A method for preparing silver nanowire conductive film
By using nylon filter cloth and syringe pump system, the silver nanowire solution is automatically brushed and coated, and the problem of poor thickness control and adhesion in the preparation of conductive silver nanowire films in the prior art is solved, achieving high efficiency and low cost large-area uniformity Film preparation with excellent conductivity and compatibility.
Patent Information
- Application Number
- CN202210788979.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-06
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-07-06
AI Technical Summary
In the prior art, the method for preparing a conductive silver nanowire film has problems such as difficult to accurately control the film thickness, poor adhesion between the film layer and the substrate, low manual brushing efficiency, high labor intensity and difficult to achieve standardized production.
Using nylon filter cloth as a brush coating tool, by adjusting the combination of filter cloth holes and solution viscosity, controlling the solution outflow speed, achieving uniform coating of silver nanowire solution, and achieving automation through the combination of syringe pump and movable platform. The brushing process ensures uniformity and efficient preparation of the film.
Achieve large-area, uniform and low-cost conductive film preparation of silver nanowires, with high efficiency, low material loss, low cost and good compatibility, excellent film surface flatness and conductive properties, suitable for different types of substrates, including non- Planar substrate.
Smart Images

Figure CN115148417B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of silver nanowire conductive films, and in particular to a method for preparing the silver nanowire conductive film by brushing with filter cloth. Background Art
[0002] Conductive films are widely used in optoelectronics and microelectronics, such as information display, information storage, energy conversion, bioelectronics and other devices. Silver nanowires (Ag NWs) are a very promising flexible conductive material because they exhibit better optical transmittance and surface resistance than other conductive materials. Silver nanowires have high thermal conductivity and electrical conductivity, and their uses include transparent conductive films, biosensors and surface enhanced Raman scattering. At present, the main types of preparation of silver nanowire conductive films include spin coating, brush coating, rod coating, drop coating, vacuum filtration, dip coating, inkjet printing, and pulling.
[0003] In the preparation of large-area silver nanowire conductive films, rod coating is a simple and easy process. Specifically, a Meyer rod is used as a coating tool to spread the silver nanowire solution on the substrate to form a film. Using different types of Meyer rods can change the film thickness. However, in the process of preparing silver nanowire films by rod coating, the Meyer rod has no contact with the substrate, and the solution is pulled into film by the shear force of the liquid. Therefore, there are problems such as difficulty in accurately controlling the film thickness and poor adhesion between the film layer and the substrate.
[0004] The brush coating method is another simple and easy preparation method. A brush or writing brush is used to dip a silver nanowire solution and brush it on the surface of the substrate to form a uniform silver nanowire film. The brush coating method has low requirements for equipment, high utilization rate of the silver nanowire solution, and has the advantages of low cost and high performance. However, since the amount of silver nanowires stored in the bristles during the dipping process is difficult to control, and it is difficult to achieve continuous replenishment of the solution during the brush coating process, the uniformity of the large-area silver nanowire conductive film cannot be guaranteed. For example, the patent with publication number CN105355262B provides a transparent conductive film and a preparation method thereof. By using a brush coating element that has been carboxylated with a surfactant, the silver nanowire slurry is brushed on a transparent substrate, which ensures that the silver nanowires are uniformly and directional arranged on the transparent substrate to a certain extent, and are firmly bonded to the transparent substrate. After drying, a transparent conductive film with high light transmittance and good conductivity is obtained. However, its film preparation process is still based on manual brush coating. The manual brush coating process is inefficient, consumes man-hours, has high labor intensity, and has large performance differences between different electrode products, making it difficult to achieve standardized production;
[0005] Therefore, the current prior art lacks a low-cost method for preparing silver nanofilms that can be sustainably automated and produced while ensuring good performance of the electrode film. Summary of the invention
[0006] In view of the shortcomings of the existing silver nanowire film preparation technologies such as rod coating or brush coating, the present invention provides a method for preparing a silver nanowire conductive film, folding a filter cloth material such as a nylon filter cloth in half as a coating tool, using a silver nanowire mixed solution with a certain viscosity, and using the mutual coordination between the filter cloth holes and the solution viscosity to control the outflow rate of the solution, so that the silver nanowire solution is evenly coated on the substrate surface, aiming to solve the defects of preparing a silver nanowire conductive film using conventional scraping and brush coating methods. The preparation method of the present invention realizes simple, low-cost, large-area, and relatively uniform square resistance film preparation through the selection of solvents and the optimization of preparation conditions.
