Preparation method of nickel-molybdenum-iron water electrolysis catalyst and the obtained product and application
The nickel-molybdenum iron electrolytic water catalyst prepared by the thermal shock method solves the problem of insufficient stability of nickel-based catalysts in seawater and achieves efficient and stable electrocatalytic oxygen evolution reaction in seawater. It has low cost and high activity and is suitable for seawater. Electrolysis to produce hydrogen.
Patent Information
- Application Number
- CN202210782486.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-05
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-07-05
AI Technical Summary
In the process of electrolytic hydrogen production in seawater, the existing nickel-based catalysts have insufficient stability and resistance to corrosion by impurity ions, resulting in catalyst deactivation. The production cost of precious metal catalysts is high, which limits their large-scale application.
The thermal shock method is used to convert the precursors of iron, molybdenum and nickel into a nickel-molybdenum-iron electrolytic water catalyst. Through thermal shock treatment on the carbon cloth substrate, a catalyst with high activity and stability is formed, which is suitable for simulating seawater and alkalinity. Electrocatalytic oxygen evolution reaction in seawater.
The prepared nickel-molybdenum iron electrolysis water catalyst has high electrocatalytic activity and long-term stability under alkaline conditions, and can maintain stability for more than 1950 hours in simulated seawater and more than 550 hours in alkaline seawater. , the cost is lower than traditional precious metal catalysts, and it is not prone to peeling.
Smart Images

Figure CN115161690B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method of a nickel-molybdenum-iron water electrolysis catalyst and a product obtained therefrom, and also relates to application of the nickel-molybdenum-iron water electrolysis catalyst in electrocatalytic seawater decomposition to produce hydrogen, and belongs to the technical field of inorganic functional materials. Background Art
[0002] Since John Bockris coined the term hydrogen economy in the 1970s, hydrogen energy has been considered one of the cleanest and most promising energy utilization models. There are three main synthetic pathways for preparing hydrogen fuel: methane steam reforming, coal gasification, and water electrolysis. In the process of methane steam reforming and coal gasification, methane or coal reacts with water vapor at high temperature to produce hydrogen and carbon dioxide at the same time. Although these two methods account for more than 95% of global hydrogen fuel production, it is obvious that these two methods consume a large amount of fossil fuels and cause environmental pollution problems such as carbon emissions. In contrast, water splitting to produce hydrogen, as the reverse reaction of hydrogen combustion, uses water as the only raw material and realizes a closed hydrogen cycle with zero carbon emissions. Therefore, it is considered to be the greenest and most sustainable method. The current total hydrogen consumption market is about US$115 billion and is expected to quickly reach US$155 billion by 2022, indicating that people's interest in hydrogen as an energy carrier is growing day by day. (Adv. Mater. 2021, 33, 2007100)
[0003] For electrocatalytic water splitting, the oxygen evolution reaction (OER) at the anode end is the bottleneck of the technology due to its slow kinetics caused by the proton-coupled multi-electron transfer step. In order to accelerate this process, a highly active catalyst is required. Currently, the commonly used oxygen evolution catalysts are iridium-based and ruthenium-based catalysts, but the stability problems caused by long-term catalysis and the high production cost restrict their large-scale application. With the continuous development, many materials in non-precious metal catalysts have a low kinetics of 10 mA cm -2 At current density, the catalytic activity has exceeded that of precious metal iridium-based ruthenium-based catalysts. For example, nickel-based catalytic materials, so far, composite catalysts containing active nickel-based compounds and other functional additives have attracted increasing attention due to their advantages such as enhanced reaction kinetics and improved structure / performance stability (Chem. Eur. J. 2019, 25, 703–713).
