Double-sided adhesive sheet, laminate for image display device, and image display device

By optimizing the structure and performance indicators in the double-sided adhesive sheet, the problem of poor peeling of the components of the image display device under cooling operation is solved, and efficient peeling and bonding reliability is achieved, which is suitable for the reuse of large, curved and expensive components. .

CN115210332BActive Publication Date: 2024-11-08MITSUBISHI CHEM CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202180010580.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-03-31
Filing Date
2021-02-22
Publication Date
2024-11-08
Estimated Expiration
2041-02-22

AI Technical Summary

Technical Problem

The prior art failed to effectively evaluate and design the releasable adhesive sheet for image display devices under cooling operation, resulting in problems such as displacement, entrainment of air bubbles and foreign objects during bonding, especially for large images, curved surfaces and Reuse of expensive components is difficult.

Method used

Optimize the ratio of tensile energy storage modulus (E') to shear energy storage modulus (G'), loss tangent peak temperature determined by dynamic viscoelasticity, and 180° peel bonding in a double-sided adhesive sheet The adhesive sheet can be designed to peel efficiently under cooling conditions, and a multi-layer (meth)acrylic adhesive layer structure is adopted to ensure high-degree absorption and bond reliability.

Benefits of technology

It realizes efficient peeling of the components of the image display device under cooling operation, improves the bonding reliability and reworkability, is suitable for the reuse of large, curved and expensive components, and enhances the comprehensiveness of adhesive performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115210332B_ABST
    Figure CN115210332B_ABST
Patent Text Reader

Abstract

A double-sided adhesive sheet for bonding two components of an image display device, which has excellent adhesive properties such as height difference absorption, adhesive strength, and bonding reliability, and can be peeled off by cooling operation, is provided, wherein the ratio (E' / G') of the tensile storage modulus (E') to the shear storage modulus (G') is 5.0 or more, the peak temperature (T1) of the loss tangent (Tanδ) obtained by the dynamic viscoelasticity measurement in the shear mode at a frequency of 1 Hz is below -10°C, the peak temperature (T2) of the loss tangent (Tanδ) obtained by the dynamic viscoelasticity measurement in the tensile mode at a frequency of 1 Hz is above -10°C (wherein, when two or more peak temperatures are observed, the higher temperature is taken as the peak temperature (T2).), and the 180° peeling adhesive strength at 23°C with the adhered surfaces of the two components of the image display device is 5 N / 20 mm or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a double-sided pressure-sensitive adhesive sheet for bonding two components of an image display device, a laminate for an image display device, and an image display device. Background Art

[0002] In recent years, in order to improve the visibility of image display devices, the following operations have been performed: the gaps between an image display panel of a liquid crystal display (LCD), a plasma display (PDP) or an electroluminescent display (ELD) and a protective panel and a touch panel member arranged on the front side (visible side) thereof are filled with resins such as adhesives and bonding agents to suppress reflections of incident light and outgoing light from the displayed image at the air layer interface.

[0003] For example, Patent Document 1 discloses a method for manufacturing a laminated body for an image display device having a structure in which constituent components for an image display device are laminated on at least one side of a transparent double-sided adhesive sheet. The method comprises: attaching an adhesive sheet that has been cross-linked once by ultraviolet rays to the constituent components for an image display device, and then curing the adhesive sheet by irradiating it with ultraviolet rays for a second time with the aid of the constituent components for an image display device.

[0004] When the components of the image display device are bonded and integrated with an adhesive in this way, errors such as displacement, entrainment of bubbles, and foreign matter may occur during the bonding operation. Therefore, in order to correct the error, it is necessary to peel off the components of the image display device, and therefore, the adhesive used for this purpose is sometimes required to be re-peelable (reworkable). In particular, when the laminated bodies of non-bendable plate-like components are not easy to separate after being temporarily bonded, and when bonding components of large screens that are difficult to bond, components with curved shapes, and expensive components, etc., an adhesive with reworkability is required.

[0005] In addition, even when the components of the image display device are completely bonded together using an adhesive, defects such as poor bonding and poor curing may occur after bonding. It is desired to reuse some components such as expensive components instead of discarding them. From the perspective of recycling, the requirements for re-peelability (reworkability) are also increased.

[0006] In the past, as an adhesive with re-peelability (reworkability) suitable for image display devices, for example, Patent Document 2 proposed an adhesive for optical films, which uses a specific acrylic triblock copolymer, does not require chemical crosslinking, has excellent adhesive properties and durability, and can be peeled with a moderate peel strength without leaving residual adhesive.

[0007] In addition, in Patent Document 3, as a double-sided adhesive sheet characterized in that it is constructed in a manner that at least one of the surfaces of a touch panel and a display device can be re-peeled off and having an optically isotropic structure, a re-peelable structure is disclosed, which is achieved by making the adhesive force of the adhesive layer on the display device side to the display surface of the display device smaller than the adhesive force of the adhesive layer on the touch panel side to the bonding surface of the touch panel.

[0008] Furthermore, Patent Document 4 discloses, as a removable PSA, a PSA sheet having a structure that includes an internal peelable interface (internal peeling interface) on a surface different from the bonding surface between the PSA and the adherend.

[0009] Prior art literature

[0010] Patent Literature

[0011] Patent Document 1: Japanese Patent No. 4971529

[0012] Patent Document 2: Japanese Patent No. 5203964

[0013] Patent Document 3: Japanese Patent Application Publication No. 2004-231723

[0014] Patent Document 4: International Publication No. 2010 / 137523 Summary of the invention

[0015] Problem that the invention aims to solve

[0016] In actual manufacturing processes, the image display device component is sometimes peeled (separated) by cooling, but the evaluation of re-peelability disclosed in the above-mentioned Patent Documents 2 to 4 is performed at room temperature, and the evaluation of re-peelability based on the cooling operation is not performed. Therefore, the design of the adhesive sheet from the viewpoint of re-peelability based on the cooling operation is not performed in the above-mentioned Patent Documents 2 to 4.

[0017] Therefore, an object of the present invention is to provide a double-sided PSA sheet which has excellent adhesive properties such as step absorption, adhesive strength, and lamination reliability and can be peeled (separated) from a constituent member for an image display device by a cooling operation.

[0018] Solutions for solving problems

[0019] The present inventors have conducted intensive studies to solve the above-mentioned problems and have found that, in a double-sided adhesive sheet, the above-mentioned problems can be solved by setting the ratio of the tensile storage modulus (E') to the shear storage modulus (G'), the peak temperature of the loss tangent obtained by the dynamic viscoelasticity measurement in the shear mode, the peak temperature of the loss tangent obtained by the dynamic viscoelasticity measurement in the tensile mode, and the 180° peel adhesion to specified values.

[0020] That is, the gist of the present invention lies in the following [1] to

[13] .

[0021] [1] A double-sided adhesive sheet for bonding two components of an image display device.

[0022] The ratio (E' / G') of the tensile storage modulus (E') to the shear storage modulus (G') of the double-sided adhesive sheet is 5.0 or more,

[0023] The peak temperature (T1) of the loss tangent (Tanδ) obtained by the dynamic viscoelasticity measurement in the shear mode at a frequency of 1 Hz is below -10°C.

[0024] The peak temperature (T2) of the loss tangent (Tanδ) obtained by dynamic viscoelasticity measurement in a tensile mode at a frequency of 1 Hz is -10°C or higher (when two or more peak temperatures are observed, the highest temperature is the peak temperature (T2)).

[0025] The 180° peeling strength at 23° C. with respect to each adherend surface of the two image display device constituent members is 5 N / 20 mm or more.

[0026] [2] The double-sided adhesive sheet according to [1], wherein the difference between the peak temperature (T2) of the loss tangent (Tanδ) obtained by the dynamic viscoelasticity measurement in the tensile mode at a frequency of 1 Hz and the peak temperature (T1) of the loss tangent (Tanδ) obtained by the dynamic viscoelasticity measurement in the shear mode at a frequency of 1 Hz is 5 to 50°C.

[0027] [3] The double-sided pressure-sensitive adhesive sheet according to [1] or [2], wherein the two image display device components are formed of different materials.

[0028] [4] A double-sided adhesive sheet according to any one of [1] to [3], wherein one of the two components for the image display device is glass, and the other comprises any one or a combination of two or more of the group consisting of a touch sensor, an image display panel, a surface protection panel, a polarizing film and a phase difference film.

[0029] [5] The double-sided adhesive sheet according to [4], wherein the glass is a cover glass having a curved shape.

[0030] [6] The double-sided pressure-sensitive adhesive sheet according to any one of [1] to [5], wherein the two image display device components can be separated by cooling.

[0031] [7] The double-sided PSA sheet according to [6], wherein the cooling step is performed to cool to -50°C or lower.

[0032] [8] The double-sided PSA sheet according to any one of [1] to [7], which has a thickness of 50 to 1000 μm.

[0033] [9] The double-sided PSA sheet according to any one of [1] to [8], wherein the double-sided PSA sheet comprises at least three layers, the outermost layer and the innermost layer being (meth)acrylic PSA layers,

[0034] The total ratio of the thickness of the outermost layer and the innermost layer to the overall thickness is 5 to 70%.

[0035]

[10] The double-sided pressure-sensitive adhesive sheet according to any one of [1] to [9], which is photocurable.

[0036]

[11] A laminate for an image display device, comprising two components for an image display device bonded together via the double-sided pressure-sensitive adhesive sheet according to any one of [1] to

[10] .

[0037]

[12] A laminate for an image display device, wherein two components for an image display device are bonded together via the cured adhesive layer of the double-sided adhesive sheet according to any one of [1] to

[10] .

[0038]

[13] An image display device, which is formed using the laminate for an image display device described in

[12] .

[0039] Effects of the Invention

[0040] The double-sided adhesive sheet of the present invention has excellent adhesive properties such as height difference absorption, adhesive force, and lamination reliability, and has excellent reworkability that allows the image display device component to be easily peeled off by cooling operation. Therefore, it can be suitable for laminating components for image display devices, and can be particularly suitable for laminating components of large screens that are difficult to laminate, components with curved surfaces, and expensive components. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 Figures for illustrating the evaluation test method of ITO corrosion resistance reliability and Cu corrosion resistance reliability performed in the examples, (A) is a top view of an ITO pattern on an ITO glass substrate or a top view of a copper pattern on a copper glass substrate for corrosion resistance reliability evaluation, (B) is a top view showing a state in which an adhesive sheet is covered on an ITO glass substrate for ITO corrosion resistance reliability evaluation or a top view showing a state in which an adhesive sheet is covered on a copper glass substrate for Cu corrosion resistance reliability evaluation, (C) is a cross-sectional view of a sample for ITO corrosion resistance reliability evaluation, and (D) is a cross-sectional view of a sample for Cu corrosion resistance reliability evaluation. DETAILED DESCRIPTION

[0042] Hereinafter, an example of an embodiment of the present invention will be described in detail. However, the present invention is not limited to the following embodiment.

[0043] In addition, in this specification, "(meth)acrylic acid" means including "acrylic acid" and "methacrylic acid", and "(meth)acrylate" means including "acrylate" and "methacrylate".

[0044] The double-sided adhesive sheet of the present invention is usually composed of a plurality of (meth) acrylic adhesive layers and is used to bond two image display device components. In addition, from the viewpoint of improving bonding reliability, the double-sided adhesive sheet of the present invention preferably has photocurability that is cured by irradiating active energy rays such as ultraviolet rays.

[0045] In addition, the peak temperature (T1) of the loss tangent (Tanδ) obtained by the dynamic viscoelasticity measurement in the shear mode with a frequency of 1 Hz of the double-sided adhesive sheet of the present invention is below -10°C, preferably -100 to -15°C, and particularly preferably -50 to -20°C. By making the peak temperature (T1) of the loss tangent (Tanδ) within the above range, the height difference absorbency and lamination reliability can be excellent. It should be noted that the peak temperature (T1) of the loss tangent obtained by the dynamic viscoelasticity measurement in the shear mode is obtained according to the following method.