[0007] To achieve the above object, the present invention adopts the following technical solution:
[0008] A method for preparing a silver nanowire conductive film comprises the following steps:
[0009] The silver nanowire stock solution and the dispersion liquid containing silver nanowires are mixed evenly to prepare a silver nanowire / dispersion liquid material mixed solution, hereinafter referred to as the mixed solution, wherein the concentration range of the silver nanowires in the mixed solution is 2-10 mg / ml, and the diameter range of the silver nanowires is 30-90 nm; the dispersion liquid is prepared by dissolving the dispersion material in deionized water and fully dissolving it, and the concentration range of the prepared dispersion liquid is 3-7 mg / ml; the dispersion material is any one of hydroxypropyl methylcellulose (HPMC), nitrocellulose plastic, cellulose acetate butyrate, cellulose acetate, methyl cellulose, and polyaniline;
[0010] Clean the substrate, which includes a glass sheet, a PET flexible substrate and a paper material; cut a filter cloth with a width greater than the substrate, wherein the filter pore size of the filter cloth is 50-150 μm;
[0011] After the syringe absorbs a certain amount of mixed solution, it is fixed on the syringe pump. The syringe is used to store the silver nanowire mixed solution. The needle contacts the silver nanowire solution on the filter cloth. The syringe pump is used to push the syringe to supply the solution. The motor movement speed of the syringe pump is controlled by the circuit board to determine the amount of liquid discharged from the syringe. The movement time of the syringe pump is set by the size of the substrate.
[0012] The filter cloth is folded in half and sealed and fixed, and then the outer side of the seal is fixed on the upper module of the movable platform. The upper module is fixed during the brushing process, and the needle of the syringe is inserted into the middle position of the folded filter cloth, and it is necessary to ensure that the filter cloth is flat in the horizontal and vertical directions after being folded in half;
[0013] Slowly move the filter cloth until it contacts the substrate horizontally and then lower it 1-2 mm. Place the substrate on the lower module of the movable platform. Control the movement of the substrate through the lower module so that the filter cloth is brushed over the substrate at a uniform speed. After brushing, place the silver nanowire conductive film on a hot stage for annealing.
[0014] Preferably, a silver nanowire stock solution is weighed as a solute, wherein the mass fraction of the stock solution is 1-5 wt %.
[0015] Preferably, the filter cloth is a nylon filter cloth, the length of the filter cloth is 4-6 cm, and the width is 1-2 cm greater than the width of the substrate;
[0016] Preferably, the process of dissolving the dispersed material in deionized water and fully dissolving the dispersed material comprises: weighing the dispersed material and dissolving it in deionized water, sealing the dispersed material and stirring it with a magnetic stirrer for more than six hours to fully dissolve it, thereby obtaining a dispersion.
[0017] Preferably, the dispersing material is hydroxypropyl methylcellulose HPMC, which not only reduces the agglomeration of silver nanowires in the mixed solution, but also forms an HPMC protective layer on the surface of the finally prepared silver nanowire film to reduce the roughness of the film surface.
[0018] Preferably, the substrate cleaning process comprises: ultrasonically cleaning the substrate for at least 15 minutes, drying it with N2 and performing hydrophilic treatment in a plasma cleaning machine; further preferably, the ultrasonic cleaning is performed using deionized water, ethanol and isopropanol in sequence;
[0019] Preferably, a certain amount of silver nanowires is pre-dropped at the folded position of the filter cloth, and the pre-dropping is for draining the mixed solution so that the solution is evenly spread on the substrate along the pre-dropping direction; the volume of the pre-dropped silver nanowire mixed solution should ensure that the silver nanowire mixed solution does not drip from the filter cloth;
[0020] Preferably, the moving speed of the lower module of the movable platform is 20 cm / min, and the movement speed of the syringe pump pushing the syringe is 20-50 mm / s; the automatic brushing of silver nanowire conductive films of different thicknesses is achieved by the moving speed of the lower module; accordingly, the movement speed of the syringe pump pushing the syringe is set to 20-50 mm / s, and the specification of the syringe is 1-5 ml;
[0021] Preferably, the final silver nanowire conductive film can be obtained by annealing on a hot plate at 100-120° C. for 5-10 minutes.
