A method for purifying ultrafine nanowires

Through the nuclear pore membrane-tangential flow filtration device combined with centrifugal treatment, the problems of high cost and low efficiency of ultra-fine nanowire purification are solved, and efficient and environmentally friendly nanowire purification is achieved, which avoids nanowire winding and agglomeration and improves purification effect and yield.

CN115213395BActive Publication Date: 2024-11-08NUOVO FILM SUZHOU CHINA INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210987954.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-17
Publication Date
2024-11-08
Estimated Expiration
2042-08-17

AI Technical Summary

Technical Problem

The existing ultrafine nanowire purification methods are costly and inefficient, and are prone to cause nanowire winding and agglomeration, affecting filtration efficiency.

Method used

Using a nuclear pore membrane-tangential flow filtration device, the pH value of ultrafine nanowire emulsion is adjusted, combined with high-speed centrifugation and low-speed centrifugation to remove impurities, and high-transmissive flux ratio nuclear pore membrane-tangential flow filtration is used to achieve efficient purification. , avoid nanowire wrapping and accumulation.

Benefits of technology

It improves the purification efficiency and effect of ultra-fine nanowires, reduces costs and environmental hazards, and achieves high productivity and high yield purification effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115213395B_ABST
    Figure CN115213395B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for purifying ultrafine nanowires, and belongs to the technical field of nanomaterials. The method of the present invention uses a nuclear pore membrane-tangential flow filtration device as a core purification device, and the nuclear pore membrane-tangential flow filtration device includes multiple groups of internal pressure tubular nuclear pore membrane groups, and the nuclear pore membrane groups are formed by multiple single nuclear pore tubular membranes. The purification method includes the following steps: adjusting the pH of the ultrafine nanowire emulsion, centrifuging, and taking a solid phase; dispersing the solid phase in a polyvinyl pyrrolidone solution, centrifuging, and taking a liquid phase; transferring the liquid phase to the nuclear pore membrane-tangential flow filtration device, filtering the tangential flow at a permeation flux ratio of 10%-30%, and obtaining purified ultrafine nanowires. The present invention solves the problem of easy clogging of traditional tangential flow microfiltration membranes for purifying ultrafine nanowires through the method of tubular nuclear pore membrane tangential flow filtration, and realizes solvent replacement, cleaning, and concentrated collection of ultrafine silver nanowires while removing small particles in the ultrafine silver nanowire emulsion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nanomaterials, and in particular relates to a method for purifying ultrafine nanowires. Background Art

[0002] The existing purification methods of ultrafine metal nanowires mainly include centrifugation, positive and negative pressure filtration, acetone sedimentation, static sedimentation, centrifugal filtration and tangential flow filtration. The method of sedimentation and filtration of organic solvents such as acetone is the earliest and most commonly used method in the laboratory, but the organic solvent used in this method is highly toxic and takes a long time to settle. Large-scale purification requires a large sedimentation tank and a large amount of organic solvents (such as acetone). Although the purification effect is good and easy to operate in the laboratory, it is costly, inefficient and not environmentally friendly, so it is not conducive to industrial production. The positive and negative pressure filtration method does not use organic solutions, which is more environmentally friendly than the acetone sedimentation method, but the ultrafine nanowires will accumulate on the surface of the filter membrane and block the pores during the positive and negative pressure filtration process, which seriously affects the efficiency and effect of the filtration.

[0003] To this end, a stirred centrifugal filtration method has recently been proposed to purify ultrafine nanowires. This method has improved efficiency and effect compared to positive pressure filtration, but it also has some problems, such as limited production capacity and high cost of polymer membranes. The shear force of stirring may cause the entanglement and breakage of ultrafine nanowires.

[0004] Tangential flow filtration is a method of purifying ultrafine silver nanowires through organic hollow fiber membranes or inorganic ceramic membranes. It does not require a large amount of organic solution. Due to the effect of tangential flow, it is difficult for nanowires to accumulate in the membrane. The purification efficiency is high and can be mass-produced. However, when purifying ultrafine nanowires through tangential flow filtration, due to the small diameter of ultrafine nanowires and the rough inner wall of conventional filtration membranes such as hollow fiber membranes and silicon carbide ceramic membranes, ultrafine nanowires are easily embedded, causing the ultrafine nanowires to entangle with each other and accumulate on the inner wall of the membrane, resulting in reduced flux and a rapid decrease in filtration efficiency. Summary of the invention

[0005] Therefore, the technical problem to be solved by the present invention is to overcome the problems of high cost and low efficiency in the purification of ultrafine nanowires in the prior art.