[0046] [Dynamic viscoelasticity measurement in shear mode]

[0047] The sample to be measured was stacked in a manner of 0.6 to 0.8 mm in thickness and punched into a circle with a diameter of 8 mm as a measurement sample. For the measurement sample, a rheometer ("DiscoveryHR2" manufactured by TA Instruments) was used to measure the dynamic viscoelastic spectrum in the shear mode under the following measurement conditions. From the dynamic viscoelastic spectrum data obtained by the measurement, the temperature at which the loss tangent (Tanδ) reaches a maximum value, that is, the peak temperature (T1), was read.

[0048] It should be noted that, as mentioned above, the dynamic viscoelasticity measurement in the shear mode is a value when the thickness of the sample to be measured is set to 0.6-0.8 mm. This is because, in order to accurately measure the dynamic viscoelasticity in the shear mode, it is necessary to avoid the influence of the measuring jig caused by the insufficient thickness of the sample, which causes changes in the measurement results. Therefore, in order to measure the dynamic viscoelasticity in the shear mode, the sample must be adjusted to a certain thickness range before measurement. After the thickness of the sample is adjusted to the above range in advance, the dynamic viscoelasticity in the shear mode is measured, so that the dynamic viscoelasticity spectrum of the sample can be accurately grasped without being affected by the measuring jig.

[0049] When the sample is photocurable, the sample to be used may be before or after curing.

[0050] [Measurement conditions]

[0051] Bonding fixture: Φ8mm parallel plate

[0052] Strain: 0.1%

[0053] Frequency: 1Hz

[0054] Temperature: -120~200℃

[0055] Heating rate: 5℃ / min

[0056] In addition, the peak temperature (T2) of the loss tangent (Tanδ) obtained by the dynamic viscoelasticity measurement in the tensile mode at a frequency of 1 Hz of the double-sided adhesive sheet of the present invention is -10°C or higher, preferably -5 to 20°C, and particularly preferably 0 to 15°C. When the peak temperature (T2) of the loss tangent (Tanδ) is within the above range, the re-peelability (reworkability) and cutting processability can be excellent.

[0057] In addition, the peak temperature (T2) of the loss tangent (Tanδ) obtained by the dynamic viscoelasticity measurement in the tensile mode is obtained by the following method.

[0058] [Dynamic viscoelastic measurement in tensile mode]

[0059] For the sample to be measured, a dynamic viscoelasticity measuring device (IT Meter and Control, itkDVA-200) was used to measure the dynamic viscoelasticity spectrum in the stretching mode at a vibration frequency of 1 Hz, a measuring temperature of -120 to 80°C, and a heating rate of 3°C / min. The temperature at which the loss tangent (Tanδ) becomes a maximum value, i.e., the peak temperature (T2), was read from the dynamic viscoelasticity spectrum data obtained by the measurement. Among them, when two or more peak temperatures are observed, the highest temperature is taken as the peak temperature (T2).

[0060] When the sample is photocurable, the sample to be used may be before or after curing, but is preferably after curing.

[0061] Furthermore, in the present invention, the difference between the peak temperature (T2) of the loss tangent (Tanδ) obtained by the dynamic viscoelasticity measurement in the tensile mode at a frequency of 1 Hz and the peak temperature (T1) of the loss tangent (Tanδ) obtained by the dynamic viscoelasticity measurement in the shear mode at a frequency of 1 Hz is preferably 5 to 50° C., more preferably 10 to 40° C., and particularly preferably 15 to 30° C. By setting it in the above range, the balance of the performances of the height difference absorbability, the lamination reliability, the impact resistance, the removability (reworkability), and the cutting processability can be excellent.

[0062] The double-sided adhesive sheet of the present invention has a 180° peeling adhesive strength at 23°C with respect to the adhered surfaces of the two image display device components to be attached, which is 5N / 20mm or more, preferably 6N / 20mm or more, and particularly preferably 7N / 20mm or more. In addition, the upper limit of the 180° peeling adhesive strength is usually 50N / 20mm. It should be noted that the above 180° peeling adhesive strength is measured according to the following method.

[0063] [180° peel adhesion measurement method]

[0064] A polyethylene terephthalate (PET) film (DIAFOILT100 manufactured by Mitsubishi Chemical Corporation) with a thickness of 100 μm was bonded to one side of a double-sided adhesive sheet, and the other side was roll-bonded to a soda-lime glass plate to form a bonded product. The bonded product was then subjected to an autoclave treatment (60°C, gauge pressure 0.2 MPa, 20 minutes) for fine bonding. A high-pressure mercury lamp was then used to illuminate the product with a cumulative light intensity of 3000 mJ / cm 2 After irradiating the PET film surface with 365 nm ultraviolet rays in a manner, the sample was aged for 12 hours at 23°C and 50% RH, and the obtained sample was used as a sample for 180° peeling adhesion measurement. The sample was used as the peeling force (N / cm) when peeled at a peeling angle of 180° and a peeling speed of 300 mm / min at 23°C and 50% RH as the 180° peeling adhesion.

[0065] The layer structure of the double-sided adhesive sheet of the present invention is preferably a two-layer structure in which the outer layer and the inner layer are (meth) acrylic adhesive layers, more preferably at least three layers in which the outermost layer and the innermost layer are (meth) acrylic adhesive layers, and particularly preferably three layers in which the outermost layer and the innermost layer are (meth) acrylic adhesive layers [outermost layer (adhesive layer) / intermediate layer / innermost layer (adhesive layer)]. By making the layer structure multi-layer, excellent reworkability, height difference absorption, and lamination reliability can be achieved.

[0066] Furthermore, in the present invention, from the aspects of reworkability, height difference absorption, adhesive force, and lamination reliability, it is preferred to have at least two layers with different glass transition temperatures, and it is particularly preferred to have: an outermost layer and an innermost layer (hereinafter referred to as a "low Tg layer") formed of a (meth) acrylic adhesive layer having a glass transition temperature of -10°C or less, and an intermediate layer (hereinafter referred to as a "high Tg layer") formed of a resin composition containing a (meth) acrylic resin having a glass transition temperature higher than -10°C. In this specification, unless otherwise specified, the glass transition temperature is defined by the peak temperature of the loss tangent (Tanδ) obtained by the dynamic viscoelasticity measurement in the shear mode at a frequency of 1 Hz, and is measured according to the above method.

[0067] The glass transition temperature of the low Tg layer is usually -10°C or lower, preferably -100 to -15°C, particularly preferably -50 to -20°C.

[0068] The glass transition temperature of the high Tg layer is usually higher than -10°C, preferably -5 to 20°C, and particularly preferably 0 to 15°C.

[0069] In addition, the difference in glass transition temperature between the high Tg layer and the low Tg layer (high Tg layer-low Tg layer) is usually 5°C or more, preferably 10°C or more, and particularly preferably 20°C or more. The upper limit is usually 50°C. By making the difference in glass transition temperature the above range, there is a tendency for excellent reworkability, height difference absorption, adhesion, and lamination reliability. It should be noted that when the double-sided adhesive sheet has a plurality of high Tg layers and low Tg layers, the difference in glass transition temperature between the high Tg layer and the low Tg layer is the difference in glass transition temperature between the high Tg layer with the highest glass transition temperature and the low Tg layer with the lowest glass transition temperature.

[0070] As the preferred layer constitution of the double-sided adhesive sheet of the present invention, as described above, the outermost layer and the innermost layer are set to at least 3 layers of (meth) acrylic adhesive layer, and it is particularly preferred that the outermost layer and the innermost layer are set to 3 layers of (meth) acrylic adhesive layer [outermost layer (adhesive layer) / intermediate layer / innermost layer (adhesive layer)], at this time, the outermost and innermost surfaces (surfaces bonded to the image display device with constituent members) of the preferred double-sided adhesive sheet are low Tg layers. In addition, the intermediate layer sandwiched between the outermost and innermost surfaces is preferably a high Tg layer. Furthermore, the low Tg layer used in the outermost and innermost layers can have glass transition temperatures different from each other, but the outermost layer and the innermost layer are preferably the same glass transition temperature, and it is particularly preferred that the outermost layer and the innermost layer are (meth) acrylic adhesive layers formed by the same resin composition.

[0071] That is, one of the most preferred layer structures of the double-sided adhesive sheet of the present invention is a three-layer structure of low Tg layer / high Tg layer / low Tg layer formed by two resin compositions. By forming such a layer structure, reworkability, height difference absorption, adhesive strength, and lamination reliability can be excellent.

[0072] The shear storage modulus (G') of the double-sided adhesive sheet is preferably 5×10 3 ~5×10 8 Pa, more preferably 1×10 4 ~1×10 7 Pa, particularly preferably 2×10 4 ~1×10 6 Pa. The double-sided adhesive sheet can maintain the height difference absorbency and impart appropriate processability by having a shear storage modulus (G') in this range. The above-mentioned shear storage modulus (G') is the shear storage modulus at 25°C, and is obtained by reading the shear storage modulus (G') at 25°C from the dynamic viscoelastic spectrum data obtained by the dynamic viscoelasticity measurement in the shear mode.

[0073] When the double-sided PSA sheet has at least three layers in which the outermost layer and the innermost layer are (meth)acrylic PSA layers, the shear storage modulus (G') of the intermediate layer is preferably larger than the shear storage modulus (G') of the outermost layer and the innermost layer from the viewpoint of reworkability.

[0074] The tensile storage modulus (E') of the double-sided adhesive sheet is preferably 2.5×10 4 ~5×10 8 Pa, more preferably 5×10 4 ~5×10 7 Pa, particularly preferably 1×10 5 ~5×10 6 Pa. By having such a range of tensile storage modulus (E'), it is possible to achieve excellent operability and cutting processability. The tensile storage modulus (E') is the tensile storage modulus at 25°C, and is obtained by reading the tensile storage modulus (E') at 25°C from the dynamic viscoelastic spectrum data obtained by the dynamic viscoelasticity measurement in the aforementioned tensile mode.

[0075] As described above, the double-sided adhesive sheet of the present invention preferably has at least two layers with different glass transition temperatures, but when the double-sided adhesive sheet has at least two layers with different glass transition temperatures, it can be determined based on the ratio of the tensile storage modulus (E') obtained by tensile viscoelasticity measurement to the shear storage modulus (G') obtained by shear viscoelasticity measurement. Usually, when the adhesive sheet is an isotropic elastomer, the relationship between the tensile storage modulus (E') and the shear storage modulus (G') is E'=3G'.

[0076] However, in the case of having at least two layers having different glass transition temperatures, that is, in the case of an anisotropic elastomer, this relationship does not hold (E'≠3G').

[0077] The ratio (E' / G') of the tensile storage modulus (E') to the shear storage modulus (G') of the double-sided adhesive sheet of the present invention is 5.0 or more, preferably 6.0 or more, more preferably 7.0 or more, and further preferably 8.0 or more. In addition, it is preferably 100 or less, more preferably 50 or less, and further preferably 30 or less.

[0078] That is, since the E' / G' ratio of the double-sided adhesive sheet is greater than 5.0, it can be judged as "having at least two layers with different glass transition temperatures" or "a layer with a glass transition temperature inclined in the thickness direction", and it has excellent reworkability and becomes easy to peel off at the interface portion with the adhered surface of at least one of the components for the image display device through cooling operation.

[0079] The thickness of the double-sided adhesive sheet of the present invention is preferably 50 to 1000 μm, more preferably 60 to 500 μm, and particularly preferably 75 to 300 μm. If the sheet is too thin, the step absorption property tends to decrease, while if it is too thick, the reworkability tends to be difficult to obtain.

[0080] In addition, when the double-sided adhesive sheet has at least three layers in which the outermost layer and the innermost layer are set as (meth) acrylic adhesive layers, the total ratio of the thickness of the outermost layer and the innermost layer relative to the overall thickness is preferably 5 to 70%, more preferably 10 to 60%, and particularly preferably 20 to 45%. By making the thickness of the outermost layer and the innermost layer within the above range, it is possible to achieve excellent reworkability, height difference absorption, and lamination reliability.

[0081] The double-sided adhesive sheet of the present invention is used to bond two components of image display devices, specifically, components of LCD, PDP or EL image display devices such as personal computers, mobile terminals (PDAs), game consoles, televisions (TVs), car navigation systems, touch panels, and handwriting tablets.