[0022] The present invention can control the viscosity of the solution by adding dispersing materials of different masses. The specific dissolution method is as follows: the required water is heated to above 85°C, and the dispersing materials are gradually added under continuous stirring. The cellulose is gradually dispersed in the water and swells into a slurry. The solution is stirred and cooled until it becomes transparent, indicating that the solution is completely dissolved.
[0023] Beneficial effects of the present invention:
[0024] The preparation method of the silver nanowire conductive film provided by the present invention selects filter cloth as a brushing tool, controls the viscosity of the solution by means of a dispersing material, utilizes its excellent dispersing and glue-retaining capabilities, and cooperates with the soft characteristics of the filter cloth, so that the silver nanowire solution can form a good contact with the substrate, and is suitable for various substrates, and can also generate a strong shear force during the brushing process; in addition, the filter holes on the filter cloth can filter the agglomerates in the silver nanowire solution, so that the silver nanowire conductive film obtained by brushing has better flatness and uniformity, and the film surface roughness is lower;
[0025] The present invention provides a method for preparing a silver nanowire conductive film, wherein the filter cloth is preferably a nylon filter cloth, which has the best softness; the silver nanowire network simply brushed shows a smooth surface morphology and a good conductive network, and the filter cloth brushing method provided by the present invention itself is a simple and cost-effective method for preparing a silver nanowire conductive film, which has the advantages of low material loss, ultra-low cost and vacuum-free processing, high manufacturability and good compatibility.
[0026] The preparation method of the present invention is simple and efficient to operate, has low requirements on equipment, and is easy to implement; the present invention prepares a conductive film with a short preparation cycle, simple preparation steps, high material utilization, low preparation cost, and good film repeatability; the silver nanowire film prepared by the present invention does not have agglomeration phenomenon, and the film can maintain good morphology and performance; the present invention can realize large-area preparation and is compatible with different types of substrates, including non-planar substrates; the conductive film prepared by the present invention has good photoelectric performance and maintains uniform square resistance over a large area. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 Schematic diagram of the coating method of the silver nanowire conductive film in an embodiment of the present invention;
[0028] Figure 2 It is a diagram of each position of the four-probe square resistance instrument test described in Test Example 1 of the specific implementation method;
[0029] Figure 3 This is a physical comparison diagram of the silver nanowire conductive film prepared on the glass substrate and the glass substrate in Example 1 of the present invention;
[0030] Figure 4This is a physical picture of the silver nanowire conductive film prepared in Examples 1-4 and Comparative Examples 1-2 of the present invention. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific implementation methods.
[0032] Example 1
[0033] like Figure 1 As shown, the preparation method of the silver nanowire conductive film according to the present invention is implemented as follows:
[0034] Step S1, weighing 0.4 g of silver nanowire stock solution, the silver nanowire stock solution was purchased from Zhejiang Kechuang Material Technology Co., Ltd., model AW045, wherein the mass of the silver nanowire solute is 4 mg;
[0035] Step S2, weighing 40 mg of HPMC polymer and dissolving it in 8 ml of deionized water to obtain an HPMC dispersion with a concentration of 5 mg / ml; taking 0.6 ml of the HPMC solution and adding it to the silver nanowire stock solution in step S1 to obtain a silver nanowire mixed solution containing silver nanowires and HPMC, at which point the concentration of the silver nanowire mixed solution is 4 mg / ml;
[0036] Step S3, using a syringe 5 to draw 0.5 ml of the silver nanowire mixed solution and fix it on the syringe pump 1;
[0037] Step S4, cutting a filter cloth 4 with a size of 6 cm × 6 cm and a pore size of 150 μm as a brushing tool; the filter cloth is folded in half and sealed and fixed, and then the outer side of the seal is fixed on the upper module 6 of the movable platform, and the upper module 6 is fixed during the brushing process, and the needle of the syringe is inserted into the middle position of the folded filter cloth, and it is necessary to ensure that the filter cloth is flat in the horizontal and vertical directions after being folded in half;
[0038] Step S5, a glass substrate 3 with a size of 2 cm×8 cm is ultrasonically cleaned for 15 minutes using deionized water, ethanol, and isopropanol in sequence, and after being subjected to plasma cleaning treatment to improve hydrophilicity, is placed on the lower module 2 of the 3D movable platform;
[0039] Step S6, pre-dropping 30 μl of the silver nanowire mixed solution on the filter cloth, and adjusting the height of the filter cloth 4 so that it contacts the glass substrate 3;
[0040] Step S7, start the movable platform and the syringe pump 1 of the 3D printer, control the module 2 below the platform to move in the Y-axis direction at a moving speed of 20 cm / min, drive the glass substrate 3 to move, and realize automatic scraping;
[0041] Step S8, placing the silver nanowire conductive film on a hot plate at a temperature of 120° C. and annealing for 10 minutes to form a film.
