A high performance lithium ion battery separator and preparation method thereof

By using a combination technology of anti-hole blocking solution and polymer solution on the lithium-ion battery separator, the problems of insufficient heat resistance and hole blocking of the separator are solved, and a high-performance separator is prepared, which improves the overall performance and safety of the battery.

CN115224439BActive Publication Date: 2024-11-15CYG NEW ENERGY MATERIAL RESEARCH INSTITUTE (GUANGDONG) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210961464.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-11
Publication Date
2024-11-15
Estimated Expiration
2042-08-11

AI Technical Summary

Technical Problem

The existing lithium-ion battery separators lack heat resistance, and secondary processing can easily lead to hole blockage problems, affecting the application performance of the battery.

Method used

Using a combination of anti-hole-blocking solution and polymer solution, excellent heat resistance is prepared by pre-coating anti-blocking solution on the polyolefin separator substrate, coating the polymer solution, pre-drying, wet solidification and water washing. High performance lithium-ion battery separator with high porosity and high strength.

Benefits of technology

It significantly improves the heat resistance and porosity of the diaphragm, avoids hole blockage, improves the overall performance of the battery, and meets the safety and high performance requirements of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115224439B_ABST
    Figure CN115224439B_ABST
Patent Text Reader

Abstract

The present invention discloses a high-performance lithium-ion battery separator and a preparation method thereof, belonging to the technical field of lithium-ion battery separators. The preparation method of the separator is as follows: S1, pre-coating an anti-pore blocking solution on one or both sides of a polyolefin separator substrate, allowing the anti-pore blocking solution to quickly penetrate into the pores of the substrate, and removing excess anti-pore blocking solution on the surface of the substrate; S2, coating a polymer solution on one side of the polyolefin separator substrate obtained in step S1 to obtain a coating separator; S3, pre-drying the coating separator to form a film of the polymer solution on the polyolefin separator substrate, and wet coagulating the pre-dried coating separator; S4, washing the coagulated and fixed coating separator with water, and then drying it twice to obtain a high-performance lithium-ion battery separator. The lithium-ion battery separator obtained by the preparation method of the present invention has the advantages of excellent heat resistance, high porosity, high strength, high heat resistance, ultra-thinness, and liquid affinity and liquid retention.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion battery separators, and in particular to a high-performance lithium ion battery separator and a preparation method thereof. Background Art

[0002] The diaphragm is one of the essential key materials for lithium-ion batteries. It is a porous film with electronic insulation and ion conductivity. It is generally made of polyolefin as raw material and is continuously processed by equipment through wet or dry processes. The physical and chemical properties of the diaphragm greatly affect the comprehensive electrical properties of the battery.

[0003] At present, most of the diaphragms are mainly polyethylene (PE), polypropylene (PP) diaphragms or composite films of these two materials. Although PE diaphragms, PP diaphragms or PP / PE / PP composite diaphragms are low in cost, easy to process, mature in technology, and can meet the requirements of large-scale production and application, due to the inherent lack of heat resistance of polyolefin materials themselves, it is difficult to meet the growing requirements of lithium-ion batteries for safe application performance. Therefore, it is necessary to improve the diaphragm or select film materials with better performance. At present, there are diaphragm products made of new materials such as PET non-woven diaphragms, cellulose diaphragms, PI diaphragms and electrospinning diaphragms on the market. These new diaphragms generally have excellent heat resistance, good air permeability, high porosity, and good battery application safety performance, but there are also problems such as high cost, insufficient product uniformity, and poor consistency. Therefore, it is difficult for these to replace the current mainstream polyolefin diaphragms.

[0004] Technical improvement of polyolefin diaphragms is a more common and effective method to make up for the shortcomings of polyolefin diaphragms. The usual technical improvement method is to perform secondary processing on polyolefin diaphragms. The processing method is mainly to use a micro-gravure coater to coat one or more functional coatings on the surface of the polyolefin diaphragm substrate, thereby giving the diaphragm substrate new functions or improving the diaphragm's physical and chemical properties. This processing method has the advantages of easy processing, high efficiency, flexible combination, and customization to meet the requirements of different customers. However, due to the inherent defects of the coating process itself, it is inevitable that the coating material will penetrate into the pore structure of the diaphragm, and the polymer binder will form a dense film on the surface of the diaphragm substrate, resulting in pore blockage, which significantly affects the application performance of the diaphragm in the battery.