[0082] In addition, from the viewpoint of reworkability, it is preferable that the two image display device constituent members are formed of different materials.

[0083] As the constituent component for the above-mentioned image display device, more specifically, it is preferred that one of the two constituent components for the image display device is glass and the other is a film, and it is particularly preferred that the glass is tempered glass, and the film is a laminate comprising any one or a combination of two or more of the group consisting of a touch sensor, an image display panel, a surface protection panel, a polarizing film and a phase difference film.

[0084] In recent years, in image display panels such as liquid crystal displays (LCDs), plasma displays (PDPs), or electroluminescent displays (ELDs), protective glasses with curved shapes are increasingly used from the perspective of design. However, the above-mentioned protective glasses are expensive and are components that are intended to be recycled. Therefore, by using the double-sided adhesive sheet of the present invention, the reworkability is excellent, and therefore, it can also be effectively used for protective glasses with curved shapes.

[0085] As the substrate of the above-mentioned film, a transparent resin is preferably used, for example, polyester resin, polyolefin resin, (meth) acrylic resin, polyurethane resin, polyether sulfone resin, polycarbonate resin, polysulfone resin, polyether resin, polyether ketone resin, (meth) acrylonitrile resin, cycloolefin resin, etc. can be mentioned, among which polyester resin is preferred, and polyethylene terephthalate (PET) is particularly preferred. These can be used alone or in combination of two or more.

[0086] By laminating the image display device constituent members on both adhesive surfaces of the double-sided adhesive sheet of the present invention, a laminated body for an image display device having two image display device constituent members laminated by means of the double-sided adhesive sheet can be obtained. In addition, by irradiating the above-mentioned laminated body for an image display device with active energy rays to photo-cure the adhesive sheet, a laminated body for an image display device having two image display device constituent members laminated by means of the adhesive layer cured by the double-sided adhesive sheet can be obtained.

[0087] The double-sided adhesive sheet of the present invention is preferably configured to be able to peel off (separate) two image display device constituent members by cooling operation. It is particularly preferably configured to be able to peel off (separate) at the interface portion of the adhered surface of at least any one image display device constituent member by cooling operation. It should be noted that "can be peeled off (separated)" means: the image display device constituent member bonded by the double-sided adhesive sheet can be easily peeled off (separated) without destroying the aforementioned member, and particularly refers to a state in which the double-sided adhesive sheet and the image display device constituent member can be peeled off (separated) at the interface. In addition, the above-mentioned cooling operation is carried out by the following method.

[0088] 〔Cooling operation〕

[0089] By cooling the image display device laminate, the image display device constituent members can be separated, and in particular, separation is caused at the interface portion with the adherend surface of at least one image display device constituent member.

[0090] In addition, depending on the situation, the image display device stack before irradiation with active energy rays is sometimes cooled and peeled off without irradiation with the above-mentioned active energy rays. In this case, the image display device components can be separated, especially by causing peeling at the interface portion with the adhered surface of at least one image display device component.

[0091] According to the above method, the constituent members for the image display device can be easily reused.

[0092] The cooling temperature of the image display device laminate is preferably -50°C or lower, more preferably -80°C or lower, and further preferably -100°C or lower. The lower limit of the cooling temperature is not particularly limited, but is usually about -300°C, preferably about -200°C.

[0093] In addition, when cooling the above-mentioned image display device stack, it is preferably allowed to stand in a manner that one of the image display components of the image display device stack is in contact with a SUS cooling plate set to the above-mentioned cooling temperature, and it is particularly preferred to stand in a manner that the component side with a low linear expansion coefficient of the image display device component is in contact with the SUS cooling plate.

[0094] The peelable time is usually within 600 seconds, particularly preferably within 300 seconds, more preferably within 180 seconds, particularly preferably within 120 seconds, further preferably within 60 seconds, and particularly preferably within 30 seconds.

[0095] The principle that the double-sided adhesive sheet of the present invention can make the image display device component (adherend) peel off by cooling operation is considered as follows. If the double-sided adhesive sheet attached to 2 adherends is cooled, the adherend shrinks with the reduction of temperature, and the stress of the elastic modulus × shrinkage strain of the adherend is generated. The strain or stress becomes the peeling force for separation at the interface portion of the double-sided adhesive sheet and the adherend. Therefore, the 2 adherends contacted with the double-sided adhesive sheet are preferably materials with different linear expansion coefficients, and further preferably 2 adherends are materials of different types.

[0096] The double-sided adhesive sheet of the present invention is not easy to relax the strain or stress (difference) received from the above-mentioned adherend, or becomes difficult to relax by cooling, which becomes the key point of the double-sided adhesive sheet for having reworkability. Specifically, the glass transition temperature (Tg) of the double-sided adhesive sheet can be raised. However, if only by raising the glass transition temperature (Tg), the adhesive properties such as height difference absorbency, adhesive force, and lamination reliability will be reduced. Therefore, in the present invention, the ratio (E' / G') of the tensile storage modulus (E') to the shear storage modulus (G') of the double-sided adhesive sheet is set to 5.0 or more, and further, the peak temperature (T1) of the loss tangent (Tanδ) obtained by measuring the dynamic viscoelasticity of the double-sided adhesive sheet in a shear mode at a frequency of 1 Hz is set to be below -10°C, and further, the peak temperature (T2) of the loss tangent (Tanδ) obtained by measuring the dynamic viscoelasticity of the double-sided adhesive sheet in a tensile mode at a frequency of 1 Hz is set to be above -10°C (wherein, when two or more peak temperatures are observed, the highest temperature is taken as the peak temperature (T2).).

[0097] The double-sided PSA sheet of the present invention having the above-mentioned properties preferably has at least two (meth)acrylic PSA layers, wherein the (meth)acrylic PSA layers are formed from a resin composition containing a (meth)acrylic copolymer.

[0098] When the intermediate layer has at least three layers including the outermost layer and the innermost layer as the (meth)acrylic pressure-sensitive adhesive layer, it is also formed from a resin composition containing a (meth)acrylic copolymer.

[0099] Hereinafter, the resin composition for forming the (meth)acrylic pressure-sensitive adhesive layer and the intermediate layer will be described.

[0100] The resin composition contains a (meth)acrylic copolymer as a main component, and may further contain a crosslinking agent (B), a photoinitiator (C), a silane coupling agent (D), an antiseptic (E), and other additives.

[0101] The “main component” mentioned above refers to a (meth)acrylic copolymer containing 50% by mass or more, preferably 70% by mass or more, more preferably 80% by mass or more, based on the entire resin composition.

[0102] [(Meth)acrylic acid copolymer]

[0103] Examples of the (meth)acrylic copolymer include a copolymer of an alkyl (meth)acrylate monomer having an alkyl group with 4 to 18 carbon atoms and a monomer component copolymerizable with the alkyl (meth)acrylate monomer.

[0104] Examples of the (meth)acrylic acid alkyl ester monomers in which the alkyl group has 4 to 18 carbon atoms include straight-chain alkyl (meth)acrylate monomers such as n-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, n-octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, hexadecyl (meth)acrylate, and stearyl (meth)acrylate, and examples thereof include isobutyl (meth)acrylate, sec-butyl (meth)acrylate, and cetyl (meth)acrylate. Branched alkyl (meth)acrylate monomers such as tert-butyl acrylate, isopentyl (meth)acrylate, neopentyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, isodecyl (meth)acrylate, and isostearyl (meth)acrylate, and alicyclic (meth)acrylate monomers such as cyclohexyl (meth)acrylate, tert-butylcyclohexyl (meth)acrylate, 3,5,5-trimethylcyclohexane (meth)acrylate, dicyclopentyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, and isobornyl (meth)acrylate. These can be used alone or in combination of two or more.

[0105] Examples of the monomer component copolymerizable with the above-mentioned (meth)acrylate alkyl ester monomer having an alkyl group with 4 to 18 carbon atoms include hydroxyl group-containing (meth)acrylate monomers, nitrogen atom-containing (meth)acrylate monomers, carboxyl group-containing (meth)acrylate monomers, epoxy group-containing (meth)acrylate monomers, vinyl monomers, (meth)acrylate alkyl ester monomers having an alkyl group with 1 to 3 carbon atoms, and other copolymerizable monomers.

[0106] Examples of the hydroxyl group-containing (meth)acrylate monomer include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxy-1-methylethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, glycerol mono(meth)acrylate, polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, polyethylene glycol polypropylene glycol mono(meth)acrylate, polyethylene glycol polybutylene glycol mono(meth)acrylate, polypropylene glycol polybutylene glycol mono(meth)acrylate, and hydroxyphenyl (meth)acrylate. These monomers may be one or a combination of two or more.

[0107] Examples of the nitrogen atom-containing (meth)acrylate monomer include aminoalkyl (meth)acrylates such as aminomethyl (meth)acrylate, aminoethyl (meth)acrylate, aminopropyl (meth)acrylate, and aminoisopropyl (meth)acrylate, amino (meth)acrylate monomers such as N-alkylaminoalkyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, and N,N-dimethylaminopropyl (meth)acrylate, (meth)acrylamide, N,N-dimethyl (meth)acrylamide, N-butyl (meth)acrylamide, N-methylol (meth)acrylamide, N-methylolpropane (meth)acrylamide, N-methoxymethyl (meth)acrylamide, N-butoxymethyl (meth)acrylamide, diacetone (meth)acrylamide, maleamide, and maleimide. These may be used alone or in combination of two or more.

[0108] Moreover, as said carboxyl group-containing (meth)acrylate monomer, (meth)acrylic acid, (meth)acrylic acid dimer, etc. are mentioned, for example. These may be used alone or in combination of two or more.

[0109] Examples of the epoxy group-containing (meth)acrylate monomer include glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate glycidyl ether. These may be used alone or in combination of two or more.

[0110] Examples of the vinyl monomer include (meth)acrylic acid alkyl esters having an alkyl group with 1 to 12 carbon atoms, functional monomers having a functional group such as a hydroxyl group, an amide group, and an alkoxyalkyl group in the molecule, polyalkylene glycol di(meth)acrylates, vinyl ester monomers such as vinyl acetate, vinyl propionate, and vinyl laurate, and aromatic vinyl monomers such as styrene, chlorostyrene, chloromethylstyrene, α-methylstyrene, and other substituted styrenes. These may be one or a combination of two or more.

[0111] Examples of the (meth)acrylic acid alkyl ester monomers having an alkyl group with 1 to 3 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, etc. These may be used alone or in combination of two or more.

[0112] Examples of the other copolymerizable monomers include acid anhydride group-containing monomers such as maleic anhydride and itaconic anhydride, heterocyclic basic monomers such as vinyl pyrrolidone, vinyl pyridine and vinyl carbazole, and macromonomers, etc. These may be used alone or in combination of two or more.

[0113] In the present invention, a (meth)acrylic copolymer obtained by copolymerizing the above-mentioned various monomer components can be used in a manner such that a double-sided adhesive sheet has a predetermined peak temperature of loss tangent and specific physical properties when formed. The copolymerization method can also be carried out according to conventionally known methods, such as solution radical polymerization, suspension polymerization, bulk polymerization, emulsion polymerization, etc.

[0114] Among them, when the double-sided adhesive sheet of the present invention has at least three layers in which the outermost layer and the innermost layer are (meth)acrylic adhesive layers, it is preferred that the outermost and innermost (meth)acrylic adhesive layers are formed from a resin composition containing a (meth)acrylic copolymer (A) having a glass transition temperature of -10°C or less, and it is more preferred that the (meth)acrylic copolymer contained in the resin composition consists only of the (meth)acrylic copolymer (A).

[0115] [(Meth)acrylic acid copolymer (A)]

[0116] The (meth)acrylic copolymer (A) having a glass transition temperature of -10°C or less preferably comprises: a polar group-containing (meth)acrylate monomer (a2) that is substantially free of structural units derived from a carboxyl group-containing (meth)acrylate monomer and that contains at least one selected from the group consisting of a hydroxyl group-containing (meth)acrylate monomer and a nitrogen atom-containing (meth)acrylate monomer; and a (meth)acrylate monomer (a1) other than the monomer (a2) having a glass transition temperature (Tg) of less than -30°C when forming a homopolymer from the monomer components as monomer components constituting the (meth)acrylic copolymer (A).