[0004] Although the activity and stability of nickel-based catalysts in alkaline media have been studied in depth, there are still limited reports on the development of nickel-based catalysts in seawater, especially on effectively improving stability. Seawater accounts for 96.5% of the total water reserves on Earth, so it is an almost unlimited resource. However, compared with fresh water, seawater has a complex composition and contains a large number of impurity ions and microorganisms that seriously interfere with the normal electrocatalytic process. According to existing literature reports, among these impurity ions, chloride ions, magnesium ions, and calcium ions have the greatest impact on catalytic materials (ACS Energy Lett. 4, 933–942 (2019).). The chlorine evolution reaction (CLER) of chloride ions at low pH and the hypochlorite formation reaction (HCFR) in high pH solutions are the main OER competitive reactions. At the same time, the presence of chloride ions will also destroy the metal passivation film. Magnesium ions and calcium ions will form insoluble precipitates on the catalyst surface, thereby deactivating the catalyst (Energy Environ. Sci., 2020, 13, 3253—3268). Therefore, in the context of many challenges faced by seawater electrolysis and the increasing scarcity of freshwater resources, it is necessary to develop catalysts for hydrogen production by electrolysis in seawater. Summary of the invention
[0005] In view of the shortcomings of the prior art, the present invention provides a method for preparing a nickel-molybdenum-iron water electrolysis catalyst and the resulting product. The method uses a thermal shock method (TSS technology) to convert a metal precursor into a metal catalyst. The method has simple operation, short time consumption and a rapid preparation process. The resulting catalyst has excellent stability in both simulated seawater and alkaline seawater, and can exert a lasting catalytic effect.
[0006] The specific technical solutions of the present invention are as follows:
[0007] A method for preparing a nickel-molybdenum-iron water electrolysis catalyst comprises the following steps:
[0008] (1) grinding an iron source, a molybdenum source, a nickel source, and urea in the presence of a solvent to obtain a precursor paste;
[0009] (2) attaching the precursor paste to the substrate and drying it naturally;
[0010] (3) placing the substrate with the attached precursor on the carbon cloth, applying electricity to both ends of the carbon cloth, and subjecting the substrate with the attached precursor to at least one thermal shock until the precursor is completely converted into the corresponding metal, thereby obtaining a nickel-molybdenum-iron water electrolysis catalyst.
[0011] Furthermore, the molar ratio of the iron source, the molybdenum source, the nickel source, the urea and the solvent is 5:2:6:50~60:75~85.
[0012] Furthermore, the iron source is ferric chloride, the molybdenum source is ammonium molybdate, the nickel source is nickel chloride, and the solvent is anhydrous ethanol.
[0013] Further, the substrate is a nickel mesh, nickel foam or nickel-molybdenum foam. When the substrate is a nickel mesh, the mesh number of the nickel mesh is generally 40-100 meshes.
[0014] Furthermore, the grinding is performed at room temperature. After grinding, the average particle size of the particles in the paste is less than 150 microns.
[0015] Furthermore, the substrate is cleaned before use to remove impurities on the surface. The cleaning step may be: ultrasonically treating the substrate with hydrochloric acid, acetone, ethanol, and water in sequence.
[0016] Furthermore, the precursor paste can be attached to the substrate by coating, dipping, etc. In a specific embodiment of the present invention, the substrate is dipped into the precursor paste for 3-5 minutes to allow the precursor paste to fully adhere to the substrate.
[0017] Furthermore, the thermal shock is performed under gas protection, and the protective gas is argon, helium or a mixture of the two.
[0018] Further, during the thermal shock, when the substrate is a nickel mesh, the voltage is set to 5-20V, and when the substrate is a nickel foam or a nickel-molybdenum foam, the voltage is set to 5-10V. The voltage is provided by a DC regulated power supply, and the voltage can make the precursor obtain an instantaneous high temperature. The time of each thermal shock is 0.1-4 seconds. Preferably, the voltage of each thermal shock is set to 10V, and the time of each shock is 2-4s.
[0019] Furthermore, the number of thermal shocks may be 1, 2, 3, 4, etc., as long as the precursor is completely reacted.
