF3 catalyst rich in unsaturated coordination using a silicon-aluminum molecular sieve as a precursor is characterized in that the fluorine source is a gas-phase fluorine source, and the specific process of fluorinating the catalyst precursor after calcination is as follows: placing the silicon-aluminum molecular sieve in a tube furnace, introducing a gas-phase fluorine source, calcining at 250-450°C for 8-60h, and switching N 2 atmosphere, and then cooled naturally to room temperature to obtain carbon-interval-rich unsaturated coordination nano-AlF 3 The catalyst, the calcination temperature is preferably 300-400°C, the calcination time is preferably 20-30h; the gas phase fluorine source includes HF, CHFCl 2 , CHF 3 or CHClF 2 Fluorine-containing gases.

[0012] The method of using silicon aluminum molecular sieve as a precursor to prepare carbon-interval-rich unsaturated coordination nano AlF 3 The catalyst method is characterized in that the fluorine source is a fluorine-containing polymer, wherein the fluorine-containing polymer is one of PVDF, PTFE and PVF, and the mass ratio of the fluorine-containing polymer to the catalyst precursor is 2 to 3:1. The specific process of fluorinating the calcined catalyst precursor is as follows: dissolving the fluorine-containing polymer in an organic solvent to obtain a solution, adding the catalyst precursor and uniformly mixing, drying at 60 to 120° C. to remove the organic solvent, and then calcining at 250 to 400° C. in a muffle furnace for 2 to 15 hours, and then cooling to room temperature to obtain a carbon-spaced nano-AlF rich in unsaturated coordination. 3 Catalyst; wherein the fluorine-containing polymer is one of PVDF, PTFE and PVF, the organic solvent is N,N-dimethylformamide or butanone, the temperature for drying to remove the organic solvent is preferably 70-120°C, the temperature for calcining in a muffle furnace is preferably 300-350°C, and the calcining time is preferably 4-10h.

[0013] The method for preparing a carbon-intervaled unsaturated coordinated nano AlF3 catalyst using a silicon-aluminum molecular sieve as a precursor is characterized in that the fluorine source is a fluorine-containing compound, and the fluorine-containing compound is one of ammonium fluoride or ammonium bifluoride, preferably ammonium fluoride. The mass ratio of the fluorine-containing compound to the catalyst precursor is 1.5 to 2.5:1, preferably 2:1. The specific process of fluorinating the calcined catalyst precursor is as follows: Place the fluorine-containing compound and the catalyst precursor in a ball mill together for ball milling, with a mill speed of 200 to 450 r / min and a ball milling time of 4 to 6 hours; dry after ball milling, and then place in a tubular furnace N 2 The carbon-spaced nano-AlF 3 catalyst.

[0014] The carbon-spaced nano AlF prepared by the method defined in the present invention 3 catalyst.

[0015] The carbon spaced nano-AlF 3 The catalyst is used in catalytic cracking and dehydrofluorination reaction of fluorinated alkanes, wherein the fluorinated alkanes are 1,1-difluoroethane or 1,1,1,3,3-pentafluoropropane, the temperature of the reaction for removing HF from the fluorinated alkanes to prepare fluorinated olefins is 300-450°C, the reaction pressure is normal pressure, and the prepared fluorinated olefins are vinyl fluoride or 1,1,1,3-tetrafluoropropylene.

[0016] By adopting the above technology, compared with the prior art, the beneficial effects of the present invention are as follows:

[0017] 1) The Si-Al bonds in the calcined Si-Al molecular sieve have an interaction force, and Si will be converted to SiF during the HF removal reaction or under the fluorination of the fluorine source. 4 The original Si-Al bond is changed to Al-F bond, and a special AlF bond is produced under the action of carbon. 3 Defect sites, thus producing higher catalytic activity. Carbon-spaced nano-AlF prepared using silicon-aluminum molecular sieve as a precursor 3 The catalytic activity of the catalyst in the HF removal reaction of HFCs is higher than that of ordinary AlF 3 The catalyst is 20-25% higher, and still has a high activity of 60% after 60 hours of reaction, and has excellent stability. 3 The catalyst has good application prospects in the field of HFCs HF removal.

[0018] 2) Carbon-spaced nano-AlF 3 The catalyst is prepared by using silicon-alumina molecular sieve as precursor and N 2 Or argon calcination, the preparation method is simple, the obtained carbon spacer nano AlF 3 The catalyst has high catalytic activity and stability in the reaction of preparing fluorinated olefins by removing HF from fluorinated alkanes in the gas phase, thereby increasing the service life of the catalyst. The catalyst is not easy to sinter and deactivate during the reaction, and the yield of the target product is high and it is easy to industrialize. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a comparison of the relationship between the conversion rate of the reactant 1,1,1,3,3-pentafluoropropane catalyzed by different catalysts and the reaction time in the examples of the present invention. DETAILED DESCRIPTION

[0020] The present invention will be further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.