[0042] like Figure 3 , which is a physical comparison diagram of the silver nanowire conductive film prepared on the glass substrate in Example 1 of the present invention and the glass substrate.
[0043] Example 2
[0044] The method for preparing the conductive film in Example 2 is the same as that in Example 1, except that the glass substrate used in step S5 has a specification of 5 cm×5 cm, and 50 μl of the silver nanowire mixed solution is pre-dropped in step S6.
[0045] The testing method is the same as that in Example 1. After testing, the average square resistance of the film is 28.45Ω / sq, and the transmittance at 550nm is 85.92%.
[0046] Example 3
[0047] The preparation method of the conductive film in Example 3 is the same as that in Example 1, except that the substrate used in step S5 is a PET film. The testing method is the same as that in Example 1. After testing, the average square resistance of the film is 27.94Ω / sq, and the transmittance at 550nm is 79.18%.
[0048] Example 4
[0049] The preparation method of the conductive film in Example 4 is the same as that in Example 1, except that the filter pore size of the filter cloth used in step S4 is 50 μm, and the substrate used in step 5) is A4 paper; the testing method is the same as that in Example 1, and after testing, the average square resistance of the film is 6.01Ω / sq,
[0050] Comparative Example 1
[0051] The preparation method of the conductive film in Comparative Example 1 is the same as that in Example 1, except that HPMC is not added in step S2, and only 0.6 ml of ethanol is weighed and mixed into the silver nanowire stock solution to obtain a silver nanowire solution.
[0052] The testing method is the same as that in Example 1. After testing, the average square resistance of the film is 58.1Ω / sq, and the transmittance at 550nm is 87.18%.
[0053] Comparative Example 2
[0054] The preparation method of the conductive film in Comparative Example 2 is the same as that in Example 1, except that the amount of HPMC used in step S2 is different. The details are as follows:
[0055] 120 mg of HPMC polymer was weighed and dissolved in 8 ml of water to obtain a silver nanowire solution with a concentration of 15 mg / ml; the solution obtained by mixing HPMC with silver nanowires at this concentration could not be brushed on the substrate to obtain a uniform film. The test method was the same as that in Example 1. After testing, the average square resistance of the film was 6.86 Ω / sq, and the transmittance at 550 nm was 69.05%.
[0056] Comparative Example 3
[0057] Comparative Example 3 is the same as the conductive film preparation method in Example 1, except that the filter cloth used in step S3 has a filter hole size of 38 μm. With this filter cloth, the silver nanowires cannot penetrate smoothly through the filter holes, and the surface of the prepared silver nanowire conductive film is unevenly distributed with obvious scratches. The test method is the same as that in Example 1. After testing, the average square resistance of the film is 85.68Ω / sq, and the transmittance at 550nm is 89.13%.
[0058] Test Example 1
[0059] like Figure 4 As shown in FIG. 1 , the silver nanowire conductive films prepared in Examples 1-4 and Comparative Examples 1-3 of the present invention are physically shown. The silver nanowire conductive films prepared in all the embodiments and comparative examples are tested using a handheld four-probe square resistance tester. Four probes are directly placed flat on the prepared silver nanowire conductive films. The uniformity of square resistance is tested by moving the positions of the four probes. A total of 8 positions are selected for each test. The specific positions are as follows: Figure 2 As shown, the test results are shown in Table 1. After calculation, the average square resistance of the film is 27.15Ω / sq. Use a UV-visible spectrophotometer to test the transmittance of the conductive film. Let the instrument preheat for 15 minutes. After the instrument self-check is completed, open the software to perform full-scale calibration with a clean glass substrate, set the test wavelength to 300-800nm, and finally select the transmittance curve to start the test. After testing, the average square resistance of the film is 27.15Ω / sq, and the transmittance at 550nm is 85.13%.