[0005] Therefore, it is very necessary to develop a high-performance lithium-ion battery separator with excellent heat resistance, high porosity, high strength, ultra-thinness, liquid affinity and liquid retention, and a preparation method thereof. Summary of the invention

[0006] In order to overcome the deficiencies of the prior art, the present invention aims to provide a high-performance lithium-ion battery separator.

[0007] To solve the above problems, the technical solution adopted by the present invention is as follows:

[0008] A method for preparing a high-performance lithium-ion battery separator comprises the following steps:

[0009] S1. Adding a penetrant to a low-boiling point solvent to prepare an anti-pore blocking solution; pre-coating the anti-pore blocking solution on one or both sides of a polyolefin diaphragm substrate, allowing the anti-pore blocking solution to quickly penetrate into the pores of the substrate, and removing excess anti-pore blocking solution on the surface of the polyolefin substrate;

[0010] S2, preparing a polymer solution; coating the polymer solution on one side of the polyolefin diaphragm substrate prepared in step S1 to obtain a coated diaphragm;

[0011] S3, pre-drying the coating membrane to form a film of the polymer solution on the polyolefin membrane substrate, and wet-coagulating the pre-dried coating membrane;

[0012] S4, washing the coated separator after solidification and fixation with water, and drying it twice after washing to obtain the high-performance lithium-ion battery separator.

[0013] Preferably, the penetrant in step S1 is one of ethylene glycol, glycerol, tripropylene glycol, PEG-200, PEG-400, or a combination of any two or more thereof.

[0014] Preferably, the low-boiling point solvent in step S1 is an amphiphilic solvent having a boiling point of less than 100°C and containing a polar group and a non-polar group; wherein the polar group is one of -OH, -O-, -CO-, -Cl, and -COO-; and the non-polar group is one of -CH3, -CH2CH2-, -CH2CH2CH2-, -C6H5-, -CH3CH(CH3)-, and -CH2C(CH3)2-.

[0015] Preferably, the low boiling point solvent is selected from one or a combination of any two or more of methanol, ethanol, isopropanol, dichloromethane, ethyl ether, acetone, butanone, tetrahydrofuran, ethyl acetate, and ethylene glycol dimethyl ether.

[0016] Preferably, in step S1, the low boiling point solvent is used in an amount of 100 parts by weight, and the penetrant is used in an amount of 0.5 to 5 parts by weight.

[0017] Preferably, the anti-pore blocking solution in step S1 is coated on the polyolefin diaphragm substrate by dip coating or roller coating.

[0018] Preferably, the polyolefin diaphragm substrate is one of a dry-process single-layer or multi-layer PP diaphragm, a wet-process single-layer or multi-layer PE diaphragm or a PE and PP composite diaphragm; the thickness of the polyolefin diaphragm substrate is 3 to 16 μm.

[0019] Preferably, the coating amount of the anti-pore blocking solution in step S1 is m=V*P*ρ, where V is the volume of the polyolefin diaphragm substrate in cm 3 ; P is the porosity of the polyolefin diaphragm substrate, in %; ρ is the density of the anti-blocking solution, in g / cm 3 .

[0020] Preferably, the polymer solution in step S2 has a solid content of 1 to 30% and a viscosity of 100 to 5000 mPa.s.

[0021] Preferably, the polymer solution is composed of the following components in parts by mass: 100 parts of a good solvent, 5 to 30 parts of a polymer resin, 1 to 10 parts of a coagulant, and 0.1 to 2 parts of an auxiliary agent.

[0022] Further preferably, the good solvent is selected from one or a combination of any two or more of dimethylformamide, dimethylacetamide, N-methylpyrrolidone, dimethyl sulfoxide, m-cresol, dibutyl carbonate, ethyl acetate or water.

[0023] More preferably, the polymer resin is a polar polymer resin with a melting point of more than 100°C or a Tg value of more than 100°C.

[0024] More preferably, the polymer resin is selected from one or a combination of any two or more of polyacrylonitrile, polyethylene terephthalate, polyarylether, polyarylate, polyamide, polyimide, aromatic polyamide, polyetheretherketone or polyvinyl alcohol.

[0025] More preferably, the coagulant is selected from one or a combination of any two or more of methanol, ethanol, isopropanol, isobutanol, ethylene glycol, glycerol or water.