[0021] Example 1

[0022] Preparation of the low silicon molecular sieve catalyst of the present invention: according to the following composition 1.0Al 2 O 3 :1.0Triethylamine:0.4SiO 2 :40H 2 O (molar ratio) in turn, pseudo-boehmite, triethylamine, silica sol and deionized water were mixed and stirred to form a uniform gel. The gel was transferred to a stainless steel crystallization kettle and crystallized at 180°C for 48 hours, and then the product was cooled to room temperature. The product was filtered, washed and dried to obtain low-silicon molecular sieve raw powder. It can be seen that the pseudo-boehmite of the raw material for preparing the low-silicon molecular sieve raw powder is Al 2 O 3 The molar ratio of the organic template agent triethylamine is 1:1.

[0023] Silicon-aluminum ratio detection method: using X-ray fluorescence spectrometer (XRF) manufactured by Philips of the Netherlands, model (PHILIPS PW-2400 X-ray spectrometer). The XRF detection of the low-silicon molecular sieve raw powder prepared above showed that its silicon-aluminum ratio Si / Al=1.

[0024] With low silicon molecular sieve (Si / Al=1) as the precursor, 5.357 g of low silicon molecular sieve (Si / Al=1) was placed in an atmosphere tube furnace and N was introduced at 250 °C. 2 , N 2 The flow rate was 5 mL / min, and the calcination was carried out for 10 hours. After the calcination, the temperature was naturally cooled to room temperature to obtain stable carbon-spaced nano-AlF 3 Catalyst precursor: The obtained catalyst sample was pressed into tablets at 10-20 MPa, crushed, and sieved with a 20-40 mesh sieve.

[0025] The carbon-spaced nano-AlF 3 The catalyst precursor is used to catalyze the cracking of 1,1-difluoroethane (HFC-152a) to prepare vinyl fluoride, and the in-situ fluorination reaction is as follows:

[0026]

[0027] The reaction conditions are as follows: the catalyst is loaded into a fixed bed reactor with a catalyst loading of 1 mL and N 2 Mixed gas of HFC-152a, N 2 Flow rate 10mL / min, HFC-152a flow rate 10mL / min, N 2The total space velocity of the mixed gas of 1,1-difluoroethane (HFC-152a) and HCFC-152a was 1200 / h, and the reaction temperature was 350°C. After 22 hours of reaction, the sample was analyzed, and the results were: the conversion rate of the reactant 1,1-difluoroethane (HFC-152a) was 63.25%, and the selectivity of the product vinyl fluoride was 100%, and after 29 hours of catalytic reaction, the sample was analyzed, and the conversion rate of the reactant HFC-152a was 67.8%, and the selectivity of the product vinyl fluoride was 100% (that is, the conversion rate of the reactant and the selectivity of the target product remained basically unchanged).

[0028] Example 2

[0029] The silicon-rich molecular sieve (Si / Al=34) in the embodiment of the present invention was purchased from the catalyst factory of Nankai University. According to its product description: the silicon-aluminum ratio Si / Al=34, the organic template agent for preparing the raw material of the silicon-rich molecular sieve (Si / Al=34) is hexamethylenediamine, and the aluminum source for preparing the raw material is Al 2 O 3 The molar ratio of the organic template agent hexamethylenediamine is 0.8:1.

[0030] With silicon-rich molecular sieve (Si / Al=34) as the precursor, 6.11 g of silicon-rich molecular sieve (Si / Al=34) was placed in an atmosphere tube furnace, argon was introduced at 400°C, and the argon flow rate was 15 mL / min for 5 h. The temperature was naturally cooled to room temperature to obtain stable carbon-spaced nano-AlF 3 Catalyst precursor: The obtained catalyst sample was pressed into tablets at 10-20 MPa, crushed, and sieved with a 20-40 mesh sieve.

[0031] The carbon-spaced nano-AlF 3 The catalyst precursor is used to catalyze the cracking of 1,1-difluoroethane (HFC-152a) to prepare vinyl fluoride and perform in-situ fluorination. The reaction conditions are: the catalyst is loaded into a fixed bed reactor with a catalyst loading of 1 mL, and N 2 and HFC-245fa mixed gas, N 2 Flow rate 10mL / min, HFC-245fa flow rate 10mL / min, N 2 The total space velocity of the mixed gas of 1,200 / h and HFC-245fa was 350°C. The results of sampling and analysis after 25h of reaction were as follows: the conversion rate of the reactant (HFC-152a) was 64.5%, and the selectivity of the product vinyl fluoride was 100%. After 29h of catalytic reaction, the conversion rate of the reactant HFC-152a was 63.8%, and the selectivity of the product vinyl fluoride was 100% (i.e., the conversion rate of the reactant and the selectivity of the target product remained basically unchanged).

[0032] Example 3

[0033] The Y-type molecular sieve (Si / Al=2.8) in the embodiment of the present invention was purchased from the catalyst factory of Nankai University. According to its product description: the silicon-aluminum ratio Si / Al=2.8, the organic template agent for preparing the raw material of the Y-type molecular sieve (Si / Al=2.8) is tetramethylammonium hydroxide, and the aluminum source for preparing the raw material is Al 2 O 3 The molar ratio of the organic template agent to tetramethylammonium hydroxide is 0.8:1.