[0117] It should be noted that the above-mentioned “substantially containing no structural unit derived from a carboxyl group-containing (meth)acrylate monomer” includes not only the case where no structural unit is contained at all, but also includes the case where the structural unit derived from a carboxyl group-containing (meth)acrylate monomer is contained in the (meth)acrylic copolymer (A) at less than 0.5% by mass, preferably less than 0.1% by mass.

[0118] As the (meth)acrylate monomer (a1) having a glass transition temperature (Tg) of less than -30°C (preferably less than -40°C, particularly preferably less than -50°C) when forming a homopolymer from the monomer components, examples include those having a glass transition temperature of less than -30°C among the aforementioned (meth)acrylate alkyl ester monomers having an alkyl group with 4 to 18 carbon atoms. Specifically, examples include: (meth)acrylate straight-chain alkyl ester monomers such as n-propyl (meth)acrylate, n-butyl (meth)acrylate, n-heptyl acrylate, n-hexyl acrylate, n-octyl acrylate, nonyl acrylate, lauryl methacrylate, stearyl methacrylate; (meth)acrylate branched alkyl ester monomers such as 2-ethylhexyl acrylate, isononyl acrylate, isodecyl acrylate, etc. These may be one kind or a combination of two or more kinds. Among them, branched alkyl (meth)acrylate is preferred, and 2-ethylhexyl acrylate is particularly preferred.

[0119] Examples of the polar group-containing (meth)acrylate monomer (a2) include the aforementioned hydroxyl group-containing (meth)acrylate monomers and nitrogen atom-containing (meth)acrylate monomers. Among them, hydroxyl group-containing (meth)acrylate monomers are preferred, and 2-hydroxyethyl acrylate is particularly preferred.

[0120] In addition, as the copolymerization component of the (meth)acrylic copolymer (A), monomers other than the above-mentioned monomers (a1) and (a2) can be used. As monomers other than the above-mentioned monomers (a1) and (a2), various monomers mentioned above can be used, among which, (meth)acrylic acid alkyl ester monomers having an alkyl group with 1 to 3 carbon atoms are preferably used, and methyl (meth)acrylate is particularly preferably used.

[0121] The glass transition temperature of the (meth)acrylic copolymer (A) obtained by copolymerizing these is preferably -10°C or lower, more preferably -100 to -15°C, particularly preferably -50 to -20°C, from the viewpoint of step absorption and bonding reliability.

[0122] The mass average molecular weight of the (meth)acrylic copolymer (A) is preferably 50,000 to 1,500,000, more preferably 100,000 to 700,000, and particularly preferably 150,000 to 600,000.

[0123] In this specification, the mass average molecular weight is measured by the following method.

[0124] A sample prepared by dissolving 4 mg of a (meth)acrylic copolymer in 12 mL of THF was used as a measurement sample. The molecular weight distribution curve was measured under the following conditions using a gel permeation chromatography (GPC) analyzer (HLC-8320GPC manufactured by Tosoh Corporation) to determine the mass average molecular weight (Mm).

[0125] Guard column: TSKguardcolumnHXL

[0126] Separation column: TSKgelGMHXL (4 pieces)

[0127] Temperature: 40℃

[0128] Injection volume: 100μL

[0129] Polystyrene conversion

[0130] Solvent: THF

[0131] Flow rate: 1.0mL / min

[0132] The hydroxyl value of the (meth)acrylic copolymer (A) is usually 20 to 150 mgKOH / g, preferably 30 to 100 mgKOH / g, and more preferably 40 to 80 mgKOH / g.

[0133] In addition, when the double-sided adhesive sheet of the present invention has at least three layers in which the outermost layer and the innermost layer are (meth)acrylic adhesive layers, the intermediate layer (layer sandwiched between the outermost layer and the innermost layer) is preferably formed from a resin composition containing a (meth)acrylic copolymer (A') having a glass transition temperature higher than -10°C, and it is more preferred that the (meth)acrylic copolymer contained in the resin composition consists only of the (meth)acrylic copolymer (A').

[0134] [(Meth)acrylic acid copolymer (A')]

[0135] The (meth)acrylic copolymer (A') having a glass transition temperature higher than -10°C preferably comprises, as monomer components constituting the (meth)acrylic copolymer (A'), at least one polar group-containing (meth)acrylic ester monomer (a2) selected from the group consisting of a hydroxyl group-containing (meth)acrylic ester monomer and a nitrogen atom-containing (meth)acrylic ester monomer, and an alkyl (meth)acrylic acid ester monomer (a3) ​​having an alkyl group with 1 to 18 carbon atoms.

[0136] Examples of the polar group-containing (meth)acrylate monomer (a2) include the aforementioned hydroxyl group-containing (meth)acrylate monomers and nitrogen atom-containing (meth)acrylate monomers. Among them, nitrogen atom-containing (meth)acrylates are preferred, amide group-containing (meth)acrylates are more preferred, and (meth)acrylamide is particularly preferred.

[0137] Examples of the (meth)acrylic acid alkyl ester monomer (a3) ​​having an alkyl group with 1 to 18 carbon atoms include the aforementioned (meth)acrylic acid alkyl ester monomer having 4 to 18 carbon atoms and (meth)acrylic acid alkyl ester monomer having 1 to 3 carbon atoms. Among them, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, and isobornyl (meth)acrylate are particularly preferred. Furthermore, from the viewpoint of the versatility of the monomers and the Tg of the (meth)acrylic copolymer (A') being -10°C or higher, methyl (meth)acrylate, ethyl methacrylate, tert-butyl (meth)acrylate, isobutyl methacrylate, and isobornyl (meth)acrylate are more preferred.

[0138] In addition, as the copolymerization component of the (meth)acrylate copolymer (A'), monomers other than the above-mentioned monomers (a2) and (a3) ​​can be used. As monomers other than the above-mentioned monomers (a2) and (a3), various monomers mentioned above can be used.

[0139] The glass transition temperature of the (meth)acrylic copolymer (A') obtained by copolymerizing these is preferably higher than -10°C, more preferably -5 to 20°C, and particularly preferably 0 to 15°C, from the viewpoint of reworkability.

[0140] The mass average molecular weight of the (meth)acrylic copolymer (A') is preferably 50,000 to 1,000,000, particularly preferably 70,000 to 700,000, and particularly preferably 100,000 to 500,000.

[0141] [Crosslinking agent (B)]

[0142] The resin composition forming each layer may contain a crosslinking agent (B) in addition to the (meth)acrylic copolymer. In particular, it is preferred to mix the crosslinking agent (B) in the resin composition forming the intermediate layer of the double-sided adhesive sheet.

[0143] As the crosslinking agent (B), a crosslinking agent having at least double bond crosslinking is preferred. For example, a crosslinking agent having at least one crosslinkable functional group selected from (meth)acryloyl, epoxy, isocyanate, carboxyl, hydroxyl, carbodiimide, oxazoline, aziridine, vinyl, amino, imino, and amide can be mentioned, and one or a combination of two or more can be used. In addition, as the crosslinking agent (B), a solution in which the crosslinking agent (B) is chemically bonded to the above-mentioned (meth)acrylic copolymer is also included.

[0144] Among them, a crosslinking agent having a (meth)acryloyl group is preferred, and multifunctional (meth)acrylates are particularly preferred in terms of cutting processability and lamination reliability. Here, multifunctional refers to: having two or more crosslinking functional groups. It should be noted that, as required, it may have three or more, or four or more crosslinking functional groups. In addition, the crosslinking functional groups may be protected by a protective group that can be deprotected.

[0145] Examples of the polyfunctional (meth)acrylate include 1,4-butanediol di(meth)acrylate, glycerol di(meth)acrylate, neopentyl glycol di(meth)acrylate, glyceryl glycidyl ether di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, tricyclodecane dimethacrylate, tricyclodecane dimethanol di(meth)acrylate, bisphenol A polyethoxy di(meth)acrylate, bisphenol A polypropoxy di(meth)acrylate. ) acrylate, bisphenol F polyethoxy di(meth)acrylate, ethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane trioxyethyl (meth)acrylate, ε-caprolactone modified tri(2-hydroxyethyl) isocyanurate tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propoxylated pentaerythritol tri(meth)acrylate, ethoxylated pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, propoxylated pentaerythritol tetra (Meth)acrylate, ethoxylated pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, tri(acryloyloxyethyl) isocyanurate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol penta(meth)acrylate, tripentaerythritol hexa(meth)acrylate, tripentaerythritol penta(meth)acrylate, hydroxypivalate neopentyl glycol di(meth)acrylate The present invention relates to polyfunctional (meth) acrylic acid monomers such as polyfunctional (meth) acrylic acid monomers, ...

[0146] The content of the crosslinking agent (B) is usually 0.5 to 50 parts by mass, preferably 1 to 40 parts by mass, and particularly preferably 5 to 30 parts by mass based on 100 parts by mass of the (meth)acrylic copolymer. If the content is within the above range, cutting processability and bonding reliability can be easily obtained, which is preferred.

[0147] [Photopolymerization initiator (C)]

[0148] The resin composition preferably contains a photopolymerization initiator (C). As the photopolymerization initiator (C), conventionally known ones can be appropriately used, and among them, photopolymerization initiators that are sensitive to ultraviolet rays having a wavelength of 380 nm or less are preferred from the viewpoint of ease of controlling the crosslinking reaction.

[0149] Photopolymerization initiators (C) are roughly divided into two categories based on the mechanism of free radical generation: cleavage-type photopolymerization initiators in which the single bonds of the photopolymerization initiator itself are cleaved and decomposed to generate free radicals, and hydrogen-abstraction-type photopolymerization initiators in which the photopolymerization initiator after light excitation forms an excited complex with a hydrogen donor in the system and can transfer hydrogen from the hydrogen donor.

[0150] The above-mentioned cleavage-type photopolymerization initiator decomposes into other compounds when generating free radicals by light irradiation, and loses its function as a reaction initiator when it is excited once. Therefore, it is preferred because it does not remain as active species in the cured product such as the adhesive after the crosslinking reaction is completed, and there is no possibility of causing unexpected light degradation to the cured product.

[0151] On the other hand, hydrogen abstraction type photopolymerization initiators do not produce decomposition products like cleavage type photopolymerization initiators when undergoing a radical generation reaction based on irradiation with active energy rays such as ultraviolet rays. Therefore, they are less likely to become volatile components after the reaction is completed, and are useful in terms of reducing damage to the adherend.

[0152] Examples of the cleavage-type photopolymerization initiator include 2,2-dimethoxy-1,2-diphenylethane-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propane-1-one, 1-(4-(2-hydroxyethoxy)phenyl)-2-hydroxy-2-methyl-1-propane-1-one, 2-hydroxy-1-[4-{4-(2-hydroxy-2-methyl-propionyl)benzyl}phenyl]-2-methyl-propane-1-one, oligo(2-hydroxy-2-methyl-1-(4-(1 1-(4-(1-methylvinyl)phenyl)acetone), methyl phenylglyoxylate, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butane-1-one, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1-one, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholino)phenyl]-1-butanone, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and derivatives thereof. Among them, oligo(2-hydroxy-2-methyl-1-(4-(1-methylvinyl)phenyl)acetone) is preferred.

[0153] Examples of the hydrogen abstraction type photopolymerization initiator include benzophenone, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, 4-phenylbenzophenone, 3,3'-dimethyl-4-methoxybenzophenone, methyl 2-benzoylbenzoate, methyl benzoylformate, bis(2-phenyl-2-oxoacetate)oxybisethylene, 4-(1,3-acryloyl-1,4,7,10,13-pentaoxotridecanyl)benzophenone, thioxanthone, 2-chlorothioxanthone, 3-methylthioxanthone, 2,4-dimethylthioxanthone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 2-aminoanthraquinone, and derivatives thereof. Among them, 4-methylbenzophenone and 2,4,6-trimethylbenzophenone are preferred.

[0154] The photopolymerization initiator (C) is not limited to the above-mentioned ones. In addition, as the photopolymerization initiator (C), any one of a cleavage-type photopolymerization initiator and a hydrogen abstraction-type photopolymerization initiator may be used, and a combination of the two may be used.