[0020] The present invention also provides a nickel-molybdenum-iron water electrolysis catalyst obtained according to the above method, wherein the catalyst structure is composed of a nickel mesh substrate and a material layer containing a nickel-molybdenum-iron mixed phase attached to the substrate. Experimental verification shows that the nickel-molybdenum-iron water electrolysis catalyst has a high electrocatalytic oxygen evolution activity under alkaline conditions, and can maintain the stability of the catalytic performance for a long time in simulated seawater and alkaline seawater, and has excellent stability.
[0021] Furthermore, based on the excellent performance of the nickel-molybdenum-iron water electrolysis catalyst of the present invention, the present invention also provides the application of the nickel-molybdenum-iron catalyst in the field of water splitting to produce hydrogen and seawater splitting to produce hydrogen, and the splitting of water or seawater to produce hydrogen is carried out under alkaline conditions.
[0022] The present invention proposes for the first time a method for rapidly and efficiently preparing a highly active and highly stable nickel-molybdenum-iron water electrolysis catalyst. Compared with the hydrothermal synthesis method and the electrochemical deposition method reported in the prior art, the present invention has the following beneficial effects:
[0023] 1. The thermal shock method of the present invention has a simple process flow, is easy to operate, and has a rapid preparation process. The precursor can be heated to the temperature required for the reaction (700-1000°C) within a few seconds, and then quickly cooled. A reactive material layer can be quickly generated on the surface of the substrate. The prepared samples have good properties and high repeatability.
[0024] 2. The synthesis conditions of the present invention are highly controllable, the main raw materials for preparation are widely available, and the cost has significant advantages over traditional iridium and ruthenium-based precious metal catalysts.
[0025] 3. Compared with powdered catalysts, the nickel-based catalyst obtained in the present invention integrates the fluid electrode and the catalyst into one, and will not peel off in a working environment.
[0026] 4. The catalyst of the present invention can be directly used as the anode for water electrolysis and has high electrocatalytic oxygen evolution activity and stability under alkaline conditions: the current density is 10 mA cm -2 When the overpotential is optimal, only 201 mV is required.
[0027] 5. The catalyst of the present invention was tested in simulated seawater (1 M KOH + 0.5 M NaCl), 100 mA cm -2 The stability under optimal conditions can be maintained for more than 1950 hours.
[0028] 6. The catalyst of the present invention is in alkaline seawater (1 M KOH + seawater) at 100 mA cm -2 The stability under the optimal conditions can be maintained for more than 550 hours. It can be seen that the catalyst has the performance of long-term, stable and efficient electrocatalytic water splitting to produce hydrogen in alkaline seawater, and has potential commercial value.
[0029] 7. The catalyst of the present invention has good catalytic activity and excellent catalytic stability in both simulated seawater and alkaline seawater, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 : X-ray diffraction (XRD) pattern of NiMoFe-NM (NM is the abbreviation of Nickel Mesh) obtained in Example 1.
[0031] Figure 2 : Raman spectrum of NiMoFe-NM obtained in Example 1.
[0032] Figure 3 : Scanning electron microscope (SEM) photograph of the pure nickel mesh substrate in Example 1.
[0033] Figure 4: Scanning electron microscope (SEM) photograph of the NiMoFe-NM sample in Example 1.
[0034] Figure 5 : Transmission electron microscope (TEM) photograph of the NiMoFe-NM sample in Example 1.
[0035] Figure 6 : Polarization curves of the NiMoFe-NM sample obtained in Example 1, the NiMo-NM sample obtained in Comparative Example 1, and the NiFe-NM sample obtained in Comparative Example 2 for water splitting and oxygen extraction in an alkaline electrolyte (1 M KOH).
[0036] Figure 7 : Stability curve of oxygen released by water splitting of the NiMoFe-NM sample obtained in Example 1 in simulated seawater (1 M KOH+0.5 M NaCl).