[0034] Using Y-type molecular sieve (Si / Al=2.8) as the precursor, 7.06 g of Y-type molecular sieve (Si / Al=2.8) was placed in an atmosphere tube furnace and N2 was introduced at 450°C. 2 , N 2 The flow rate was 15 mL / min and the mixture was calcined for 5 h. After the calcination, the mixture was cooled to room temperature naturally. 5 g of calcined 3A molecular sieve and 15 g of PVDF (average molecular weight 55 W, the same below) were placed in 100 mL of DMF and stirred for 1 h. After stirring, the mixture was placed in an oven at 120 ° C until the DMF was dried. The dried sample was placed in a muffle furnace and calcined at 350 ° C for 8 h. This resulted in the stable carbon-spaced nano-AlF 3 Catalyst: The obtained catalyst sample was pressed into tablets at 10-20 MPa, crushed, and sieved with a 20-40 mesh sample sieve.

[0035] The carbon-spaced nano-AlF 3 The catalyst is used to catalyze the cracking of 1,1-difluoroethane (HFC-152a) to produce vinyl fluoride. The reaction formula is as follows:

[0036]

[0037] The reaction conditions are as follows: the catalyst is loaded into a fixed bed reactor with a catalyst loading of 1 mL and N 2 Mixed gas of HFC-152a, N 2 Flow rate 10mL / min, HFC-152a flow rate 10mL / min, N 2 The total space velocity of the mixed gas of 1,1-difluoroethane and HFC-152a was 1200 / h, and the reaction temperature was 350°C. After 25 hours of reaction, the sample was analyzed, and the results were: the conversion rate of the reactant 1,1-difluoroethane (HFC-152a) was 65.9%, the selectivity of the product vinyl fluoride was 100%, and after 35 hours of catalytic reaction, the sample was analyzed, and the conversion rate of the reactant was 65.8%, and the selectivity of the target product was 100%.

[0038] Example 4

[0039] Take the low silicon molecular sieve (Si / Al=1) of Example 1 as the precursor, put 7.24g of low silicon molecular sieve (Si / Al=1) into an atmosphere tube furnace, introduce argon at 550℃, and roast for 1h at a flow rate of 20mL / min, then wait until the roasting is completed and naturally cool to room temperature, put 6g of the roasted low silicon molecular sieve (Si / Al=1) and 12g of ammonium bifluoride into a ball mill, and put the ball mill into the ball mill and fix it. Set the ball mill program to 400r / min, the ball milling time to 3.5h, and pause for 30min every hour until the program ends. Put the ball mill and its ball-milled sample into an oven and dry it at 80℃ for 6h, take out the sample, and put it in a tube furnace N 2 Stable carbon-spaced nano-AlF was obtained by calcining at 400℃ for 3h in an atmosphere. 3 Catalyst: The obtained catalyst sample was pressed into tablets at 10-20 MPa, crushed, and sieved with a 20-40 mesh sample sieve.

[0040] The carbon-spaced nano-AlF 3 The catalyst is used to catalyze the cracking of 1,1,1,3,3-pentafluoropropane (HFC-245fa) to prepare 1,3,3,3-tetrafluoropropylene (HFO-1234ze). The reaction formula is as follows:

[0041]

[0042] The reaction conditions are as follows: the catalyst is loaded into a fixed bed reactor with a catalyst loading of 1 mL and N 2 and HFC-245fa mixed gas, N 2 Flow rate 10mL / min, HFC-245fa flow rate 10mL / min, N 2 The total space velocity of the mixed gas of HFC-245fa was 1200 / h, and the reaction temperature was 350°C. After 20 hours of reaction, the sample was taken for analysis, and the results were: the conversion rate of the reactant 1,1,1,3,3-pentafluoropropane was 66.3%, the selectivity of the product cis-trans 1,3,3,3-tetrafluoropropene (HFO-1234ze) was 99.5%, and after 28 hours of catalytic reaction, the sample was taken for analysis, and the conversion rate of the reactant was 65.8%, and the selectivity of the target product was 99.2%.

[0043] Example 5

[0044] The Y-type molecular sieve (Si / Al=2.8) of Example 3 was used as a precursor. 6.58 g of the Y-type molecular sieve (Si / Al=2.8) was placed in an atmosphere tube furnace and calcined at 550°C with argon gas at a flow rate of 15 mL / min for 4 h. After the temperature was naturally cooled to room temperature, a stable carbon-spaced nano-AlF 3Catalyst precursor: The obtained catalyst sample was pressed into tablets at 10-20 MPa, crushed, and sieved with a 20-40 mesh sieve.