[0155] The content of the photopolymerization initiator (C) is not particularly limited, but is usually 0.1 to 10 parts by mass, preferably 0.2 to 5 parts by mass, particularly preferably 0.3 to 3 parts by mass, based on 100 parts by mass of the (meth)acrylic copolymer.

[0156] When the content of the photopolymerization initiator (C) is within the above range, appropriate reaction sensitivity to active energy rays can be obtained.

[0157] [Silane coupling agent (D)]

[0158] In addition, in order to improve the adhesion to the components for image display devices, especially to glass, the resin composition preferably contains a silane coupling agent (D). Among them, the silane coupling agent (D) is preferably contained in the resin composition forming the (meth) acrylic adhesive layer in contact with the components for image display devices of the double-sided adhesive sheet.

[0159] Examples of the silane coupling agent (D) include compounds having an unsaturated group such as a vinyl group, an acryloxy group, or a methacryloxy group, an amino group, an epoxy group, and a hydrolyzable functional group such as an alkoxy group.

[0160] As the above-mentioned silane coupling agent (D), for example, N-(β-aminoethyl)-γ-aminopropyl trimethoxysilane, N-(β-aminoethyl)-γ-aminopropyl methyl dimethoxysilane, γ-aminopropyl triethoxysilane, γ-glycidoxypropyl trimethoxysilane, γ-methacryloxypropyl trimethoxysilane, etc. can be cited. They can be used alone or in combination of two or more. Among them, γ-glycidoxypropyl trimethoxysilane is preferred from the aspects of good adhesion to the constituent members of the image display device, less discoloration such as yellowing, etc.

[0161] The content of the silane coupling agent (D) is preferably 0.01 to 5 parts by mass, particularly preferably 0.2 to 3 parts by mass, based on 100 parts by mass of the (meth)acrylic copolymer.

[0162] In addition, similarly to the silane coupling agent (D), a coupling agent such as an organic titanate compound can also be effectively utilized.

[0163] [Metal anticorrosion agent (E)]

[0164] The resin composition preferably further contains a metal corrosion inhibitor (E). Among them, the metal corrosion inhibitor (E) is preferably contained in the resin composition forming the (meth)acrylic adhesive layer in contact with the image display device component of the double-sided adhesive sheet.

[0165] Examples of the metal corrosion inhibitor (E) include benzotriazole compounds, benzimidazole compounds, benzothiazole compounds, and other triazole derivatives.

[0166] As the metal corrosion inhibitor, it is preferred to be any one or more selected from benzotriazole compounds, 1,2,3-triazole and 1,2,4-triazole. Among them, from the perspective of excellent metal corrosion resistance and reliability as a double-sided adhesive sheet, triazole derivatives such as 1,2,3-triazole and 1,2,4-triazole are preferred, and 1,2,3-triazole is particularly preferred.

[0167] The content of the metal anticorrosion agent (E) is preferably 0.01 to 5 parts by mass, more preferably 0.03 to 1 part by mass, and particularly preferably 0.05 to 0.5 parts by mass based on 100 parts by mass of the (meth)acrylic copolymer, from the viewpoint of metal anticorrosion agent bleeding and metal anticorrosion effect.

[0168] [Other additives]

[0169] In the resin combination, other additives may also be included in addition to the above-mentioned components. As the above-mentioned other additives, for example, various additives such as light stabilizer, ultraviolet absorber, metal deactivator, antioxidant, antistatic agent, hygroscopic agent, foaming agent, defoamer, inorganic particles, viscosity modifier, tackifying resin, photosensitizer, fluorescent agent, reaction catalyst (tertiary amine compound, quaternary ammonium compound, tin laurate compound, etc.) etc. can be cited. They can be used alone or in combination of two or more.

[0170] In addition, known components generally blended in a resin composition forming an adhesive may be appropriately contained.

[0171] The above-mentioned resin composition can be obtained by mixing a predetermined amount of a (meth) acrylic copolymer, a crosslinking agent (B) as required, a photopolymerization initiator (C), a silane coupling agent (D), a metal preservative (E) and other additives. There is no particular restriction on their mixing method, and the mixing order of each component is not particularly limited. In addition, a heat treatment process can also be introduced when manufacturing the resin composition. In this case, it is desirable to heat-treat the components of the resin composition after mixing them in advance. In the above-mentioned mixing, various mixed components can be concentrated and masterbatched.

[0172] In addition, as mentioned above, as mixing method, there is no particular restriction yet, for example, a universal mixer, planetary mixer, Banbury mixer, kneader, frame mixer, pressurized kneader, three-roll grinder, double-roll grinder etc. can be used. When each component of resin combination is mixed, solvent can be used to mix as required. In addition, resin combination can also be used as solvent-free system without solvent. By using as solvent-free system, the advantages of no residual solvent, heat resistance and light resistance improving can be possessed.

[0173] [Method for producing double-sided adhesive sheet]

[0174] The following describes the method for manufacturing the double-sided adhesive sheet of the present invention, but is not limited to the method. The double-sided adhesive sheet of the present invention preferably has at least 2 layers of (meth) acrylic adhesive layers, and more preferably has at least 3 layers in which the outermost layer and the innermost layer are set as (meth) acrylic adhesive layers. The double-sided adhesive sheet of the present invention is preferably typically manufactured by the following steps to have a double-sided adhesive sheet with a release film having a structure formed by laminating a double-sided adhesive sheet and a release film. It should be noted that the pre-curing of the following steps can also be omitted.

[0175] First, a (meth) acrylic adhesive layer (or intermediate layer) with a release film is prepared. The (meth) acrylic adhesive layer (or intermediate layer) with a release film can be obtained by heating and melting a resin composition (hot melting), applying the obtained substance on a release film, and further sandwiching and heating with other release films. The (meth) acrylic adhesive layer (or intermediate layer) with a release film is prepared according to the number of layers required for the double-sided adhesive sheet.

[0176] As the above-mentioned release film, for example, films comprising polyester resin, polyolefin resin, polycarbonate resin, polystyrene resin, acrylic resin, triacetyl cellulose resin, fluororesin, etc. can be cited. In addition, those formed by coating these films with silicone resin and performing release treatment, release paper, etc. can also be appropriately selected and used. Among them, polyester resin and polyolefin resin are preferred, and polyester resin and polyolefin resin that have been subjected to release treatment are particularly preferred. Furthermore, it is also preferred to use release films having different peeling forces and release films having different thicknesses on both sides of the (meth) acrylic adhesive layer.

[0177] Next, the release film is peeled off from the obtained (meth)acrylic PSA layer (or intermediate layer) with the release film, and a (meth)acrylic PSA layer (or intermediate layer) is laminated to obtain the double-sided PSA sheet of the present invention laminated with the release film.

[0178] In addition, in the case of a double-sided adhesive sheet having at least three layers in which the outermost layer and the innermost layer are set as (meth) acrylic adhesive layers, for example, a double-sided adhesive sheet having three layers of outermost layer (adhesive layer) / middle layer / innermost layer (adhesive layer), the present adhesive sheet can be prepared by the following methods: a method in which the above-mentioned resin composition is applied on a release film to form the outermost layer, a resin composition for forming an intermediate layer is applied on the formed outermost layer to form an intermediate layer, and the innermost layer is further formed on the formed intermediate layer; a method in which the resin composition is applied on a release film in the same manner as described above to form the outermost layer and the intermediate layer in advance, and then the coated surfaces are bonded to each other; a method in which the resin composition is simultaneously formed into the outermost layer, the intermediate layer, and the innermost layer by multilayer coating and co-extrusion molding; etc.

[0179] In addition to the above method, a multilayer double-sided adhesive sheet can also be produced by, for example, coating a resin composition on a release film to form a (meth)acrylic adhesive layer, and then further coating another resin composition on the formed (meth)acrylic adhesive layer to form a resin layer, and repeating this operation to produce a multilayer double-sided adhesive sheet.

[0180] The obtained double-sided adhesive sheet is preferably cross-linked and pre-cured by active energy rays in a manner having potential active energy ray reactivity, in other words, in a manner that the active energy ray reactivity remains. In the case of pre-curing, active energy rays can be irradiated through the release film to cross-link each layer by active energy rays. At this time, the degree of active energy ray cross-linking can be adjusted by controlling the irradiation amount of active energy rays, but as mentioned above, the degree of active energy ray cross-linking can also be adjusted by irradiating ultraviolet rays through the release film to block a part of the active energy rays.

[0181] The double-sided adhesive sheet thus obtained is an optically transparent adhesive sheet. Here, “optically transparent” is intended to mean that the total light transmittance is 80% or more, preferably 85% or more, and more preferably 90% or more.

[0182] The double-sided adhesive sheet of the present invention is usually circulated in a state where the (meth) acrylic adhesive layers on both sides are sandwiched by release films. In addition, when using the double-sided adhesive sheet, the release film can be peeled off from the (meth) acrylic adhesive layer to make the (meth) acrylic adhesive layer adhere to the image display component.

[0183] (Explanation of terms, etc.)

[0184] It should be noted that, generally, "sheet" refers to a thin product with a small thickness in length and width as defined in JIS, and generally, "film" refers to a thin and flat product with a very small thickness compared to length and width and an arbitrarily limited maximum thickness, and is generally supplied in the form of a roll (Japanese Industrial Standard JIS K6900). However, the boundary between sheet and film is unclear, and there is no need to distinguish between the two in words in the present invention. Therefore, in the present invention, the case of "film" also includes "sheet", and the case of "sheet" also includes "film".

[0185] In addition, when the term "panel" is used, such as an image display panel, a protective panel, etc., it includes a plate body, a sheet, and a film.

[0186] In the present specification, when "x to y" is described (x and y are arbitrary numbers), unless otherwise specified, it includes the meaning of "x or more and y or less", and includes the meaning of "preferably greater than x" and "preferably less than y".

[0187] In addition, when recorded as "or more than x" (x is an arbitrary number), unless otherwise specified, it includes the meaning of "or more than x" and includes the meaning of "preferably greater than x", and when recorded as "or less than y" (y is an arbitrary number), unless otherwise specified, it includes the meaning of "or less than y" and includes the meaning of "preferably less than y".

[0188] Example

[0189] Hereinafter, the present invention will be described in more detail based on Examples and Comparative Examples, but the present invention is not limited to these Examples.

[0190] In the examples, the hydroxyl value, mass average molecular weight, and glass transition temperature of the (meth)acrylic copolymer were measured according to the following methods.

[0191] <Hydroxy value>

[0192] The hydroxyl value of the (meth)acrylic copolymer is measured by a neutralization titration method.

[0193] Collect 2g of sample in a conical flask, add 10mL of a mixed solution of acetic anhydride:pyridine=1:13 with a full pipette, and further add 10mL of toluene. Install an air condenser on the top of the conical flask and heat at 95°C for 90 minutes. After heating, add 10mL of toluene and 10mL of pure water, and cool naturally while stirring to room temperature (23°C). Then, add a few drops of phenolphthalein solution and titrate with 0.1mol / L potassium hydroxide solution. In addition, as a blank test, perform the same operation as above without collecting a sample in the conical flask. Calculate the hydroxyl value based on the following calculation formula (1).

[0194] [Calculation formula]

[0195] Hydroxyl value = 5.611 × (Vb-Vt) × f / Ws + Av…(1)

[0196] In formula (1), Vb is the amount of potassium hydroxide solution used in the blank test (mL), Vt is the amount of potassium hydroxide solution used in the titration (mL), f is the coefficient of 0.1 mol / L potassium hydroxide solution, Ws is the amount of sample collected (g), and Av is the acid value.

[0197] 〔Acid value〕

[0198] The acid value is measured by the following method. The (meth)acrylic acid copolymer Yg is collected in a beaker and dissolved in a mixed solvent of toluene:methanol=7:3. After dissolution, an appropriate amount of phenolphthalein is added, and the mixture is titrated with a 0.1 mol / L potassium hydroxide solution while stirring with a stirrer. The amount of potassium hydroxide solution XmL when the solution turns light pink is read as the end point, and the acid value is calculated based on the following calculation formula (2).