[0037] Figure 8 : Stability curve of oxygen released by hydrolysis of the NiMoFe-NM sample obtained in Example 1 in alkaline seawater (1 M KOH+seawater). DETAILED DESCRIPTION
[0038] The present invention is further described below by way of examples and in conjunction with the accompanying drawings, but the protection scope of the present invention is not limited to the following examples. It is clear to those skilled in the art that changes or adjustments can be made to the present invention without departing from the spirit and scope of the present invention, and these changes or adjustments are also included in the protection scope of the present invention.
[0039] Example 1
[0040] Preparation of NiMoFe-NM (NM is the abbreviation of Nickel Mesh) catalyst:
[0041] (1) Cut the nickel mesh into strips with a length and width of 1 cm*3 cm, and ultrasonically clean them with 0.5 M HCL, acetone, ethanol, and water for 10 min respectively, and then dry them for later use;
[0042] (2) Weigh 0.143 g (0.6 mmol) of nickel chloride hexahydrate, 0.247 g (0.2 mmol) of ammonium molybdate, 0.0812 g (0.5 mmol) of anhydrous ferric chloride, and 0.36 g (6 mmol) of urea into a mortar and grind them while adding about 0.5 ml (8 mmol) of anhydrous ethanol with a dropper. Continue grinding until the mixture becomes a paste.
[0043] (3) using a brush to evenly apply the paste obtained in step (2) onto the nickel mesh cleaned and dried in step (1), or soaking the nickel mesh obtained in step (1) in the paste to fully immerse it (immersion time is 3-5 min), and then naturally drying the nickel mesh covered with the slurry for later use;
[0044] (4) Under an inert protective atmosphere, the nickel mesh loaded with the dried slurry obtained in step (3) was placed on a 4 cm*4 cm carbon cloth, and the electrode clamps of a DC regulated power supply were clamped at both ends of the carbon cloth. The power supply voltage was set to 10 V, and thermal shock was performed 3 times, each time for 2-3 seconds;
[0045] (5) The sample obtained in step (4) was washed twice with ethanol and water respectively to obtain a NiMoFe-NM catalyst.
[0046] Figure 1 The XRD spectrum of the NiMoFe-NM material (NM is the abbreviation of Nickel Mesh) prepared by the thermal shock method in Example 1 is shown. The position in the spectrum is attributed to the nickel mesh (PDF#25-2865).
[0047] Figure 2 Shown is the Raman spectrum of the NiMoFe-NM material prepared by the thermal shock method in Example 1. The chemical structure of the NiMoFe-NM material includes locally disordered Mo-O bonds, OO bonds and Ni-O-Fe states, OO and Ni-O-Fe vibrations, indicating the presence of a mixed nickel-iron (oxygen) hydroxide structure, while the characteristic Mo-O vibrations of different phases are attributed to NiMoO4.
[0048] Figure 3 Shown is a SEM image of the nickel mesh substrate used in Example 1. From the image, it can be seen that the surface of the nickel mesh is smooth and has no attachments.
[0049] Figure 4 The SEM images of the surface (a) and cross section (b) of the NiMoFe-NM material obtained in Example 1 are shown respectively. Figure 4 (a) It can be seen that after the thermal shock, a layer of material composed of a mixed phase of nickel, molybdenum and iron grows uniformly on the nickel mesh substrate. Figure 4 (b) shows that the thickness of the material layer is about 0.9-2.5 microns.
[0050] Figure 5 The TEM image of the NiMoFe-NM material obtained in Example 1 is shown. It can be seen from the figure that the NiMoFe-NM material has both amorphous and crystalline structures. By measuring the different lattice fringe spacings, it is found that the crystalline structure is mainly a mixed nickel iron (oxygen) hydroxide, which is consistent with Figure 2 (Raman spectrum) The results are consistent.