[0045] The carbon-spaced nano-AlF 3 The catalyst precursor is used to catalyze the cracking of 1,1-difluoroethane (HFC-152a) to produce vinyl fluoride. The reaction formula is as follows:

[0046]

[0047] The reaction conditions are as follows: the catalyst is loaded into a fixed bed reactor with a catalyst loading of 1 mL and N 2 Mixed gas of HFC-152a, N 2 Flow rate 10mL / min, HFC-152a flow rate 10mL / min, N 2 The total space velocity of the mixed gas of 1,1-difluoroethane (HFC-152a) and HFC-152a was 1200 / h, and the reaction temperature was 350°C. The results of sampling and analysis after 22 hours of reaction were: the conversion rate of the reactant 1,1-difluoroethane (HFC-152a) was 65.5%, the selectivity of the product fluoroethylene was 100%, and the sampling and analysis after 30 hours of catalytic reaction showed that the conversion rate of the reactant was 65.1% and the selectivity of the target product was 100%.

[0048] Example 6

[0049] Take the low silicon molecular sieve (Si / Al=1) molecular sieve of Example 1 as the precursor, put 5.87g of low silicon molecular sieve (Si / Al=1) into an atmosphere tube furnace, introduce argon at 350°C with an argon flow rate of 10mL / min and roast for 8h, then put 7.52g of the roasted low silicon molecular sieve (Si / Al=1) and 15.218g of PVDF into 100mL of DMF and stir for 1h. After stirring, put it into an oven at 120°C until the DMF is dried, and the dried sample is placed in a muffle furnace and roasted at 350°C for 8h. Then wait until the roasting is completed and cool naturally to room temperature to obtain a stable carbon-spaced AlFx catalyst. The obtained catalyst sample is pressed into tablets at 10-20MPa, crushed, and sieved with a 20-40 mesh sieve.

[0050] The carbon-spaced nano-AlF 3 The catalyst is used to catalyze the cracking of 1,1-difluoroethane (HFC-152a) to prepare vinyl fluoride. The reaction formula is as follows:

[0051]

[0052] The reaction conditions are as follows: the catalyst is loaded into a fixed bed reactor with a catalyst loading of 1 mL and N 2Mixed gas of HFC-152a, N 2 Flow rate 10mL / min, HFC-152a flow rate 10mL / min, N 2 The total space velocity of the mixed gas of 1,1-difluoroethane and HFC-152a was 1200 / h, and the reaction temperature was 350°C. After 21h of reaction, the sample was taken for analysis, and the results were: the conversion rate of the reactant 1,1-difluoroethane (HFC-152a) was 66.5%, and the selectivity of the product vinyl fluoride was 100%. After 28h of catalytic reaction, the sample was taken for analysis, and the conversion rate of the reactant was 67.2%, and the selectivity of the target product was 100%.

[0053] Example 7

[0054] The silicon-rich molecular sieve (Si / Al=34) of Example 2 was used as a precursor. 5.88 g of the silicon-rich molecular sieve (Si / Al=34) was placed in an atmosphere tube furnace and N was introduced at 350°C. 2 , N 2 The flow rate was 10 mL / min, and the calcination was performed for 8 hours. Then 5.7 g of the calcined silicon-rich molecular sieve (Si / Al=34) and 16.92 g of PWF were placed in 120 mL of DMF and stirred for 1 hour. After stirring, the mixture was placed in an oven at 120°C until the DMF was dried. The dried sample was placed in a muffle furnace and calcined at 350°C for 10 hours. Then the mixture was cooled naturally to room temperature to obtain a stable carbon-spaced nano-AlF 3 Catalyst: The obtained catalyst sample was pressed into tablets at 10-20 MPa, crushed, and sieved with a 20-40 mesh sample sieve.

[0055] The carbon-spaced nano-AlF 3 The catalyst is used to catalyze the cracking of 1,1,1,3,3-pentafluoropropane (HFC-245fa) to prepare 1,3,3,3-tetrafluoropropylene (HFO-1234ze). The reaction formula is as follows:

[0056]

[0057] The reaction conditions are as follows: the catalyst is loaded into a fixed bed reactor with a catalyst loading of 1 mL and N 2 and HFC-245fa mixed gas, N 2 Flow rate 10mL / min, HFC-245fa flow rate 10mL / min, N 2The total space velocity of the mixed gas of HFC-245fa was 1200 / h, and the reaction temperature was 350°C. After 18 hours of reaction, the sample was taken for analysis, and the results were: the conversion rate of the reactant 1,1,1,3,3-pentafluoropropane was 62.3%, the selectivity of the product cis-trans 1,3,3,3-tetrafluoropropene (HFO-1234ze) was 99.3%, and after 28 hours of catalytic reaction, the sample was taken for analysis, and the conversion rate of the reactant was 68.4%, and the selectivity of the target product was 99.1%.