[0026] Further preferably, the auxiliary agent is an amphiphilic material containing both a hydrophilic group and a lipophilic group.

[0027] Further preferably, the auxiliary agent is one of fatty alcohol polyoxyethylene ether, multi-branched alcohol modified polyoxyethylene ether, acetylene glycol modified polyoxyethylene ether, polydimethylsiloxane, polyethylene glycol 200-400, or a combination of any two or more thereof.

[0028] Further preferably, the polymer solution is prepared according to the following method: adding a polymer resin to a formulated amount of a good solvent, heating to 40-80°C, stirring for 0.5-2.0h, after the polymer resin is dissolved until the solution becomes clear and transparent, cooling to room temperature, adding a formulated amount of a coagulant and an auxiliary agent, and stirring for another 0.1-1.0h to obtain a polymer solution.

[0029] Preferably, in step S2, the polymer solution is coated on one side of the polyolefin diaphragm substrate by spot coating or spray coating.

[0030] Preferably, the coating droplets of the polymer solution have a thickness of 10 to 50 μm, a diameter of 0.1 to 1 mm, and a coating speed of 20 to 100 m / min.

[0031] Preferably, the pre-drying method in step S3 is microwave drying.

[0032] Further preferably, the power of the microwave drying is 500-900W, the temperature is 20-60°C, and the drying time is 1-5min.

[0033] Preferably, the coagulation liquid used in the wet coagulation in step S3 is a mixture of the good solvent and water in a mass ratio of 1:1.

[0034] Preferably, the wet coagulation treatment temperature in step S3 is 30-50° C. and the treatment time is 1-10 min.

[0035] Preferably, the water washing treatment temperature in step S4 is 20-40° C. and the water washing time is 1-10 min.

[0036] Preferably, in step S4, secondary drying is performed by roller contact drying and / or hot air drying.

[0037] More preferably, the secondary drying has a drying temperature of 40 to 100° C. and a drying time of 0.5 to 5 min.

[0038] Preferably, the high-performance lithium-ion battery separator has a thickness of 5-20 μm, a tensile strength MD / TD ≥ 150 MPa, 130°C, 1.0 h, a thermal shrinkage MD / TD ≤ 3 / 2, a porosity of 45-50%, and a liquid retention rate ≥ 100%.

[0039] Compared with the prior art, the present invention has the following beneficial effects:

[0040] The preparation method of the lithium-ion battery separator provided by the present invention combines an original anti-pore blocking solution, a polymer solution coating formula and a unique preparation process, so that the prepared lithium-ion battery separator not only ensures the physical and chemical indicators such as high strength of the polyolefin separator substrate, but also has excellent heat resistance, significantly improves the high porosity and liquid retention rate of the ultra-thin separator, and has good comprehensive performance, effectively solving the problem of insufficient heat resistance and other properties of the current mainstream polyolefin separators and the problem of pore blocking caused by secondary processing of the coated separator. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1This is a scanning electron microscope (SEM) image of the high-performance lithium-ion battery separator prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0042] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0043] A method for preparing a high-performance lithium-ion battery separator, which comprises the steps of coating an anti-pore blocking solution on a separator substrate, coating a polymer solution on the separator substrate, pre-drying, wet coagulation, water washing, and secondary drying, as follows:

[0044] S1. Add the penetrant into a low boiling point solvent to prepare an anti-pore blocking solution; pre-coat the anti-pore blocking solution on one or both sides of the polyolefin diaphragm substrate by dip coating or roller coating through the first coating device of the coating machine, so that the anti-pore blocking solution can quickly penetrate into the pores of the substrate, fill the pores of the polyolefin diaphragm substrate and maintain a saturated state, and remove excess anti-pore blocking solution on the surface of the polyolefin substrate by self-leveling or scraping with equipment.