[0006] To solve the above technical problems, the present invention provides a method for purifying ultrafine nanowires. The method of the present invention can efficiently purify ultrafine nanowires, does not require organic solvents, is environmentally friendly, has high production efficiency, and does not cause the ultrafine nanowires to entangle and agglomerate.

[0007] The first object of the present invention is to provide a method for purifying ultrafine nanowires, with a nuclear pore membrane-tangential flow filtration device as the core purification device, the nuclear pore membrane-tangential flow filtration device comprising a plurality of groups of internal pressure tubular nuclear pore membrane groups, the nuclear pore membrane groups being formed by a plurality of single nuclear pore tubular membranes, the purification method comprising the following steps:

[0008] (1) adjusting the pH of the ultrafine nanowire emulsion, centrifuging, and collecting the solid phase;

[0009] (2) dispersing the solid phase described in step (1) in a polyvinyl pyrrolidone solution, centrifuging, and taking a liquid phase;

[0010] (3) The liquid phase described in step (2) is transferred to a nucleopore membrane-tangential flow filtration device, and tangential flow filtration is performed at a permeation flux ratio of 10%-30% to obtain the purified ultrafine nanowires.

[0011] In one embodiment of the present invention, the diameter of the internal pressure tubular nuclear pore membrane group is 10-500 mm; the diameter of the single nuclear pore tubular membrane is 1-50 mm; and the filtration accuracy of the nuclear pore membrane is 0.1-5 μm.

[0012] In one embodiment of the present invention, a nuclear pore membrane with a filtration accuracy of 0.1-5 μm (the diameter of a single nuclear pore tubular membrane is 1-50 mm) is first rolled, welded or glued together to form a nuclear pore membrane cylinder, and then the nuclear pore membrane cylinder is inserted into the inner wall of a 10-500 mm tubular microfiltration membrane, and the two ends of the nuclear pore membrane roll are welded or glued to the inner wall of the microfiltration membrane to form an internal pressure tubular nuclear pore membrane group. Multiple groups of internal pressure tubular nuclear pore membrane groups are connected in parallel, and other auxiliary devices are added at both ends to form a nuclear pore membrane-tangential flow filtration device.

[0013] In one embodiment of the present invention, in step (1), the ultrafine nanowire emulsion is an ultrafine nanowire emulsion synthesized by a polyol method.

[0014] In one embodiment of the present invention, in step (1), the ultrafine nanowires are ultrafine metal nanowires and / or ultrafine metal oxide nanowires.

[0015] In one embodiment of the present invention, the ultrafine metal nanowires are one or more of ultrafine silver nanowires, ultrafine copper nanowires, ultrafine nickel nanowires and ultrafine cobalt nanowires.

[0016] In one embodiment of the present invention, the ultrafine metal oxide nanowires are ultrafine copper oxide nanowires and / or ultrafine iron oxide nanowires.

[0017] In one embodiment of the present invention, in step (1), the diameter of the ultrafine nanowire is ≤25 nm.

[0018] In one embodiment of the present invention, in step (1), the pH is 8-10, which prevents the ultrafine nanowires from being pulverized in an acidic water environment, neutralizes the unreacted silver ions, and prevents the further generation of particles.

[0019] In one embodiment of the present invention, in step (1), the pH regulator is sodium hydroxide and / or sodium bicarbonate.

[0020] In one embodiment of the present invention, in step (1), the centrifugal speed is 8000-10000 rpm and the centrifugal time is 5-60 min. Removing polyols reduces the viscosity of the system and facilitates subsequent tangential flow filtration.

[0021] In one embodiment of the present invention, in step (2), the proportion of polyvinyl pyrrolidone in the polyvinyl pyrrolidone solution is 0.01-0.1 wt %.

[0022] In one embodiment of the present invention, in step (2), the centrifugal speed is 2000-4000 rpm; the centrifugal time is 5-60 min.

[0023] In one embodiment of the present invention, in step (3), the solid content of the liquid phase is 0.1-0.8 wt %.

[0024] In one embodiment of the present invention, in step (3), the core component of the nuclear pore membrane-tangential flow filtration device is a tubular nuclear pore microfiltration membrane modified from a nuclear pore membrane. The nuclear pore membrane uses thermal neutrons in a nuclear reactor to cause uranium-235 to fission. The fragments produced by the fission penetrate an organic high-density plastic film, thereby leaving a narrow radiation damage channel on the path of the fission fragments. After oxidation, this channel is etched with appropriate chemical reagents to turn the channel on the film into a cylindrical micropore. By controlling the irradiation conditions and etching conditions of the nuclear reactor, nuclear pore membranes with different pore densities and pore sizes can be obtained. The surface of the nuclear pore membrane is extremely smooth, the pores are uniform and through-holes, and it is not easy to embed ultrafine nanowires.