[0058] Example 8

[0059] Take the silicon-rich molecular sieve (Si / Al=34) of Example 2 as a precursor, put 6.09g of silicon-rich molecular sieve (Si / Al=34) into an atmosphere tube furnace, introduce argon at 400°C, and roast for 3h at a flow rate of 20mL / min, then naturally cool to room temperature, put 6.03g of the roasted silicon-rich molecular sieve (Si / Al=34) and 11.93g of ammonium bifluoride into a ball mill, and put the ball mill into the ball mill and fix it. Set the ball mill program to 400r / min, ball mill for 3.5h, and pause for 30min every hour until the program ends. Put the ball mill and its ball-milled sample into an oven and dry at 80°C for 6h, take out the sample, and put it in a tube furnace N 2 Stable carbon-spaced nano-AlF 3 Catalyst: The obtained catalyst sample was pressed into tablets at 10-20 MPa, crushed, and sieved with a 20-40 mesh sample sieve.

[0060] The carbon-spaced nano-AlF 3 The catalyst is used to catalyze the cracking of 1,1-difluoroethane (HFC-152a) to prepare vinyl fluoride. The reaction formula is as follows:

[0061]

[0062] The reaction conditions are as follows: the catalyst is loaded into a fixed bed reactor with a catalyst loading of 1 mL and N 2 Mixed gas of HFC-152a, N 2 Flow rate 10mL / min, HFC-152a flow rate 10mL / min, N 2 The total space velocity of the mixed gas of 1,1-difluoroethane (HFC-152a) and HCFC-152a was 1200 / h, and the reaction temperature was 350°C. After 20 hours of reaction, the sample was analyzed, and the results showed that the conversion rate of the reactant 1,1-difluoroethane (HFC-152a) was 63.5%, and the selectivity of the product vinyl fluoride was 100%. After 30 hours of catalytic reaction, the sample was analyzed, and the conversion rate of the reactant was 64.8%, and the selectivity of the target product was 100%.

[0063] Example 9

[0064] Using the Y-type molecular sieve (Si / Al=2.8) of Example 3 as a precursor, 5.29 g of the Y-type molecular sieve (Si / Al=2.8) was placed in an atmosphere tube furnace and N was introduced at 550°C. 2 , N 2 The flow rate was 15 mL / min and the calcination was continued for 4 h. Then, the gaseous fluorine source CHF was introduced at 300 °C. 3 , the gas phase fluorine source flow rate is 10mL / min for fluorination for 3 hours, wait until the gas phase fluorination is completed and the temperature naturally drops to room temperature, put 5.01g of Y-type molecular sieve (Si / Al=2.8) and 11.57g of ammonium bifluoride into the ball mill, and put the ball mill into the ball mill and fix it. Set the ball mill program to 450r / min, ball mill for 3 hours, and pause for 30 minutes every hour until the program ends. Put the ball mill and the ball milled sample into an oven and dry it at 100℃ for 5 hours, take out the sample, and put it in a tube furnace N 2 Stable carbon-spaced nano-AlF 3 Catalyst: The obtained catalyst sample was pressed into tablets at 10-20 MPa, crushed, and sieved with a 20-40 mesh sample sieve.

[0065] The nano-AlFx catalyst prepared above is used to catalyze the cracking of 1,1-difluoroethane (HFC-152a) to prepare vinyl fluoride, and the reaction formula is as follows:

[0066]

[0067] The reaction conditions are as follows: the catalyst is loaded into a fixed bed reactor with a catalyst loading of 1 mL and N 2 Mixed gas of HFC-152a, N 2 Flow rate 10mL / min, HFC-152a flow rate 10mL / min, N 2 The total space velocity of the mixed gas of 1,1-difluoroethane and HFC-152a was 1200 / h, and the reaction temperature was 350°C. After 25 hours of reaction, the sample was analyzed, and the results showed that the conversion rate of the reactant 1,1-difluoroethane (HFC-152a) was 64.5%, and the selectivity of the product vinyl fluoride was 100%. After 30 hours of catalytic reaction, the sample was analyzed, and the conversion rate of the reactant was 65.1%, and the selectivity of the target product was 100%.

[0068] Example 10

[0069] The silicon-rich molecular sieve (Si / Al=63) in the embodiment of the present invention was purchased from the catalyst factory of Nankai University. According to its product description: the silicon-aluminum ratio Si / Al=63, the organic template agent for preparing the raw material of the silicon-rich molecular sieve (Si / Al=63) is hexamethylenediamine, and the aluminum source for preparing the raw material is Al 2 O3 The molar ratio of the organic template agent hexamethylenediamine is 0.8:1.

[0070] With silicon-rich molecular sieve (Si / Al=63) as the precursor, 6.21 g of silicon-rich molecular sieve (Si / Al=63) was placed in an atmosphere tube furnace, argon was introduced at 400°C, and the argon flow rate was 15 mL / min for 5 h, and then the gas phase fluorine source CHF was introduced at 300°C. 3 The gas phase fluorine source flow rate is 20 mL / min for 1 hour, and the temperature is naturally cooled to room temperature to obtain stable carbon-spaced nano-AlF 3 Catalyst: The obtained catalyst sample was pressed into tablets at 10-20 MPa, crushed, and sieved with a 20-40 mesh sample sieve.