[0045] The anti-pore blocking solution prepared in step S1 has strong pore permeability, excellent affinity with the polyolefin diaphragm substrate, is easy to volatilize, and is suitable for dip coating, roller coating or spray coating. Specifically, the anti-pore blocking solution is composed of a solvent and a penetrant, the main body of the anti-pore blocking solution is the solvent, and the penetrant plays an auxiliary role. Specifically, by mass, the solvent is 100 parts and the penetrant is 0.5 to 5 parts. The solvent contains an amphiphilic structure, that is, it contains polar groups and non-polar groups. The polar group can be one of -OH, -O-, -CO-, -Cl, and -COO-; the non-polar group can be one of -CH3, -CH2CH2-, -CH2CH2CH2-, -C6H5-, -CH3CH(CH3)-, and -CH2C(CH3)2-. The solvent can specifically be one or a combination of methanol, ethanol, isopropanol, dichloromethane, ether, acetone, butanone, tetrahydrofuran, ethyl acetate, and ethylene glycol dimethyl ether with a boiling point of <100°C. The penetrant can reduce the surface tension of the solvent and assist the solvent to quickly penetrate into the pore structure of the polyolefin membrane substrate. It can generally be a small molecule non-ionic surfactant, specifically one of ethylene glycol, glycerol, tripropylene glycol, PEG-200, PEG-400, or any combination thereof.

[0046] The polyolefin diaphragm substrate used in the present invention can be a dry-process single-layer or multi-layer PP diaphragm, a wet-process single-layer or multi-layer PE diaphragm, or a PE and PP composite diaphragm, and its thickness is 3 to 16 μm. The coating amount of the anti-pore blocking solution is related to the diaphragm substrate, and the specific coating amount is m=V*P*ρ, where V is the volume of the polyolefin diaphragm substrate, in cm 3 ; P is the porosity of the polyolefin diaphragm substrate, in %; ρ is the density of the anti-blocking solution, in g / cm3 . Select the appropriate coating roller mesh size according to the characteristics of the substrate to determine the coating amount.

[0047] S2, prepare a polymer solution; apply the polymer solution on one side of the polyolefin diaphragm substrate obtained in step S1 by dot coating or spraying through the second coating device of the coater (dot-carved coating roller or rotary sprayer), the coating or spraying droplet size is: thickness is 10 to 50 μm, diameter is 0.1 to 1 mm, coating speed is 20 to 100 m / min, and a coated diaphragm is obtained after coating.

[0048] In step S2, since the pore structure in the polyolefin diaphragm substrate has been filled with the anti-pore blocking solution, when the polymer solution is applied, the polymer material will hardly penetrate into the pore structure of the substrate. The polymer solution is a solution with high solid content, moderate viscosity and suitable for roller coating or spraying. Specifically, the solid content of the polymer solution is greater than 1%, specifically 1-30%, preferably 5-30%; the viscosity is 100-5000mPa.s. The polymer solution comprises a ternary system composed of a good solvent, a polymer resin, a coagulant and an additive, and the specific composition is, by mass, 100 parts of a good solvent, 5-30 parts of a polymer resin, 1-10 parts of a coagulant, and 0.1-2 parts of an additive.

[0049] In the polymer solution, the good solvent as a good solvent for the polymer resin can be one or a combination of any two or more of dimethylformamide, dimethylacetamide, N-methylpyrrolidone, dimethyl sulfoxide, m-cresol, dibutyl carbonate, ethyl acetate or water.

[0050] As the main functional resin, polymer resin is used to modify the surface of the interface between high-performance lithium-ion battery separator materials, which can significantly improve the heat resistance, liquid affinity and liquid retention performance, and porosity of the separator material, thereby improving the electrical performance and safety performance of the separator battery. The polymer resin is a polar polymer material with a melting point of more than 100°C or a Tg value of more than 100°C, and can be specifically one of polyacrylonitrile, polyethylene terephthalate, polyarylether, polyarylate, polyamide, polyimide, aromatic polyamide, polyetheretherketone or polyvinyl alcohol, or a combination of any two or more thereof.

[0051] The coagulant is a poor solvent that is insoluble in the polymer resin, and specifically can be one or a combination of any two or more of methanol, ethanol, isopropanol, isobutanol, ethylene glycol, glycerol or water. The interaction between the poor solvent as a coagulant and the polymer resin chain unit is small, resulting in the polymer resin chain segment coils being compacted and the end distance being small, making the polymer tend to be insoluble, coagulated, precipitated and fibrosed.

[0052] The auxiliary agent is an amphiphilic material containing both a hydrophilic group and a lipophilic group, and specifically can be one of fatty alcohol polyoxyethylene ether, multi-branched alcohol modified polyoxyethylene ether, acetylene glycol modified polyoxyethylene ether, polydimethylsiloxane, polyethylene glycol 200-400, or a combination of any two or more thereof. The auxiliary agent is used to promote the ternary system composed of solvent, polymer resin, and coagulant to form a homogeneous solution and stabilize it.