[0025] In one embodiment of the present invention, in step (3), the permeate flux ratio = permeate water flow rate / circulation water flow rate.

[0026] In one embodiment of the present invention, in step (3), the circulating water flow rate of the nucleopore membrane-tangential flow filtration device is 10-15 t / h, and the permeate water flow rate is 1-3 t / h.

[0027] In one embodiment of the present invention, in step (3), the liquid inlet pressure of the nuclear pore membrane-tangential flow filtration device is 0.02-0.1 MPa; the permeation pressure is 0-0.1 MPa. Too high a pressure may easily cause the nanowires to entangle and accumulate.

[0028] The second object of the present invention is to provide a purified ultrafine nanowire prepared by the method.

[0029] The technical solution of the present invention has the following advantages over the prior art:

[0030] (1) The method for purifying ultrafine nanowires described in the present invention first blocks the continued generation of silver particles by adjusting the pH; then removes polyols by high-speed centrifugation to reduce viscosity, which is convenient for subsequent tangential flow filtration. Large particles and short rods in the ultrafine nanowire emulsion are removed by low-speed centrifugation. Then, the method using nuclear pore membrane-tangential flow filtration as the core purification process solves the problem of easy clogging of traditional tangential flow microfiltration membrane purification of ultrafine nanowires, and achieves high production capacity and high yield of ultrafine nanowire purification while removing impurities in the ultrafine nanowire emulsion.

[0031] (2) The method for purifying ultrafine nanowires described in the present invention solves the problem of easy clogging of traditional tangential flow microfiltration membranes for purifying ultrafine nanowires, improves the efficiency and effect of ultrafine nanowire purification, and greatly reduces the cost and environmental damage of ultrafine nanowire purification. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein:

[0033] Figure 1 Schematic diagram of the purification of ultrafine nanowires of the present invention.

[0034] Figure 2 These are SEM images of the nucleopore membrane of Example 1 of the present invention and the PET hollow fiber membrane of Comparative Example 1; wherein a is a SEM image of the inside of the nucleopore membrane; and b is a SEM image of the inner wall of the PET hollow fiber membrane.

[0035] Figure 3 : are SEM images of the ultrafine silver nanowires of Example 1 of the present invention; wherein, ab are SEM images of the ultrafine silver nanowires before purification; and cd are SEM images of the ultrafine silver nanowires after purification. DETAILED DESCRIPTION

[0036] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0037] In the present invention, unless otherwise specified, the nuclear pore membrane-tangential flow filtration device is firstly wound, welded or glued together a nuclear pore membrane with a filtration accuracy of 0.1-5 μm (the diameter of a single nuclear pore tubular membrane is 1-50 mm) to form a nuclear pore membrane cylinder, and then the nuclear pore membrane cylinder is inserted into the inner wall of a 10-500 mm tubular microfiltration membrane, and the two ends of the nuclear pore membrane roll are welded or glued to the inner wall of the microfiltration membrane to form an internal pressure tubular nuclear pore membrane group. Multiple groups of internal pressure tubular nuclear pore membrane groups are connected in parallel, and other auxiliary devices are added at both ends to form a nuclear pore membrane-tangential flow filtration device.

[0038] In the present invention, unless otherwise specified, the nuclear pore membrane-tangential flow filtration device is the main core purification device, such as Figure 1 As shown, the liquid phase with adjusted solid content is first transferred to the solvent water tank, and the PVP solution is added, and circulated in the tubular membrane through valves 1, 2, and 3 by a magnetic pump. The particles of the tubular membrane flow into the waste liquid tank through valve 4, and the purified nanowires are collected in the finished product water tank through valve 5.

[0039] Example 1

[0040] A method for purifying ultrafine nanowires, comprising the following steps:

[0041] (1) 5 kg of deionized water was added to 5 kg of 20 nm ultrafine silver nanowire synthesis stock solution (more than 30% of particles) with a solid content of 0.4% to dilute the solution to obtain an ultrafine silver nanowire mixed solution, and 20 g of sodium bicarbonate was added to the ultrafine silver nanowire mixed solution while stirring to adjust the pH to about 8.

[0042] (2) Centrifuge at 10,000 rpm for 20 min to collect the solid phase and remove the PG used in the synthesis.