[0199] [Calculation formula]

[0200] Acid value (mgKOH / g) = X × (f × M × 56.1) / Y… (2)

[0201] f: coefficient of potassium hydroxide solution

[0202] M: molar concentration (mol / L)

[0203] X: Potassium hydroxide solution volume (mL)

[0204] Y: Sample amount (g)

[0205] It should be noted that when the acid value is low, a 0.01 mol / L KOH solution is used to improve the accuracy.

[0206] <Mass average molecular weight>

[0207] The mass average molecular weight of the (meth)acrylic copolymer was measured using a gel permeation chromatography (GPC) analyzer (manufactured by Tosoh Corporation, HLC-8320GPC). Specifically, 4 mg of the (meth)acrylic copolymer was dissolved in 12 mL of THF as a measurement sample, and a molecular weight distribution curve was measured under the following conditions to determine the mass average molecular weight (Mw).

[0208] Guard column: TSKguardcolumnHXL

[0209] Separation column: TSKgelGMHXL (4 columns)

[0210] Temperature: 40℃

[0211] Injection volume: 100μL

[0212] Polystyrene conversion

[0213] Solvent: THF

[0214] Flow rate: 1.0mL / min

[0215] <Glass transition temperature (Tg)>

[0216] The glass transition temperature (Tg) of the (meth)acrylic copolymer was measured using a rheometer (manufactured by TA Instruments, "Discovery HR2"). Specifically, for a (meth)acrylic copolymer having a thickness of 0.6 to 0.8 mm, a dynamic viscoelastic spectrum was measured in a temperature range of -120 to 200°C under the conditions of a jig: Φ8 mm parallel plate, a strain: 0.1%, a frequency: 1 Hz, a temperature: -120 to 200°C, and a heating rate: 5°C / min, and the temperature at which the loss tangent (Tanδ) reached a maximum value was read from the obtained data to determine the glass transition temperature (Tg).

[0217] <Example 1>

[0218] 1 kg of a copolymer (A'-1) (mass average molecular weight 290,000, Tg 4°C) comprising 2-ethylhexyl acrylate / methyl acrylate / methyl methacrylate / isobornyl methacrylate / acrylamide as a (meth)acrylic copolymer, 100 g of propoxylated pentaerythritol triacrylate (B-1) as a crosslinking agent (B), and 5 g of a mixture (C-1) of 2,4,6-trimethylbenzophenone and 4-methylbenzophenone as a photopolymerization initiator (C) were uniformly melt-kneaded to prepare a resin composition (1).

[0219] 1 kg of a copolymer (A-1) containing 2-ethylhexyl acrylate / 2-hydroxyethyl acrylate / methyl acrylate as a (meth)acrylic copolymer (mass average molecular weight 440,000, Tg-25°C, hydroxyl value 67 mgKOH / g), 10 g of a photopolymerization initiator (C-1), and 1 g of 3-glycidoxypropyltrimethoxysilane (D-1) as a silane coupling agent (D) were uniformly melt-kneaded to prepare a resin composition (2).

[0220] The resin composition (1) was sandwiched between two release-treated polyethylene terephthalate films ("DIAFOIL MRF (thickness 75 μm)" manufactured by Mitsubishi Chemical Corporation / "DIAFOIL MRT (thickness 38 μm)" manufactured by Mitsubishi Chemical Corporation), i.e., two release films, and formed into a sheet at a temperature of 80°C so as to have a thickness of 50 μm to prepare an intermediate layer sheet (S-1).

[0221] The resin composition (2) was sandwiched between two release-treated polyethylene terephthalate films ("DIAFOIL MRF (thickness 75 μm)" manufactured by Mitsubishi Chemical Corporation / "DIAFOIL MRT (thickness 38 μm)" manufactured by Mitsubishi Chemical Corporation), i.e., two release films, and formed into a sheet at a temperature of 80°C so as to have a thickness of 25 μm, thereby preparing two pressure-sensitive adhesive sheets (S-2) for the front and inner layers.

[0222] The intermediate layer sheet (S-1) with the release films on both sides peeled off was attached to the adhesive surface of the front and inner layer pressure-sensitive adhesive sheet (S-2) with the release film on one side peeled off to prepare a laminate having a layer structure of (S-2) / (S-1) / (S-2).

[0223] The accumulated light intensity at a wavelength of 365 nm was 2000 mJ / cm 2 The double-sided adhesive sheet (precured product) of Example 1 was prepared by irradiating light with a high-pressure mercury lamp for precuring.

[0224] It should be noted that in the double-sided PSA sheet of Example 1, the shear storage modulus (G') of the front and rear layers at 25°C is lower than that of the middle layer, and any layer has room for photocuring by light irradiation.

[0225] <Example 2>

[0226] 1 kg of the (meth)acrylic copolymer (A-1), 10 g of the photopolymerization initiator (C-1), and 1 g of 1,2,3-triazole (E-1) as a metal anticorrosive agent (E) were uniformly melt-kneaded to prepare a resin composition (3).

[0227] It should be noted that the metal preservative (E-1) has an absorption coefficient of 0.3 mL / (g·cm) at 365 nm and a water solubility of more than 1000 g / L at 25°C.

[0228] The resin composition (1) prepared in the above-mentioned Example 1 was sandwiched between two polyethylene terephthalate films ("DIAFOIL MRF (thickness 75μm)" manufactured by Mitsubishi Chemical Corporation / "DIAFOIL MRT (thickness 38μm)" manufactured by Mitsubishi Chemical Corporation) that had been subjected to mold release treatment, i.e., two mold release films, and was formed into a sheet at a temperature of 80°C in such a way that the thickness became 67μm to prepare an intermediate layer sheet (S-1).

[0229] The resin composition (3) was sandwiched between two release-treated polyethylene terephthalate films ("DIAFOIL MRF (thickness 75 μm)" manufactured by Mitsubishi Chemical Corporation / "DIAFOIL MRT (thickness 38 μm)" manufactured by Mitsubishi Chemical Corporation), i.e., two release films, and formed into a sheet at a temperature of 80°C so as to have a thickness of 17 μm, thereby preparing two adhesive sheets (S-3) for the front and inner layers.

[0230] The intermediate layer sheet (S-1) from which the release films on both sides were peeled off was attached to the adhesive surface of the front and inner layer pressure-sensitive adhesive sheet (S-3) from which the release films on one side were peeled off to prepare a laminate having a layer structure of (S-3) / (S-1) / (S-3).

[0231] The accumulated light intensity at a wavelength of 365 nm was 1000 mJ / cm 2 In this manner, light was irradiated with a high-pressure mercury lamp to perform pre-curing, thereby producing a double-sided adhesive sheet (pre-cured product) of Example 2.

[0232] It should be noted that in the double-sided PSA sheet of Example 2, the shear storage modulus (G') of the front and rear layers at 25°C is lower than that of the middle layer, and any layer has room for photocuring by light irradiation.

[0233] <Example 3>

[0234] 1 kg of a (meth)acrylic copolymer (A'-1), 100 g of a crosslinking agent (B-1), 4 g of a photopolymerization initiator (C-1), and 4 g of oligo(2-hydroxy-2-methyl-1-(4-(1-methylvinyl)phenyl)propanone) (C-2) were uniformly melt-kneaded to prepare a resin composition (4).

[0235] The resin composition (4) was sandwiched between two release-treated polyethylene terephthalate films ("DIAFOIL MRF (thickness 75 μm)" manufactured by Mitsubishi Chemical Corporation / "DIAFOIL MRT (thickness 38 μm)" manufactured by Mitsubishi Chemical Corporation), i.e., two release films, and formed into a sheet at a temperature of 80°C so as to have a thickness of 75 μm to prepare an intermediate layer sheet (S-4).

[0236] The resin composition (2) prepared in the above-mentioned Example 1 was sandwiched between two polyethylene terephthalate films ("DIAFOIL MRF (thickness 75μm)" manufactured by Mitsubishi Chemical Corporation / "DIAFOIL MRT (thickness 38μm)" manufactured by Mitsubishi Chemical Corporation) that had been subjected to mold release treatment, i.e., two mold release films, and was formed into a sheet at a temperature of 80°C in such a way that the thickness became 13μm, thereby preparing two adhesive sheets (S-2) for the front and inner layers.

[0237] The intermediate layer sheet (S-4) with the release films on both sides peeled off was attached to the adhesive surface of the front and inner layer pressure-sensitive adhesive sheet (S-2) with the release film on one side peeled off to prepare a laminate having a layer structure of (S-2) / (S-4) / (S-2).

[0238] The accumulated light intensity at a wavelength of 365 nm was 1000 mJ / cm 2 In this manner, light was irradiated with a high-pressure mercury lamp to perform pre-curing, thereby producing a double-sided adhesive sheet (pre-cured product) of Example 3.

[0239] It should be noted that in the double-sided PSA sheet of Example 3, the shear storage modulus (G') of the front and rear layers at 25°C is lower than that of the middle layer, and any layer has room for photocuring by light irradiation.

[0240] <Comparative Example 1>

[0241] 1 kg of the (meth)acrylic copolymer (A-1), 200 g of the crosslinking agent (B-1), and 8 g of the photopolymerization initiator (C-1) were uniformly melt-kneaded to prepare a resin composition (5).

[0242] 1 kg of the (meth)acrylic copolymer (A-1) and 10 g of the photopolymerization initiator (C-1) were uniformly melt-kneaded to prepare a resin composition (6).

[0243] The resin composition (5) was sandwiched between two release-treated polyethylene terephthalate films ("DIAFOIL MRF (thickness 75 μm)" manufactured by Mitsubishi Chemical Corporation / "DIAFOIL MRT (thickness 38 μm)" manufactured by Mitsubishi Chemical Corporation), i.e., two release films, and formed into a sheet at a temperature of 80°C so as to have a thickness of 67 μm to prepare an intermediate layer sheet (S-5).

[0244] The resin composition (6) was sandwiched between two release-treated polyethylene terephthalate films ("DIAFOIL MRF (thickness 75 μm)" manufactured by Mitsubishi Chemical Corporation / "DIAFOIL MRT (thickness 38 μm)" manufactured by Mitsubishi Chemical Corporation), i.e., two release films, and formed into a sheet at a temperature of 80°C so as to have a thickness of 17 μm, thereby preparing two adhesive sheets (S-6) for the front and inner layers.

[0245] The intermediate layer sheet (S-5) with the release films on both sides peeled off was attached to the adhesive surface of the outer layer pressure-sensitive adhesive sheet (S-6) with the release film on one side peeled off to produce a laminate having a layer structure of (S-6) / (S-5) / (S-6).

[0246] The accumulated light intensity at a wavelength of 365 nm was 2000 mJ / cm 2 The double-sided adhesive sheet of Comparative Example 1 (precured product) was prepared by irradiating light with a high-pressure mercury lamp for precuring.

[0247] In the double-sided PSA sheet of Comparative Example 1, the shear storage modulus (G') of the front and rear layers at 25°C is lower than that of the middle layer, and any layer has room for photocuring by light irradiation.

[0248] <Comparative Example 2>

[0249] 1 kg of the (meth)acrylic copolymer (A′-1), 100 g of the crosslinking agent (B-1), 5 g of the photopolymerization initiator (C-1), and 1 g of the additive (D-1) were uniformly melt-kneaded to prepare a resin composition (7).

[0250] The resin composition (7) was sandwiched between two release-treated polyethylene terephthalate films ("DIAFOIL MRF (thickness 75 μm)" manufactured by Mitsubishi Chemical Corporation / "DIAFOIL MRT (thickness 38 μm)" manufactured by Mitsubishi Chemical Corporation), i.e., two release films, and shaped into a sheet at a temperature of 80°C so as to have a thickness of 100 μm, and the accumulated light amount at a wavelength of 365 nm was 1000 mJ / cm 2 In a manner of , light was irradiated from one side of the release film with a high-pressure mercury lamp to perform pre-curing, thereby producing a double-sided pressure-sensitive adhesive sheet (pre-cured product) of Comparative Example 2.

[0251] It should be noted that the (meth)acrylic pressure-sensitive adhesive layer in the double-sided pressure-sensitive adhesive sheet of Comparative Example 2 has room for photocuring by light irradiation.