[0051] The NiMoFe-NM catalyst was used as the working electrode, the mercury / mercury oxide electrode was used as the reference electrode, the platinum wire was used as the counter electrode, and 1 M KOH was used as the electrolyte. The current density reached 10 mA cm -2 When the overpotential is 241 mV, the current density is 100 mA cm -2 The required overpotential is 298 mV. It should be noted that in the electrocatalytic test, all potentials obtained with mercury / mercury oxide electrode as reference electrode are converted into reversible hydrogen electrode potential in the property diagram, and the external power supply is the main battery of the electrochemical workstation.
[0052] Example 2
[0053] The same as Example 1, except that the nickel mesh was replaced with nickel foam (thickness 0.3 mm), to prepare a NiMoFe-NF catalyst (NF is the abbreviation of nickel foam). The overpotential was tested in the same manner as Example 1. The obtained catalyst had a current density of 10 mA cm in 1 M KOH. -2 The required overpotential is 235 mV.
[0054] Example 3
[0055] The same as Example 1, except that the nickel mesh was replaced with nickel molybdenum foam (thickness of 0.3 mm), to prepare NiMoFe-NMF catalyst (NMF is the abbreviation of nickel molybdenum foam). The overpotential was tested in the same manner as Example 1. The obtained catalyst had a current density of 10 mA cm in 1 M KOH. -2 The required overpotential is 201 mV.
[0056] Example 4
[0057] The same as Example 1, except that the iron source was changed to 0.5 mmol of ferric chloride hexahydrate. The overpotential was tested in the same manner as Example 1. The obtained catalyst had a current density of 10 mA cm in 1 M KOH. -2 The required overpotential is 252 mV.
[0058] Example 5
[0059] The same as Example 1, except that ammonium molybdate was replaced by 0.2 mmol sodium molybdate. The overpotential was tested in the same manner as Example 1. The obtained catalyst had a current density of 10 mA cm in 1 M KOH. -2 The required overpotential is 263 mV.
[0060] Example 6
[0061] The same as Example 1, except that the thermal shock voltage was changed to 20 V. The overpotential was tested in the same manner as Example 1. The obtained catalyst had a current density of 10 mA cm in 1 M KOH. -2 The required overpotential is 249mV.
[0062] Example 7
[0063] The same as Example 1, except that the number of thermal shocks was changed to 1. The overpotential was tested in the same manner as Example 1. The obtained catalyst had a current density of 10 mA cm in 1 M KOH. -2 The required overpotential is 314mV.
[0064] Comparative Example 1
[0065] The same method as in Example 1 was used, except that anhydrous ferric chloride was not added to obtain a NiMo-NM catalyst. The overpotential was tested in the same manner as in Example 1. The current density of the obtained catalyst in 1 M KOH reached 10 mA cm -2 When the overpotential is 269 mV, the current density is 100 mA cm -2 The required overpotential is 365 mV.
[0066] Comparative Example 2
[0067] The same as Example 1, except that ammonium molybdate was not added, to obtain a NiFe-NM catalyst. The overpotential was tested in the same manner as Example 1. The current density of the obtained catalyst in 1 M KOH reached 10 mA cm -2 When the overpotential is 272 mV, the current density is 100 mA cm -2 The required overpotential is 345 mV.
[0068] Comparative Example 3
[0069] Preparation of NiMoFe-NM (hydrothermal) catalyst:
[0070] (1) Cut the nickel mesh into strips with a length and width of 1 cm*3 cm, and ultrasonically clean them with 0.5 M HCL, acetone, ethanol, and water for 10 min respectively, and then dry them for later use;
[0071] (2) Weigh 0.143 g (0.6 mmol) of nickel chloride hexahydrate, 0.247 g (0.2 mmol) of ammonium molybdate, 0.0812 g (0.5 mmol) of anhydrous ferric chloride, and 0.36 g (6 mmol) of urea, add 20 ml of ultrapure water, stir evenly, and place in a 50 ml polytetrafluoroethylene liner, and then place the nickel mesh treated in step (1);
[0072] (3) The polytetrafluoroethylene liner of step (2) is encapsulated in a stainless steel reactor, placed in an oven, and the temperature is set to 180°C and the time is set to 15 hours;
[0073] (4) The sample obtained in step (3) is washed and dried to obtain a NiMoFe-NM (hydrothermal) catalyst.