[0060] Table 1 is a summary of the multi-point square resistance test of the silver nanowire conductive films prepared in each embodiment and comparative example
[0061]
[0062] Table 2 is a summary of the average square resistance and transmittance at 550 nm of the silver nanowire conductive films prepared in various embodiments and comparative examples.
[0063]
Claims
1. A method for preparing a silver nanowire conductive film, characterized in that: The specific steps include: The silver nanowire stock solution and the dispersion liquid containing silver nanowires are mixed evenly to prepare a silver nanowire / dispersion liquid material mixed solution, hereinafter referred to as the mixed solution, wherein the concentration range of the silver nanowires in the mixed solution is 2-10 mg / ml, and the diameter range of the silver nanowires is 30-90 nm; the dispersion liquid is prepared by dissolving the dispersion material in deionized water and fully dissolving it, and the concentration range of the prepared dispersion liquid is 3-7 mg / ml; the dispersion material is any one of hydroxypropyl methylcellulose (HPMC), nitrocellulose plastic, cellulose acetate butyrate, cellulose acetate, methyl cellulose, and polyaniline; Clean the substrate, which includes a glass sheet, a PET flexible substrate and a paper material; cut a filter cloth having a width greater than that of the substrate, wherein the filter pore size of the filter cloth is 50-150 μm; After the syringe absorbs a certain amount of mixed solution, it is fixed on the syringe pump. The syringe is used to store the silver nanowire mixed solution. The needle contacts the silver nanowire solution on the filter cloth. The syringe pump is used to push the syringe to supply the solution. The motor movement speed of the syringe pump is controlled by the circuit board to determine the amount of liquid discharged from the syringe. The movement time of the syringe pump is set by the size of the substrate. The filter cloth is folded in half and sealed and fixed, and then the outer side of the seal is fixed on the upper module of the movable platform. The upper module is fixed during the brushing process, and the needle of the syringe is inserted into the middle position of the folded filter cloth, and it is necessary to ensure that the filter cloth is flat in the horizontal and vertical directions after being folded in half; Slowly move the filter cloth until it contacts the substrate horizontally and then lower it 1-2 mm. Place the substrate on the lower module of the movable platform. Control the movement of the substrate through the lower module so that the filter cloth is brushed over the substrate at a uniform speed. After brushing, place the silver nanowire conductive film on a hot stage for annealing.
2. The method for preparing a silver nanowire conductive film according to claim 1, characterized in that: The silver nanowire stock solution is weighed as a solute, wherein the mass fraction of the stock solution is 1-5wt%.
3. The method for preparing a silver nanowire conductive film according to claim 1, characterized in that: The filter cloth is a nylon filter cloth.
4. The method for preparing a silver nanowire conductive film according to claim 1, characterized in that: The length of the filter cloth is 4-6 cm, and the width is 1-2 cm greater than the width of the substrate.
5. The method for preparing a silver nanowire conductive film according to claim 1, characterized in that: The process of dissolving the dispersed material in deionized water and fully dissolving the dispersed material comprises: weighing the dispersed material and dissolving it in deionized water, sealing it and stirring it with a magnetic device for more than six hours to fully dissolve it and obtain a dispersed liquid.
6. The method for preparing a silver nanowire conductive film according to claim 1, characterized in that: The substrate cleaning process includes: ultrasonically cleaning the substrate for at least 15 minutes, drying it with N2 and performing hydrophilic treatment in a plasma cleaning machine.
7. The method for preparing a silver nanowire conductive film according to claim 6, characterized in that: The ultrasonic cleaning is performed using deionized water, ethanol and isopropanol in sequence.
8. The method for preparing a silver nanowire conductive film according to claim 1, characterized in that: A certain amount of silver nanowires is pre-dropped at the folding position of the filter cloth, and the volume of the pre-dropped silver nanowire mixed solution should ensure that the silver nanowire mixed solution does not drip from the filter cloth.
9. The method for preparing a silver nanowire conductive film according to claim 1, characterized in that: The moving speed of the lower module of the movable platform is 20cm / min; the moving speed of the lower module is used to realize the automatic brushing of silver nanowire conductive films of different thicknesses; accordingly, the movement speed of the injection pump pushing the syringe is set to 20-50mm / s, and the specification of the syringe is 1-5ml.