[0043] (3) After the solid phase was washed and dissolved with 0.025 wt % PVP, it was centrifuged at 2000 rpm for 5 min using a floor-standing centrifuge. The liquid phase was collected after multiple rounds of centrifugation to remove large particles and short rods in the solid phase.

[0044] (4) The solid content of ultrafine silver nanowires was adjusted to 0.3 wt %. The mixed solution was transferred to a device equipped with a nuclear pore membrane-tangential flow filtration device (the filtration accuracy of the matching nuclear pore membrane was 2 μm, and the SEM image of the inside of the nuclear pore membrane was as shown in FIG. Figure 2 a), the circulating water flow rate was controlled at 12 t / h, the inlet pressure was 0.035 MPa, the permeate flow rate was 2 t / h, and the permeate pressure was 0.001 MPa. 180 L of 0.025 wt% PVP aqueous solution was circulated and filtered to remove small particles, and 10.5 g of purified silver wire was obtained, with an overall ultrafine nanowire yield of 52.5%.

[0045] Comparative Example 1

[0046] (1) 5 kg of deionized water was added to 5 kg of 20 nm ultrafine silver nanowire synthesis stock solution (more than 30% of particles) with a solid content of 0.4% to dilute the solution to obtain an ultrafine silver nanowire mixed solution, and 20 g of sodium bicarbonate was added to the ultrafine silver nanowire mixed solution while stirring to adjust the pH to about 8.

[0047] (2) Centrifuge at 10,000 rpm for 20 min to collect the solid phase and remove the PG used in the synthesis.

[0048] (3) After the solid phase was washed and dissolved with 0.025 wt % PVP, it was centrifuged at 2000 rpm for 5 min using a floor-standing centrifuge. The liquid phase was collected after multiple rounds of centrifugation to remove large particles and short rods in the solid phase.

[0049] (4) The solid content of ultrafine silver nanowires was adjusted to 0.3 wt %. The mixed solution was transferred to a device equipped with a nucleopore membrane-tangential flow filtration device (equipped with a common PET hollow fiber filter membrane with a pore size of 2 μm, and the SEM image of the inner wall of the PET hollow fiber membrane is as shown in FIG. Figure 2 b), the circulating water flow rate was controlled at 12 t / h, the inlet pressure was 0.035 MPa, the permeate flow rate was 2 t / h, and the pressure was 0.001 MPa. 180 L of 0.025 wt% PVP aqueous solution was circulated and filtered to remove small particles to obtain purified silver wires. A total of 2.2 g of pure silver wires were collected, and the overall ultrafine nanowire yield was 11%.

[0050] Comparative Example 2

[0051] (1) 5 kg of deionized water was added to 5 kg of 20 nm ultrafine silver nanowire synthesis stock solution (more than 30% of particles) with a solid content of 0.4% to dilute the solution to obtain an ultrafine silver nanowire mixed solution, and 20 g of sodium bicarbonate was added to the ultrafine silver nanowire mixed solution while stirring to adjust the pH to about 8.

[0052] (2) Centrifuge at 10,000 rpm for 20 min to collect the solid phase and remove the PG used in the synthesis.

[0053] (3) After the solid phase was washed and dissolved with 0.025 wt % PVP, it was centrifuged at 2000 rpm for 5 min using a floor-standing centrifuge. The liquid phase was collected after multiple rounds of centrifugation to remove large particles and short rods in the solid phase.

[0054] (4) The solid content of ultrafine silver nanowires was adjusted to 0.3wt%. The mixed solution was transferred to a device equipped with a nucleopore membrane-tangential flow filtration device (the matching nucleopore membrane filtration accuracy was 2μm), and the circulating water flow rate was controlled to be 12t / h, the inlet pressure was 0.035MPa, the permeate flow rate was 4t / h, and the permeate pressure was 0MPa. 180L of 0.025wt% PVP aqueous solution was circulated and filtered to remove small particles to obtain purified silver wires. A total of 12g of pure silver wires were collected, and the overall ultrafine nanowire yield was 60%.

[0055] Test Example 1

[0056] The SEM images of the ultrafine silver nanowire dispersion before and after purification in Example 1 are as follows: Figure 3 As shown, from Figure 3 As can be seen from c-3d, the purified ultrafine silver nanowires were detected by SEM: the diameter was about 22nm, and no obvious impurities such as particles and thick rods were observed to the naked eye.

[0057] Test Example 2

[0058] The sheet resistance and haze of the original solution ultrafine silver nanowires of Example 1, the purified ultrafine silver nanowires, the purified ultrafine silver nanowires of Comparative Example 1, and the purified ultrafine silver nanowires of Comparative Example 2 were tested. The degree of purification of the silver nanowires can be detected by spin coating to test the sheet resistance and haze of the silver nanowires.