[0074] The overpotential was tested in the same manner as in Example 1. The obtained NiMoFe-NM (hydrothermal) catalyst had a current density of 10 mA cm in 1 M KOH. -2 When the overpotential is 268 mV, the current density is 100 mA cm -2 The required overpotential is 327mV.
[0075] Comparative Example 4
[0076] The same as Example 1, except that the protective atmosphere was changed to air. The overpotential was tested in the same manner as Example 1. The current density of the obtained catalyst in 1 M KOH reached 10 mA cm -2 When , the required overpotential is 289 mV respectively.
[0077] Performance Verification
[0078] The prepared catalysts were used to study the electrocatalytic oxygen evolution (OER) performance in a standard three-electrode electrolyzer, wherein the catalysts prepared in the examples and comparative examples were used as working electrodes in the electrolyzer, the mercury / mercury oxide electrode was used as a reference electrode, the platinum wire was used as a counter electrode, and the electrolyte was 1M KOH, simulated seawater (1 M KOH+0.5 M NaCl) or alkaline seawater (1 MKOH+seawater). It should be noted that all potentials obtained with the mercury / mercury oxide electrode as the reference electrode in the electrocatalytic test were converted into reversible hydrogen electrode potentials in the property diagram, and the external power supply was the main battery of the electrochemical workstation.
[0079] Figure 6 (a) shows the electrocatalytic oxygen evolution properties of the NiMoFe-NM material obtained in Example 1, the NiMo-NM material obtained in Comparative Example 1, the NiFe-NM material obtained in Comparative Example 2, and the pure nickel mesh (abbreviated as NM) without any treatment in 1 M KOH electrolyte; it can be seen from the figure that in 1 M KOH, the current density reaches 10 mA cm -2 The required overpotentials for the above materials (in the order mentioned) are 241 mV, 269 mV, 272 mV, and 317 mV, respectively. Figure 6(b) is a comparison of the electrocatalytic oxygen evolution properties of the NiMoFe-NM material obtained in Example 1 in 1 M KOH, simulated seawater (1 M KOH + 0.5 M NaCl) and alkaline seawater (1 M KOH + seawater). It can be seen from the figure that the current density of NiMoFe-NM in alkaline medium and simulated seawater is 10 mA cm -2 When the overpotential is 0.05, the overpotential is only 6 mV different, while in the alkaline seawater medium, the overpotential is 257 mV. The slight attenuation of activity may be attributed to the presence of microorganisms or bacteria in seawater. Figure 6 (b) It shows that the activity of NiMoFe-NM material remains good in the presence of chloride ions. Figure 6 (c) shows the activity comparison of NiMoFe-NM materials prepared by thermal shock (NiMoFe-NM obtained in Example 1) and hydrothermal method (NiMoFe-NM (hydrothermal) obtained in Comparative Example 3). It can be seen from the figure that the activity of NiMoFe-NM synthesized by thermal shock is significantly better than that of the sample synthesized by hydrothermal method, and the current density is 100 mA cm -2 When the overpotential difference is 49 mV, the overpotential difference is 49 mV. In addition, the activity of the nickel mesh after thermal shock is also improved compared with the nickel mesh without any treatment. These results show that the thermal shock method is the optimal method for synthesizing NiMoFe-NM catalysts. Figure 6 (d) shows the activity comparison of the samples obtained in Example 1, Example 2, and Example 3 respectively; it can be seen from the figure that the activities of the samples with nickel molybdenum foam and nickel foam as the substrate are slightly better than those of the samples with nickel mesh as the substrate. This is because nickel molybdenum foam and nickel foam are three-dimensional structures with a larger specific surface area, which makes it easy to expose more active sites.