[0071] The carbon-spaced nano-AlF 3 The catalyst is used to catalyze the cracking of 1,1,1,3,3-pentafluoropropane (HFC-245fa) to prepare 1,3,3,3-tetrafluoropropylene (HFO-1234ze). The reaction formula is as follows:

[0072]

[0073] The reaction conditions are as follows: the catalyst is loaded into a fixed bed reactor with a catalyst loading of 1 mL and N 2 and HFC-245fa mixed gas, N 2 Flow rate 10mL / min, HFC-245fa flow rate 10mL / min, N 2 The total space velocity of the mixed gas of HFC-245fa was 1200 / h, and the reaction temperature was 350°C. After 25 hours of reaction, the sample was taken for analysis, and the results were: the conversion rate of the reactant 1,1,1,3,3-pentafluoropropane was 68.5%, the selectivity of the product cis-trans 1,3,3,3-tetrafluoropropene (HFO-1234ze) was 64.6%, and after 32 hours of catalytic reaction, the sample was taken for analysis, and the conversion rate of the reactant was 68.2%, and the selectivity of the target product was 99.0%.

[0074] Embodiment 11

[0075] Take the silicon-rich molecular sieve (Si / Al=34) of Example 2 as a precursor, put 6.09g of the silicon-rich molecular sieve (Si / Al=34) into an atmosphere tube furnace, introduce argon at 400°C, and roast for 3h at a flow rate of 20mL / min, then naturally cool to room temperature, put 6.04g of the roasted silicon-rich molecular sieve (Si / Al=63) and 11.85g of ammonium bifluoride into a ball mill, and fix the ball mill in the ball mill. Set the ball mill program to 400r / min, ball mill for 3.5h, and pause for 30min every hour until the program ends. Put the ball mill and its ball-milled sample into an oven and dry at 80°C for 6h, take out the sample, and place it in a tube furnace N 2 Stable carbon-spaced nano-AlF 3 Catalyst: The obtained catalyst sample was pressed into tablets at 10-20 MPa, crushed, and sieved with a 20-40 mesh sample sieve.

[0076] The carbon-spaced nano-AlF 3 The catalyst is used to catalyze the cracking of 1,1-difluoroethane (HFC-152a) to prepare vinyl fluoride. The reaction formula is as follows:

[0077]

[0078] The reaction conditions are as follows: the catalyst is loaded into a fixed bed reactor with a catalyst loading of 1 mL and N 2 Mixed gas of HFC-152a, N 2 Flow rate 10mL / min, HFC-152a flow rate 10mL / min, N 2 The total space velocity of the mixed gas of 1,1-difluoroethane (HFC-152a) and HCFC-152a was 1200 / h, and the reaction temperature was 350°C. After 20 hours of reaction, the sample was analyzed, and the results showed that the conversion rate of the reactant 1,1-difluoroethane (HFC-152a) was 65.5%, and the selectivity of the product vinyl fluoride was 100%. After 30 hours of catalytic reaction, the sample was analyzed, and the conversion rate of the reactant was 64.8%, and the selectivity of the target product was 100%.

[0079] Example 12

[0080] The silicon-rich molecular sieve (Si / Al=63) of Example 10 was used as a precursor. 5.84 g of the silicon-rich molecular sieve (Si / Al=63) was placed in an atmosphere tube furnace and N was introduced at 350°C. 2 , N 2The flow rate was 10 mL / min, and the calcination was performed for 8 hours. Then 5.7 g of the calcined silicon-rich molecular sieve (Si / Al=34) and 16.90 g of PWF were placed in 120 mL of DMF and stirred for 1 hour. After stirring, the mixture was placed in an oven at 120°C until the DMF was dried. The dried sample was placed in a muffle furnace and calcined at 350°C for 10 hours. Then the mixture was cooled naturally to room temperature to obtain a stable carbon-spaced nano-AlF 3 Catalyst: The obtained catalyst sample was pressed into tablets at 10-20 MPa, crushed, and sieved with a 20-40 mesh sample sieve.

[0081] The carbon-spaced nano-AlF 3 The catalyst is used to catalyze the cracking of 1,1,1,3,3-pentafluoropropane (HFC-245fa) to prepare 1,3,3,3-tetrafluoropropylene (HFO-1234ze). The reaction formula is as follows:

[0082]

[0083] The reaction conditions are as follows: the catalyst is loaded into a fixed bed reactor with a catalyst loading of 1 mL and N 2 and HFC-245fa mixed gas, N 2 Flow rate 10mL / min, HFC-245fa flow rate 10mL / min, N 2 The total space velocity of the mixed gas of HFC-245fa was 1200 / h, and the reaction temperature was 350°C. After 18 hours of reaction, the sample was taken for analysis, and the results were: the conversion rate of the reactant 1,1,1,3,3-pentafluoropropane was 64.3%, the selectivity of the product cis-trans 1,3,3,3-tetrafluoropropene (HFO-1234ze) was 99.3%, and after 28 hours of catalytic reaction, the sample was taken for analysis, and the conversion rate of the reactant was 66.4%, and the selectivity of the target product was 99.1%.