[0252] <Comparative Example 3>

[0253] A resin composition (8) was prepared by uniformly melt-kneading 1 kg of a copolymer (A"-1) (mass average molecular weight 540,000, Tg 1°C, hydroxyl value 62 mgKOH / g) containing methyl acrylate / ethyl acrylate / 2-ethylhexyl acrylate / 2-hydroxyethyl acrylate as a (meth)acrylic copolymer, 100 g of polypropylene glycol diacrylate (B-2, molecular weight 536) as a crosslinking agent (B), 10 g of a photopolymerization initiator (C-1), and 1 g of an additive (D-1) to produce a resin composition (8).

[0254] The resin composition (8) was sandwiched between two release-treated polyethylene terephthalate films ("DIAFOIL MRF (thickness 75 μm)" manufactured by Mitsubishi Chemical Corporation / "DIAFOIL MRT (thickness 38 μm)" manufactured by Mitsubishi Chemical Corporation), i.e., two release films, and shaped into a sheet at a temperature of 80°C so as to have a thickness of 100 μm, and the accumulated light amount at a wavelength of 365 nm was 1000 mJ / cm 2In a manner of , light was irradiated from one side of the release film with a high-pressure mercury lamp to perform pre-curing, thereby producing a double-sided adhesive sheet (pre-cured product) of Comparative Example 3.

[0255] It should be noted that the (meth)acrylic pressure-sensitive adhesive layer in the double-sided pressure-sensitive adhesive sheet of Comparative Example 3 has room for photocuring by light irradiation.

[0256] <Comparative Example 4>

[0257] 1 kg of the (meth)acrylic copolymer (A-1), 180 g of the substance (B-3) as the crosslinking agent (B), and 10 g of the photopolymerization initiator (C-1) were uniformly melt-kneaded to prepare a resin composition (9).

[0258] 1 kg of the (meth)acrylic copolymer (A-1) and 12 g of the photopolymerization initiator (C-1) were uniformly melt-kneaded to prepare a resin composition (10).

[0259] The resin composition (9) was sandwiched between two release-treated polyethylene terephthalate films ("DIAFOIL MRF (thickness 75 μm)" manufactured by Mitsubishi Chemical Corporation / "DIAFOIL MRT (thickness 38 μm)" manufactured by Mitsubishi Chemical Corporation), i.e., two release films, and formed into a sheet at a temperature of 80°C so as to have a thickness of 67 μm to prepare an intermediate layer sheet (S-9).

[0260] The resin composition (10) was sandwiched between two release-treated polyethylene terephthalate films ("DIAFOIL MRF (thickness 75 μm)" manufactured by Mitsubishi Chemical Corporation / "DIAFOIL MRT (thickness 38 μm)" manufactured by Mitsubishi Chemical Corporation), i.e., two release films, and formed into a sheet at a temperature of 80°C so as to have a thickness of 17 μm, thereby preparing two adhesive sheets (S-10) for the front and inner layers.

[0261] The intermediate layer sheet (S-9) from which the release films on both sides were peeled off was attached to the adhesive surface of the front and inner layer pressure-sensitive adhesive sheet (S-10) from which the release films on one side were peeled off to prepare a laminate having a layer structure of (S-10) / (S-9) / (S-10).

[0262] The accumulated light intensity at a wavelength of 365 nm was 2000 mJ / cm 2 The double-sided adhesive sheet (precured product) of Comparative Example 4 was prepared by irradiating light with a high-pressure mercury lamp for precuring.

[0263] In the double-sided PSA sheet of Comparative Example 4, the shear storage modulus (G') of the front and rear layers at 25°C is lower than that of the middle layer, and any layer has room for photocuring by light irradiation.

[0264] [Physical property evaluation]

[0265] The physical properties of the double-sided adhesive sheets of Examples 1 to 3 and Comparative Examples 1 to 4 obtained above were measured as follows. In addition, for the physical properties of each layer independently, after preparing the sheets for each layer, they were pre-cured under the same conditions and the obtained ones were used for measurement. The double-sided adhesive sheets of Examples 1 to 3 and Comparative Examples 1 to 4 and the physical properties of each layer independently are shown in Table 1 described below.

[0266] <Peak temperature (T1) of shear storage modulus (G') and loss tangent (Tanδ)>

[0267] For each of the double-sided adhesive sheets (pre-cured products) of Examples 1 to 3 and Comparative Examples 1 to 4, i.e., the double-sided adhesive sheets before curing (hereinafter collectively referred to as "double-sided adhesive sheets before curing"), two release films were peeled off, the adhesive sheets were stacked in a manner to have a thickness of 0.6 to 0.8 mm, and punched into a circle with a diameter of 8 mm, and the resulting pieces were used as measurement samples.

[0268] The dynamic viscoelastic spectrum in the shear mode was measured using a rheometer (manufactured by TA Instruments, "Discovery HR2") in the temperature range of -120 to 200°C under the following conditions: bonding jig: Φ8 mm parallel plate, strain: 0.1%, frequency: 1 Hz, temperature: -120 to 200°C, and heating rate: 5°C / min. The shear storage modulus (G') of the double-sided adhesive sheet before curing at a temperature of 25°C was determined from the obtained data.

[0269] In addition, the peak temperature (T1) at which the loss tangent (Tanδ) of the obtained dynamic viscoelastic spectrum data reaches a maximum value is read.

[0270] Next, the accumulated light intensity at a wavelength of 365 nm is 3000 mJ / cm 2 In a manner, the pre-cured double-sided adhesive sheet is irradiated with light using a high-pressure mercury lamp to perform photocuring, thereby preparing a cured double-sided adhesive sheet.

[0271] For each of the above-mentioned double-sided adhesive sheets after curing (hereinafter collectively referred to as "double-sided adhesive sheets after curing"), the two release films were peeled off in the same manner as above, and the adhesive sheets were stacked in a manner of 0.6 to 0.8 mm in thickness, and punched into a circle with a diameter of 8 mm, and the obtained was used as a measurement sample. For this measurement sample, under the same measurement conditions as the double-sided adhesive sheet before curing, the dynamic viscoelastic spectrum in the shear mode was measured, and the storage modulus (G') of the double-sided adhesive sheet after curing at a temperature of 25°C was calculated from the obtained data.

[0272] In addition, the peak temperature (T1) at which the loss tangent (Tanδ) of the obtained dynamic viscoelastic spectrum data reaches a maximum value is read.

[0273] <Peak temperature (T2) of tensile storage modulus (E') and loss tangent (Tanδ)>

[0274] The accumulated light intensity at a wavelength of 365 nm for each of the double-sided PSA sheets (pre-cured products) of Examples 1 to 3 and Comparative Examples 1 to 4, i.e., the double-sided PSA sheets before curing, was 3000 mJ / cm 2 The double-sided adhesive sheet before curing was photocured by irradiating light with a high-pressure mercury lamp and then cut into a sample size of 4 mm wide × 15 mm long. A dynamic viscoelasticity measuring device (IT Meter and Control, itkDVA-200) was used to measure the dynamic viscoelasticity spectrum in the tensile mode under the conditions of a vibration frequency of 1 Hz, a measuring temperature of -120 to 80°C, and a heating rate of 3°C / min. The tensile storage modulus (E') of the double-sided adhesive sheet after curing at a temperature of 25°C was determined from the obtained data.

[0275] In addition, the peak temperature (T2) at which the loss tangent (Tanδ) of the obtained dynamic viscoelastic spectrum data reaches a maximum value is read.

[0276] The double-sided PSA sheets of Examples 1 to 3 and Comparative Examples 1 to 4 obtained above were used to perform the following evaluations. The evaluation results are shown in Table 1 described below.

[0277] <180° peel adhesion>

[0278] For each of the double-sided adhesive sheets (pre-cured products) of Examples 1 to 3 and Comparative Examples 1 to 4, one release film was peeled off and a 100 μm PET film (manufactured by Mitsubishi Chemical Corporation, "DIAFOIL T100") was bonded as a substrate film. After cutting it into a length of 150 mm and a width of 20 mm, the adhesive surface exposed by peeling off the remaining release film was roll-bonded to a soda-lime glass plate to form a bonded product. The bonded product was subjected to autoclave treatment (60°C, gauge pressure 0.2 MPa, 20 minutes) for precision bonding, and a high-pressure mercury lamp was used, with the accumulated light intensity at 365 nm being 3000 mJ / cm 2 In the manner of , light was irradiated from the PET film surface, and then aged at a temperature of 23° C. and 50% RH for 12 hours to prepare a sample for measuring 180° peeling adhesive strength.

[0279] The samples were tested for peeling force (N / 20mm) at a peeling angle of 180° and a peeling speed of 300mm / min at a temperature of 23°C and 50%RH. The samples were easily peeled at a peeling angle of 180° and a peeling speed of 300mm / min at a peeling angle of 180°. The samples were judged as "× (bad)" if the peeling force was less than 5N / 20mm, and "○ (good)" if the peeling force was greater than 5N / 20mm.

[0280] <Reworkability>

[0281] The double-sided adhesive sheets (precured products) of Examples 1 to 3 and Comparative Examples 1 to 4 were cut into a size of 52 mm × 80 mm with a release film laminated thereon using a Thomson punching machine. The release film on one side was peeled off, and the exposed adhesive surface was bonded to a soda-lime glass plate (54 mm × 82 mm, thickness 0.6 mm) using a hand roller.

[0282] Next, the release film on the adhesive side of the polarizing plate (VLC2 manufactured by Sanritz) was peeled off, and a polyethylene terephthalate film (DIAFOIL T100 manufactured by Mitsubishi Chemical Corporation, 54 mm×82 mm, thickness 38 μm) was bonded to the exposed adhesive surface using a hand roller. Furthermore, the other release film of the double-sided adhesive sheet bonded to the soda-lime glass plate was peeled off, and bonded to the polarizing plate from which the protective film on the polarizing plate side was peeled off using a hand roller.

[0283] Next, the film was subjected to autoclave treatment (60°C, gauge pressure 0.2 MPa, 20 minutes) for fine bonding, and then a high-pressure mercury lamp was used to achieve a cumulative light intensity of 3000 mJ / cm at 365 nm. 2 The adhesive sheet was photocured (post-cured product) by irradiating light from the soda-lime glass plate side. After that, the adhesive sheet was aged at room temperature (23° C.) for 12 hours to prepare a sample for rework evaluation (soda-lime glass plate / double-sided adhesive sheet / polarizing plate with adhesive tape / PET film).

[0284] The soda lime glass plate was placed on a SUS cooling plate (surface temperature -120°C) in such a way that the soda lime glass plate was in contact with the cooling plate (soda lime glass plate was on the lower side), and the time until the soda lime glass plate and the polarizing plate separated was measured. The above-mentioned reworkability evaluation samples were prepared for each double-sided adhesive sheet, and 5 measurements were performed for each sheet, and the evaluation was performed as follows based on the average value of the time until separation.

[0285] The case where the film could be separated within 30 seconds was judged as "◎ (very good)", the case where the film did not peel within 30 seconds but could be separated within 120 seconds was judged as "○ (good)", and the case where the film could not be separated after more than 120 seconds and was not suitable for practical use was judged as "× (poor)".

[0286] <Absorption of height difference>

[0287] The double-sided pressure-sensitive adhesive sheets (pre-cured products) of Examples 1 to 3 and Comparative Examples 1 to 4 were each cut into a size of 52 mm×80 mm using a Thomson punching machine while a release film was laminated thereon.

[0288] The release film on one side was peeled off, and the exposed adhesive surface was press-bonded (temperature 25°C, pressurization pressure 0.1 MPa) to the printed surface of a soda-lime glass plate (82 mm × 54 mm × thickness 0.5 mm) with a printed surface having a thickness of 15 μm or 25 μm applied to the 5 mm peripheral edge portion using a vacuum press machine in such a way that a printing height difference was applied to the four sides of the double-sided adhesive sheet.

[0289] Then, the remaining release film was peeled off, and a soda-lime glass plate (82 mm × 54 mm × thickness 0.5 mm) without a printing height difference was pressed and laminated, and then subjected to autoclave treatment (60°C, gauge pressure 0.2 MPa, 20 minutes) for fine bonding to produce a laminate (soda-lime glass plate with a printing height difference / double-sided adhesive sheet / soda-lime glass plate).