[0080] Figure 7 The chronopotentiometry of the NiMoFe-NM material prepared by the thermal shock method in Example 1 in simulated seawater is shown. From the results, it can be seen that the catalyst has a 100 mA cm -2 At the current density, the stability can be maintained for more than 1950 hours, and the potential fluctuation is only 8.3%.
[0081] Figure 8 The chronopotentiometry of the NiMoFe-NM material prepared by the thermal shock method in Example 1 in alkaline seawater is shown. From the results, it can be seen that the catalyst has a high conductivity at 100 mA cm -2 At the highest current density, the stability can be maintained for more than 550 hours, and the potential fluctuation is only 3.2%. Figure 7 and Figure 8The results show that NiMoFe-NM still has excellent stability and resistance to chloride ion corrosion even in simulated seawater and alkaline seawater.
[0082] The catalysts of Examples 2-3 and Comparative Examples 1-2 were tested for stability in alkaline seawater using chronopotentiometry. When the current density was set to 100 mA cm -2 The results are as follows: the stability of the NiMoFe-NF catalyst obtained in Example 2 was maintained for 26 hours; the stability of the NiMoFe-NMF catalyst obtained in Example 3 was maintained for 21 hours, which shows that the stability of the catalyst is greatly improved when the substrate is a nickel mesh. The stability of the NiMo-NM catalyst obtained in Comparative Example 1 was maintained for 245 hours, and the stability of the NiFe-NM catalyst obtained in Comparative Example 2 was maintained for 187 hours, which is much lower than the catalyst of the present invention.
Claims
1. A method for preparing a nickel-molybdenum-iron water electrolysis catalyst, characterized in that The following steps are involved: (1) grinding an iron source, a molybdenum source, a nickel source, and urea in the presence of a solvent to obtain a precursor paste; (2) attaching the precursor paste to the substrate and drying it naturally; (3) placing the substrate with the attached precursor on the carbon cloth, applying electricity to both ends of the carbon cloth, and subjecting the substrate with the attached precursor to at least one thermal shock until the precursor is completely converted into the corresponding metal, thereby obtaining a nickel-molybdenum-iron water electrolysis catalyst; The substrate is nickel mesh, nickel foam or nickel-molybdenum foam; When the substrate is a nickel mesh, the voltage is set to 5-20V, and when the substrate is foamed nickel or foamed nickel-molybdenum, the voltage is set to 5-10V; the time of each thermal shock is 0.1-4 seconds; The thermal shock was carried out under inert gas protection.
2. The preparation method according to claim 1, characterized in that: The molar ratio of the iron source, the molybdenum source, the nickel source, the urea and the solvent is 5:2:6:50~60:75~85.
3. The preparation method according to claim 1 or 2, characterized in that: The iron source is ferric chloride, the molybdenum source is ammonium molybdate or sodium molybdate, the nickel source is nickel chloride, and the solvent is anhydrous ethanol or ethylene glycol.
4. The preparation method according to claim 1, characterized in that: The mesh size of the nickel mesh is 40-100 mesh.
5. The preparation method according to claim 1, characterized in that: During the thermal shock, the voltage was set to 10V, the duration was 2-4s each time, and the number of thermal shocks was 3 times.
6. The preparation method according to claim 1, characterized in that: The shielding gas is argon, helium or a mixture of the two.
7. A nickel-molybdenum-iron water electrolysis catalyst prepared according to the preparation method of the nickel-molybdenum-iron water electrolysis catalyst described in any one of claims 1-6.
8. Application of the nickel-molybdenum-iron water electrolysis catalyst according to claim 7 in the field of hydrogen production by water splitting and seawater splitting.