[0053] The polymer solution is prepared according to the following method: add the polymer resin to a formulated amount of a good solvent, heat to 40-80°C, stir for 0.5-2.0 hours, wait until the polymer resin is dissolved until the solution becomes clear and transparent, cool to room temperature, add a formulated amount of a coagulant and an auxiliary agent, and stir for another 0.1-1.0 hours to obtain a polymer solution.

[0054] S3, placing the coated diaphragm in a first microwave drying pretreatment oven for pre-drying, drying the anti-pore blocking solution and allowing the polymer solution to form a film on the polyolefin diaphragm substrate, and placing the pre-dried coated diaphragm in a first coagulation bath for wet coagulation treatment;

[0055] Step S3 firstly uses simple microwave drying to quickly heat the anti-pore blocking solution to volatilize, thereby restoring the original pore structure of the polyolefin diaphragm substrate. On the other hand, the polymer solution is preliminarily dried by microwave rapid drying to solidify and fiberize the polymer to form a continuous phase and form a film on the surface of the substrate. This will not cause the pore blocking problem of the substrate, greatly improving the pore blocking problem caused by secondary processing such as membrane substrate coating, and improving the battery application electrical performance of the coated diaphragm. The wet coagulation of the coated diaphragm pre-dried by microwave can make the coating finally solidified and porous. The coagulant in the polymer solution assists the coating to solidify, and the good solvent is exchanged out, leaving a porous structure.

[0056] In step S3, the output power of microwave drying is 500-900W, the drying temperature is 20-60°C, and the drying time is 1-5min. Under this process condition, the anti-pore blocking solution is basically completely volatilized, and the good solvent volatilization rate in the polymer solution coating is between 10-30%. If the volatility of the good solvent is less than 10%, the coating has a low degree of drying, the polymer solidification degree is low, and it is impossible to form fiberization and form a continuous phase and form a film at the interface. With the rapid volatilization of the anti-pore blocking agent, the polymer solution penetrates into the pore structure of the substrate, and finally causes the occurrence of pore blocking; if the volatility of the good solvent is greater than 30%, the coating surface solidification degree is high, forming a dense cortical structure, sealing the solution in the coating, and significantly affecting the pore forming process in the subsequent wet coagulation process, and finally resulting in a coating with few pores and small pores and obvious pore blocking. The treatment temperature of wet coagulation is 30-50°C, and the treatment time is 1-10 minutes; the coagulation liquid used in the coagulation bath is a mixture of a good solvent used in a polymer solution and water in a mass ratio of 1:1.

[0057] S4. The coated diaphragm after solidification is placed in a water washing tank for water washing at a temperature of 20 to 40°C for 1 to 10 minutes. After the washing is completed, it is subjected to secondary drying by a combination of direct roller contact drying and hot air drying through a second drying oven and a hot pressing roller. The drying temperature is 40 to 100°C and the drying time is 0.5 to 5 minutes to obtain a high-performance lithium-ion battery diaphragm.

[0058] Step S4: The residual solvent in the coating is cleaned by water washing, the pore structure is further improved and shaped, and the coating forms the final pore structure. The secondary drying can remove the residual water in the coating, so that the polymer fibers in the coating are oriented, crystallized, and shrunk.

[0059] The high-performance lithium-ion battery separator prepared by the above preparation method has a thickness of 5-20μm, a tensile strength of MD / TD≥150MPa, a thermal shrinkage rate of MD / TD≤3 / 2 at 130℃, 1.0h, a porosity of 45-50%, and a liquid retention rate of ≥100%. It is a high-performance lithium-ion battery separator that integrates high strength, high heat resistance, ultra-thinness, high porosity and excellent hydrophilic and liquid retention properties.

[0060] Example 1

[0061] A high-performance lithium-ion battery separator includes a separator substrate and a polymer functional coating coated on the separator substrate. The preparation method of the high-performance lithium-ion battery separator includes the following steps:

[0062] S1. Prepare an anti-pore blocking solution: add 1 part of PEG-200 penetrant into 100 parts of isopropanol low boiling point solvent, and stir well to obtain an anti-pore blocking solution;

[0063] S2. Prepare polymer solution: add 10 parts of polyarylate polymer resin to 100 parts of dimethylacetamide good solvent, heat to 60°C, stir for 1.0h, wait until the polyarylate polymer resin is completely dissolved and the solution becomes clear and transparent, cool to room temperature, add 5 parts of isopropyl alcohol coagulant and 1 part of polydimethylsiloxane auxiliary agent, and stir for 0.5h to obtain a polymer solution.