[0059] The ultrafine silver nanowires were diluted to 0.14wt% with 0.025wt% PVP (silver wire dispersion stabilizer) and 0.1wt% HPMC (spin coating wetting agent and adhesive), and the ultrafine silver nanowire transparent conductive film was prepared on a PET substrate (the haze of the substrate itself was 0.8%) by spin coating (400rpm, 7s) (heated on a heating table at 100°C for 10min after spin coating). The square resistance and haze were tested. The results are shown in Table 1. The changes in the photoelectric properties of the film indirectly reflect the changes in the purity of the ultrafine silver nanowire dispersion.

[0060] Table 1

[0061] Sample Square resistance / Ω Haze / % Yield / % Example 1 Synthesis of ultrafine silver nanowires from stock solution 108 3.5 - Example 1 Purified ultrafine silver nanowires 27 1.9 52.5 Comparative Example 1: Ultrafine silver nanowires after purification 35 2.2 11 Comparative Example 2: Ultrafine silver nanowires after purification 30 2.0 60

[0062] As can be seen from Table 1, Example 1 uses improved tangential flow filtration to purify ultrafine silver nanowires, solving the problem of low yield of ultrafine nanowires purified by traditional tangential flow filtration membrane groups. In addition, a centrifugal pretreatment process is introduced to further improve the overall yield, and the yield of purified ultrafine nanowires is higher and the purity is higher. The conductive film formed after coating and curing with the same solid content has lower square resistance, the purified ultrafine nanowires have less particles, the ultrafine silver nanowire network is denser, and the conductivity is better.

[0063] In Comparative Example 1, ordinary PET filter membrane was used to purify ultrafine silver nanowires. The ultrafine nanowires easily blocked the membrane pores, resulting in reduced flux, poor filtration effect, more residual particles and very low yield.

[0064] Comparative Example 2 uses a high circulation ratio, resulting in a short filtration time. When the dialysis filtration volume is the same, although the yield is slightly improved, the number of cycles is insufficient, the particle removal effect is poor, resulting in particle residue and a slight increase in square resistance haze.

[0065] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.

Claims

1. A method for purifying ultrafine nanowires, characterized in that: A nuclear pore membrane-tangential flow filtration device is used as a core purification device, wherein the nuclear pore membrane-tangential flow filtration device comprises a plurality of groups of internal pressure tubular nuclear pore membrane groups, wherein the internal pressure tubular nuclear pore membrane groups are formed by a plurality of single nuclear pore tubular membranes, and the filtration accuracy of the single nuclear pore tubular membrane is 0.1-5 μm; the purification method comprises the following steps: (1) adjusting the pH of the ultrafine nanowire emulsion, centrifuging, and taking the solid phase; the centrifugal speed is 8000-10000 rpm; the centrifugal time is 5-60 min; (2) dispersing the solid phase described in step (1) in a polyvinyl pyrrolidone solution, centrifuging, and taking a liquid phase; the centrifugal speed is 2000-4000 rpm; the centrifugal time is 5-60 min; (3) Transferring the liquid phase described in step (2) to a nuclear pore membrane-tangential flow filtration device, and filtering the liquid phase by tangential flow at a permeation flux ratio of 10%-30% to obtain the purified ultrafine nanowires; the circulating water flow rate of the nuclear pore membrane-tangential flow filtration device is 10-15 t / h, and the permeate flow rate is 1-3 t / h.

2. The method for purifying ultrafine nanowires according to claim 1, characterized in that: The diameter of the internal pressure tubular nuclear pore membrane group is 10-500 mm; the diameter of the single nuclear pore tubular membrane is 1-50 mm.

3. The method for purifying ultrafine nanowires according to claim 1, characterized in that: In step (1), the diameter of the ultrafine nanowire is ≤25 nm.

4. The method for purifying ultrafine nanowires according to claim 1, characterized in that: In step (1), the pH is 8-10; the pH regulator is sodium hydroxide and / or sodium bicarbonate.

5. The method for purifying ultrafine nanowires according to claim 1, characterized in that: In step (3), the solid content of the liquid phase is 0.1-0.8 wt %.

6. The method for purifying ultrafine nanowires according to claim 1, characterized in that: In step (3), the inlet pressure of the nucleopore membrane-tangential flow filtration device is 0.02-0.1 MPa; the permeate pressure is 0-0.1 MPa.

7. The purified ultrafine nanowires prepared by the method according to any one of claims 1 to 6.