[0290] The produced laminate was visually observed and evaluated as follows.

[0291] The case where the double-sided adhesive sheet does not follow the printing height difference and bubbles remain near it, and is not suitable for bonding with the printing height difference, will be judged as "× (normal)"; the case where there are no bubbles at a printing height difference of 15μm and the bonding can be good in appearance, but bubbles remain at a printing height difference of 25μm will be judged as "○ (good)"; the case where there are no bubbles at both printing height differences of 15μm and 25μm and the bonding can be good in appearance will be judged as "◎ (very good)".

[0292] <Lamination reliability>

[0293] Using a Thomson punching machine, the double-sided adhesive sheets (precured products) of the above-mentioned Examples 1 to 3 and Comparative Examples 1 to 4 were cut into a size of 52 mm × 80 mm in a state where a release film was laminated. The release film on one side was peeled off, and the exposed adhesive surface was bonded to the first soda-lime glass plate (54 mm × 82 mm, thickness 0.6 mm) with a hand roller. Next, the release film on the adhesive side of the adhesive polarizing plate (made by Sanritz, "VLC2") was peeled off, and the exposed adhesive surface was bonded to the second soda-lime glass plate (54 mm × 82 mm, thickness 0.6 mm) with a hand roller. Furthermore, the other release film of each double-sided adhesive sheet bonded to the first soda-lime glass plate was peeled off, and a hand roller was bonded to the polarizing plate from which the protective film on the polarizing plate side was peeled off.

[0294] Next, the film was subjected to autoclave treatment (60°C, gauge pressure 0.2 MPa, 20 minutes) for fine bonding, and then a high-pressure mercury lamp was used to achieve a cumulative light intensity of 3000 mJ / cm at 365 nm. 2 The adhesive sheet was photocured (post-cured product) by irradiating light from the first soda-lime glass plate side. After that, it was aged at room temperature (23° C.) for 12 hours to prepare a sample for evaluating heat-resistant foaming (first soda-lime glass plate / double-sided adhesive sheet / polarizing plate with adhesion / second soda-lime glass plate).

[0295] These were left to stand in an environment of 85° C. for 300 hours, and the presence or absence of foaming was visually observed.

[0296] The case where bubbles were generated at the interface of the polarizing plate / double-sided adhesive sheet to be bonded was judged as "× (poor)", and the case where bubbles were not generated and the appearance was good was judged as "○ (good)".

[0297] <ITO corrosion resistance>

[0298] like Figure 1 As shown in (A), the film is formed on a 60 mm × 45 mm glass with a thickness of 0.7 mm, a line width of 70 μm / line spacing of 30 μm (patterning accuracy ± 8 μm), a line length of 46 cm, an electrode size of 5 mm × 5 mm, and an electrode spacing of 50 mm. Substrate for evaluating ITO corrosion resistance.

[0299] The double-sided PSA sheets (pre-cured products) of Examples 1 to 3 and Comparative Examples 1 to 4 were each peeled from their single-sided release films, roll-laminated onto a PET film (DIAFOIL T100 manufactured by Mitsubishi Chemical Corporation, 50 μm thick), and then cut into 52 mm widths.

[0300] Thereafter, the release film on the other side was peeled off, and the adhesive sheet was placed between the electrodes and bonded to the substrate using a roller, followed by autoclave treatment (temperature 60° C., gauge pressure 0.2 MPa, 20 minutes) for fine bonding.

[0301] After that, the accumulated light intensity at a wavelength of 365 nm becomes 2000 mJ / cm 2 The PET film was cured by irradiating light from the PET film side with a high pressure mercury lamp (formal cured product). After that, the film was aged at room temperature for 12 hours to prepare a sample for evaluation of ITO corrosion resistance (refer to Figure 1 (C)).

[0302] The sample was subjected to an environmental test in a hot and humid environment at a temperature of 65°C and 90% RH for 500 hours, and an increase in the resistance value between the electrodes was confirmed (see Figure 1 In the above environmental test, the case where the resistance value rises by more than 4% is judged as "× (bad)", the case where the resistance value rise is suppressed to more than 3% and less than 4% is judged as "○ (good)", and the case where the resistance value rise is further suppressed to less than 3% is judged as "◎ (very good)".

[0303] <Cu corrosion resistance>

[0304] like Figure 1 As shown in (A), the following preparations were made: on a glass of 60 mm × 45 mm and 0.7 mm thickness, the films were formed in sequence under the patterning conditions of line width 70 μm / line spacing 30 μm (patterning accuracy ± 8 μm), line length 46 cm, electrode size 5 mm × 5 mm, and electrode spacing 50 mm. Copper (Cu) A substrate for evaluating Cu corrosion resistance.

[0305] The double-sided PSA sheets (pre-cured products) of Examples 1 to 3 and Comparative Examples 1 to 4 were each peeled from their single-sided release films, roll-laminated onto a PET film (DIAFOIL T100 manufactured by Mitsubishi Chemical Corporation, 50 μm thick), and then cut into 52 mm widths.

[0306] Thereafter, the release film on the other side was peeled off, and the adhesive sheet was placed between the electrodes and bonded to the substrate using a roller, followed by autoclave treatment (temperature 60° C., gauge pressure 0.2 MPa, 20 minutes) for fine bonding.

[0307] After that, the accumulated light intensity at a wavelength of 365 nm becomes 3000 mJ / cm 2 The PET film is irradiated with light from the side with a high-pressure mercury lamp to perform light curing (formal cured product).

[0308] Then, the samples were aged at room temperature (23° C.) for 12 hours to prepare samples for evaluation of Cu corrosion resistance (refer to Figure 1 (D)).

[0309] The sample was subjected to an environmental test in a hot and humid environment at a temperature of 65°C and 90% RH for 500 hours, and an increase in the resistance value between the electrodes was confirmed (see Figure 1 In the above environmental test, the case where the resistance value rises by more than 3% is judged as "× (bad)", the case where the resistance value rise is suppressed to more than 1% and less than 3% is judged as "○ (good)", and the case where the resistance value rise is further suppressed to less than 1% is judged as "◎ (very good)".

[0310] [Table 1]

[0311]

[0312] For the double-sided adhesive sheets of Examples 1 to 3, the ratio of the tensile storage modulus (E') to the shear storage modulus (G') is 5.0 or more, the peak temperature (T1) of the loss tangent (Tanδ) obtained by the dynamic viscoelasticity measurement in the shear mode with a frequency of 1 Hz is below -10°C, the peak temperature (T2) of the loss tangent (Tanδ) obtained by the dynamic viscoelasticity measurement in the tensile mode with a frequency of 1 Hz is above -10°C, and the adhesive force is 5N / 20mm or more, so it has both height difference absorption, reliability, metal corrosion resistance, and excellent reworkability. Among them, the transparent double-sided adhesive sheet laminates of Examples 2 to 3 are excellent in reworkability and metal corrosion resistance, especially according to the selection of the formulation of the outer layer and the intermediate layer, the selection of the layer thickness ratio, etc.

[0313] In contrast, the double-sided PSA sheet of Comparative Example 1 had a ratio of the tensile storage modulus (E') to the shear storage modulus (G') of 4.9, and therefore had poor reworkability.

[0314] In addition, for the double-sided adhesive sheets of Comparative Examples 2 and 3, the (meth) acrylic adhesive layer is a single layer, and the peak temperature (T1) of the loss tangent (Tanδ) obtained by the dynamic viscoelasticity measurement in the shear mode with a frequency of 1 Hz is higher than -10°C, or the adhesive force is less than 5.0 N / 20 mm. Therefore, the double-sided adhesive sheet is hard and has poor height difference absorption, or bubbles are generated at the ends of the bonding surface during the reliability test, resulting in poor bonding reliability.

[0315] The double-sided PSA sheet of Comparative Example 4 had a peak temperature (T2) of loss tangent (Tan δ) obtained by dynamic viscoelasticity measurement in a tensile mode at a frequency of 1 Hz of less than -10°C, and therefore had poor reworkability.

[0316] The above embodiments show specific aspects of the present invention, but the above embodiments are merely examples and are not to be construed as limiting. Various modifications obvious to those skilled in the art are intended to be within the scope of protection of the present invention.

[0317] Industrial Applicability

[0318] The double-sided adhesive sheet of the present invention has excellent adhesive properties such as height difference absorption, adhesive strength, and lamination reliability, and can be easily peeled (separated) from the image display device component by cooling operation. Therefore, it can be suitably used for laminating the image display device component.

[0319] Furthermore, the image display device laminate and the image display device of the present invention can be easily peeled (separated) from the constituent member for an image display device and are excellent in reworkability.

Claims

1. A double-sided adhesive sheet for bonding two components of an image display device. The double-sided adhesive sheet has at least two layers having different glass transition temperatures. The double-sided adhesive sheet has a layer structure of two layers in which the outer layer and the inner layer are (meth)acrylic adhesive layers, or at least three layers in which the outermost layer and the innermost layer are (meth)acrylic adhesive layers. The ratio (E' / G') of the tensile storage modulus (E') to the shear storage modulus (G') of the double-sided adhesive sheet is 5.0 or more, In the dynamic viscoelasticity measurement in the shear mode at a frequency of 1 Hz, the peak temperature (T1) of the loss tangent (Tanδ) obtained by setting the thickness of the sample to be measured to 0.6 to 0.8 mm is below -10°C. The peak temperature (T2) of the loss tangent (Tanδ) obtained by the dynamic viscoelasticity measurement in the tensile mode at a frequency of 1 Hz is above -10°C, wherein, When two or more peak temperatures are observed, the highest temperature is taken as the peak temperature (T2). The 180° peeling strength at 23° C. with respect to each adhered surface of the two image display device constituent members is 5 N / 20 mm or more.

2. The double-sided adhesive sheet according to claim 1, wherein The difference between the peak temperature (T2) of the loss tangent (Tanδ) obtained by the dynamic viscoelasticity measurement in the tensile mode at a frequency of 1 Hz and the peak temperature (T1) of the loss tangent (Tanδ) obtained by the dynamic viscoelasticity measurement in the shear mode at a frequency of 1 Hz is 5 to 50°C.

3. The double-sided adhesive sheet according to claim 1 or 2, wherein The two image display device components are formed of different materials.

4. The double-sided adhesive sheet according to claim 1 or 2, wherein Of the two image display device components, one is glass, and the other includes any one or a combination of two or more of the group consisting of a touch sensor, an image display panel, a surface protection panel, a polarizing film, and a retardation film.

5. The double-sided adhesive sheet according to claim 4, wherein The glass is a protective glass having a curved shape. 6 . The double-sided pressure-sensitive adhesive sheet according to claim 1 , wherein the two image display device components can be separated by a cooling operation.

7. The double-sided adhesive sheet according to claim 6, wherein The cooling operation is cooling to below -50°C. 8 . The double-sided adhesive sheet according to claim 1 , which has a thickness of 50 to 1000 μm.

9. The double-sided adhesive sheet according to claim 1 or 2, wherein The double-sided PSA sheet is a PSA sheet having at least three layers, the outermost layer and the innermost layer being a (meth)acrylic PSA layer. The total ratio of the thickness of the outermost layer and the innermost layer to the overall thickness is 5 to 70%. 10 . The double-sided pressure-sensitive adhesive sheet according to claim 1 , which is photocurable. 11 . A laminate for an image display device, wherein two constituent members for an image display device are bonded together via the double-sided pressure-sensitive adhesive sheet according to claim 1 . 12 . A laminate for an image display device, wherein two constituent members for an image display device are bonded together via a cured adhesive layer of the double-sided adhesive sheet according to claim 1 . 13 . An image display device, comprising the layered product for an image display device according to claim 12 .

Citation Information

Patent Citations

  • Pressure sensitive adhesive double-sided sheet and display device with touch panel

    JP2004231723A

  • Adhesive material having redetachability

    WO2010137523A1

  • Transparent double-sided adhesive sheet and image display device

    JP2015157884A

  • Adhesive sheet, laminating method thereof, manufacturing method therefor, laminate and image display device

    JP2016104829A

  • Adhesive sheet and display body

    JP2016216624A