[0084] Application implementation comparison experiment:

[0085] 1) Precipitation AlF 3 Catalyst preparation: 0.1 mol Al(NO) 3 9H 2 O was added to 100 mL of deionized water, referred to as solution A. 0.6 mol NH 4 F was added to 100 mL of deionized water, which was called solution B. After the solid was completely dissolved, solution B was slowly added to solution A and stirred for 3 h. Then, the obtained product was washed by centrifugation with deionized water, dried at 100 °C overnight, and calcined at 550 °C for 3 h. The obtained sample was recorded as AlF 3 -Precipitation method.

[0086] 2) Thermal decomposition of AlF3 Preparation of catalyst: 6 g (NH 4 ) 3 AlF 6 It was placed in a tube furnace and calcined at 550°C for 3 h. The resulting sample was recorded as AlF 3 - Thermal cracking method.

[0087] 3) Three carbon-spaced nano-AlF 3 The catalyst precursors (i.e., not fluorinated by a fluorine source) are: the low silicon molecular sieve (Si / Al=1) of Example 1, the Y-type molecular sieve (Si / Al=2.8) of Example 3, and the silicon-rich molecular sieve (Si / Al=63) of Example 10. The three samples are respectively labeled as AlF x - Low silicon (Si / Al=1), AlF x -Medium silicon (Si / Al=2.8) and AlF x - silicon-rich (Si / Al=63), put it into an atmosphere tube furnace, introduce argon at 400°C, and calcine for 5h at an argon flow rate of 15mL / min, and cool it naturally to room temperature to obtain carbon-spaced nano-AlF 3 Catalyst Precursors.

[0088] The three carbon-spaced nano-AlF 3 Catalyst precursor (i.e. not fluorinated by fluorine source), precipitation method AlF 3 Catalysts and thermal decomposition of AlF 3 The catalysts were used in the reaction of removing HF from fluorinated alkanes in the gas phase to prepare fluorinated olefins. The reaction conditions were completely the same. The specific process was as follows: the catalyst was pressed into tablets at 15 MPa for 3 min, taken out and crushed and sieved to 20-40 mesh, and loaded into a fixed bed reactor with a catalyst loading of 1 mL. N 2 and HFC-152a gas mixture, N 2 Flow rate 10mL / min, HFC-152a flow rate 10mL / min, N 2 The total space velocity of the mixed gas of HFC-152a is 1200 / h, and the reaction temperature is 300℃. As the catalytic reaction proceeds, the relationship between the conversion rate of the reactant 1,1,1,3,3-pentafluoropropane and the reaction time is shown in Figure 1 middle.

[0089] according to Figure 1 The results show that the carbon spacer nano-AlF 3 The catalytic activity of the catalyst is significantly higher than that of AlF prepared by conventional methods. 3 Catalyst. In addition, Figure 1 Three kinds of carbon spaced nano-AlF 3The reason why the catalytic activity of the catalyst precursor (i.e., not fluorinated by a fluorine source) gradually increased within the first 12 hours is that the reactant HFC-152a, to a certain extent, acts as a fluorine source to gradually convert the catalyst precursor into AlF with higher catalytic activity. 3 catalyst.

[0090] The contents described in this specification are merely an enumeration of implementation forms of the inventive concept, and the protection scope of the present invention should not be regarded as being limited to the specific forms described in the embodiments.

Claims

1. A method for preparing carbon-interval-rich unsaturated coordination nano-AlF using silicon-aluminum molecular sieve as precursor 3 Catalyst method, Features The preparation process includes the following steps: using a silicon-aluminum molecular sieve containing an organic template as a precursor, 2 The silicon-aluminum molecular sieve is calcined in an atmosphere or an argon atmosphere, and the organic template is retained in the pores of the silicon-aluminum molecular sieve in the form of a carbon interval to obtain a catalyst precursor, and then the calcined catalyst precursor is fluorinated under the action of a fluorine source to obtain a carbon-interval-rich unsaturated coordination nano-AlF 3 catalyst.

2. The method of claim 1 for preparing a carbon-interval-rich unsaturated coordinated nano-AlF using a silicon-aluminum molecular sieve as a precursor 3 Catalyst method, Features The organic template is triethylamine, tetramethylammonium hydroxide or hexamethylenediamine. The preparation method of the silica-alumina molecular sieve containing the organic template is as follows: an aluminum source, an organic template, a silicon source and deionized water are mixed, and the mixture is stirred to form a uniform gel. After the gel is crystallized at 160-200° C. for 40-60 hours, the product is cooled to room temperature, and the product is filtered, washed with deionized water, and dried at 100-110° C. to obtain a silica-alumina molecular sieve containing an organic template. The aluminum source of the raw material for preparing the silica-alumina molecular sieve is Al 2 O 3 The molar ratio of the organic template to the organic template is 1:0.7~1.

3. The method of claim 1 for preparing a carbon-interval-rich unsaturated coordinated nano-AlF using a silicon-aluminum molecular sieve as a precursor 3 Catalyst method, Features The silicon-aluminum molecular sieve is a low-silicon molecular sieve with a Si / Al molar ratio of 1 to 1.5, a Y-type molecular sieve with a Si / Al molar ratio of 1.5 to 3.0, or a silicon-rich molecular sieve with a Si / Al molar ratio of 3 to 100.