[0064] S3, coating and pretreatment: the anti-pore blocking solution is coated on one side of the PE diaphragm substrate by a micro-gravure roller coater, and then the polymer solution is coated on the other side of the PE diaphragm substrate, and the coated diaphragm is pre-dried by microwave, the microwave drying power is 600w, the temperature is 40℃, and the drying time is 3min; the pre-dried coated diaphragm is wet coagulated, and the wet coagulation treatment temperature is 40℃ and the treatment time is 3min. Among them, the thickness of the PE diaphragm substrate is 9μm, and the coating speed is 60m / min.

[0065] S4, water washing and drying: the coating membrane after solidification is washed with water, the water washing treatment temperature is 30 ℃, the water washing time is 5 minutes; the secondary drying temperature is 80 ℃, the drying time is 3 minutes, and the coating thickness is 3μm, and the total thickness is 12μm. High-performance lithium-ion battery membrane.

[0066] Figure 1 This is a scanning electron microscope (SEM) image of the high-performance lithium-ion battery separator prepared in this embodiment. Figure 1 It is shown that the high-performance lithium-ion battery separator prepared in this embodiment has less pore blockage, a high porosity structure, a large and rich pore structure, and a uniform and consistent pore distribution.

[0067] Example 2

[0068] A high-performance lithium-ion battery separator includes a separator substrate and a polymer functional coating coated on the separator substrate. The preparation method of the high-performance lithium-ion battery separator includes the following steps:

[0069] S1. Prepare an anti-pore blocking solution: add 5 parts of PEG-400 penetrant into a low-boiling-point solvent containing 100 parts of ethanol, and stir well to obtain an anti-pore blocking solution;

[0070] S2. Preparation of polymer solution: Add 30 parts of polyarylether polymer resin to 100 parts of dimethylformamide good solvent, heat to 80°C, stir for 1.0h, wait until the polyarylether polymer resin is completely dissolved and the solution becomes clear and transparent, cool to room temperature, add 10 parts of ethanol coagulant and 2 parts of fatty alcohol polyoxyethylene ether auxiliary, and stir for another 1.0h to obtain a polymer solution.

[0071] S3, coating and pretreatment: the anti-pore blocking solution is coated on one side of the PE diaphragm substrate by a micro-gravure roller coater, and then the polymer solution is coated on the other side of the PE diaphragm substrate, and the coated diaphragm is pre-dried by microwave, the microwave drying power is 900w, the temperature is 60℃, and the drying time is 5min; the pre-dried coated diaphragm is wet coagulated, and the wet coagulation treatment temperature is 50℃ and the treatment time is 8min. Among them, the thickness of the PE diaphragm substrate is 9μm, and the coating speed is 60m / min.

[0072] S4, water washing and drying: the coating membrane after solidification is washed with water, the water washing treatment temperature is 40 ℃, the water washing time is 8 minutes; the secondary drying temperature is 90 ℃, the drying time is 5 minutes, and a high-performance lithium-ion battery membrane with a coating thickness of 3μm and a total thickness of 12μm is obtained.

[0073] Example 3

[0074] A high-performance lithium-ion battery separator includes a separator substrate and a polymer functional coating coated on the separator substrate. The preparation method of the high-performance lithium-ion battery separator includes the following steps:

[0075] S1. Prepare an anti-pore blocking solution: add 0.5 parts of ethylene glycol penetrant into 100 parts of methanol low boiling point solvent, and stir well to obtain an anti-pore blocking solution;

[0076] S2. Prepare polymer solution: add 5 parts of polyamide polymer resin to 100 parts of di-N-methylpyrrolidone good solvent, heat to 80°C, stir for 0.5h, wait until the polyamide polymer resin is completely dissolved and the solution becomes clear and transparent, cool to room temperature, add 1 part of methanol coagulant and 0.1 part of multi-branched alcohol modified polyoxyethylene ether auxiliary agent, and stir for 0.1h to obtain a polymer solution.