4. The method of claim 1 for preparing a carbon-interval-rich unsaturated coordinated nano-Al using a silicon-aluminum molecular sieve as a precursor F3 Catalyst method, Features In N 2 The specific process of calcining the silicon-aluminum molecular sieve in an atmosphere or argon atmosphere is as follows: placing the silicon-aluminum molecular sieve in a tube furnace and introducing N 2 or argon, roast at a roasting temperature of 250~550℃ for 1~10h, and then cool naturally to room temperature after roasting.

5. A method of preparing a carbon-interval-rich unsaturated coordinated nano-Al using a silicon-aluminum molecular sieve as a precursor as claimed in claim 4 F3 Catalyst method, Features Pass N 2 Or the calcination temperature under argon is 350~550℃, and the calcination time is 2-8h.

6. The method of claim 1 for preparing carbon-interval-rich unsaturated coordinated nano-AlF using silicon aluminum molecular sieve as a precursor 3 Catalyst method, Features The fluorine source is a gas-phase fluorine source. The specific process of fluorinating the calcined catalyst precursor is as follows: the silicon-aluminum molecular sieve is placed in a tube furnace, a gas-phase fluorine source is introduced, and calcined at 250-450°C for 8-60h. After the calcination, the N 2 atmosphere, and then cooled naturally to room temperature to obtain carbon-interval-rich unsaturated coordination nano-AlF 3 Catalyst; the gas phase fluorine source includes HF, CHFCl 2 , CHF 3 or CHClF 2 Fluorine-containing gases.

7. The method of claim 6 for preparing carbon-interval-rich unsaturated coordinated nano-AlF using silicon aluminum molecular sieve as a precursor 3 Catalyst method, Features The calcination temperature under the introduction of gaseous fluorine source is 300-400°C, and the calcination time is 20-30h.

8. The method of claim 1 for preparing carbon-interval-rich unsaturated coordinated nano-AlF using silicon aluminum molecular sieve as a precursor 3 Catalyst method, Features The fluorine source is a fluorine-containing polymer. The specific process of fluorinating the calcined catalyst precursor is as follows: dissolving the fluorine-containing polymer in an organic solvent to obtain a solution, adding the catalyst precursor and uniformly mixing, drying at 60-120°C to remove the organic solvent, and then calcining at 250-400°C in a muffle furnace for 2-15 hours, and then cooling to room temperature to obtain a carbon-interval-rich unsaturated coordination nano-AlF 3 Catalyst; wherein the fluorine-containing polymer is one of PVDF, PTFE and PVF, and the mass ratio of the fluorine-containing polymer to the catalyst precursor is 2~3:1; the organic solvent is N,N-dimethylformamide or butanone.

9. The method of claim 8 for preparing carbon-interval-rich unsaturated coordinated nano-AlF using silicon aluminum molecular sieve as a precursor 3 Catalyst method, Features The fluorine-containing polymer is dissolved in an organic solvent to obtain a solution, a catalyst precursor is added and uniformly mixed, the temperature for drying and removing the organic solvent is 70-120°C, the temperature for calcining in a muffle furnace is 300-350°C, and the calcining time is 4-10h.

10. The method of claim 1 for preparing carbon-interval-rich unsaturated coordinated nano-AlF using silicon aluminum molecular sieve as a precursor 3 Catalyst method, Features The fluorine source is a fluorine-containing compound, and the fluorine-containing compound is one of ammonium fluoride or ammonium bifluoride; the mass ratio of the fluorine-containing compound to the catalyst precursor is 1.5-2.5:1; the specific process of fluorinating the calcined catalyst precursor is as follows: the fluorine-containing compound and the catalyst precursor are placed in a ball milling jar for ball milling, the milling speed is 200-450r / min, and the ball milling time is 4-6h; after the ball milling is completed, it is dried and then placed in a tube furnace N 2 The carbon-spaced nano-AlF 3 catalyst.

11. The method of claim 10 for preparing carbon-interval-rich unsaturated coordination nano-AlF using silicon aluminum molecular sieve as a precursor 3 Catalyst method, Features The fluorine-containing compound is ammonium fluoride, and the mass ratio of the fluorine-containing compound to the catalyst precursor is 2:

1.

12. Carbon-spaced nano AlF prepared by the method according to any one of claims 1 to 11 3 catalyst.

13. The carbon-spaced nano-AlF as claimed in claim 12 3 Application of the catalyst in catalytic cracking and dehydrofluorination of fluorinated alkanes.

Citation Information

Patent Citations

  • Sub-nano AlF3 catalyst as well as preparation method and application thereof

    CN112675882A

  • Carbon confinement nanometer AlF3 catalyst and preparation method and application thereof

    CN113546649A

  • Anti-sintering nano AlFx catalyst prepared from porous material precursor containing PO4 tetrahedron, preparation method and application thereof

    CN113952968A