[0077] S3, coating and pretreatment: the anti-pore blocking solution is coated on one side of the PE diaphragm substrate by a micro-gravure roller coater, and then the polymer solution is coated on the other side of the PE diaphragm substrate, and the coated diaphragm is pre-dried by microwave, the microwave drying power is 500w, the temperature is 30℃, and the drying time is 1min; the pre-dried coated diaphragm is wet coagulated, and the wet coagulation treatment temperature is 30℃ and the treatment time is 1min. Among them, the thickness of the PE diaphragm substrate is 9μm, and the coating speed is 60m / min.

[0078] S4, water washing and drying: the coating membrane after solidification is washed with water, the water washing treatment temperature is 20 ℃, the water washing time is 1 minute; the secondary drying temperature is 50 ℃, the drying time is 1 minute, and a high-performance lithium-ion battery membrane with a coating thickness of 3 μm and a total thickness of 12 μm is obtained.

[0079] Example 4

[0080] The difference between this embodiment and embodiment 1 is that: in step S3, the polymer solution is coated on both sides of the PE diaphragm substrate by a micro-gravure roller coater, the thickness of the PE diaphragm substrate is 9 μm, the thickness of the single-sided coating is 3 μm, and the total thickness of the double-sided coating is 6 μm. The remaining components and preparation methods are the same as those in embodiment 1.

[0081] Comparative Example 1

[0082] The difference between this comparative example and Example 1 is that step S1 is omitted, the anti-pore blocking solution is not prepared, the process of coating the anti-pore blocking solution is omitted in S3, and the remaining components and preparation methods are the same as those in Example 1.

[0083] Comparative Example 2

[0084] The difference between this comparative example and Example 1 is that no penetrant is added in step S1, and the remaining components and preparation method are the same as those in Example 1.

[0085] Comparative Example 3

[0086] The difference between this comparative example and Example 1 is that no coagulant and auxiliary agent are added in the preparation of the polymer solution in step S2, and the remaining components and preparation method are the same as those in Example 1.

[0087] Comparative Example 4

[0088] The wet PE substrate of Example 1 was used as Comparative Example 4, and no coating process was performed. The thickness of the PE substrate was 9 μm, and the porosity was 45%.

[0089] Comparative Example 5

[0090] The polymer solution in the above-mentioned Example 1 was used as a functional slurry and was coated on one side of the PE diaphragm substrate using the same micro-gravure roller coater as in step S3 in Example 1, and then directly dried (temperature 60°C, drying time 3 minutes) to obtain a lithium-ion battery coated diaphragm with a substrate thickness of 9 μm and a coating thickness of 3 μm.

[0091] Performance comparison experiment

[0092] The thickness, air permeability, porosity, heat resistance and lyophilic and liquid-retaining properties of the lithium ion battery separators of Examples 1 to 4 and the separators of Comparative Examples 1 to 5 were measured and compared.

[0093] The nine groups of lithium battery separators prepared in Examples 1 to 4 and Comparative Examples 1 to 5 were made into soft-pack lithium-ion batteries: model 506090, positive electrode NCM523, negative electrode: natural graphite; electrolyte: EC / PC / DMC ratio: 2:3:5 (v / v / v), 1M LiPF6, VC 2%; the battery resistance and rate performance of the battery were measured.

[0094] The results are shown in Table 1.

[0095] Table 1 Test results of the diaphragms prepared in the examples and comparative examples

[0096]

[0097]

[0098] It can be seen from Table 1 that the high-performance lithium-ion battery separator manufactured by Example 1 through a better formula combination and process has the best physical and chemical properties: low air permeability, high porosity, high liquid retention rate, high puncture strength, small thermal shrinkage rate at 150°C, 1.0h, and high membrane rupture temperature; the battery prepared by the high-performance lithium-ion battery separator manufactured by Example 1 has the best battery performance: small battery internal resistance, high capacity, and good 3C rate performance.

[0099] In Example 2, as the proportion of polymer resin and related additives increases, the air permeability of the manufactured high-performance lithium-ion battery separator increases, the porosity decreases, the liquid retention rate decreases, the 150°C thermal shrinkage rate increases, and the membrane rupture temperature decreases slightly, the internal resistance of the manufactured battery increases, the capacity decreases, and the 3C rate is slightly worse; in Example 3, as the proportion of polymer resin and related additives decreases, the air permeability of the manufactured high-performance lithium-ion battery separator increases, the porosity decreases, the liquid retention rate decreases, the 150°C thermal shrinkage rate increases, and the membrane rupture temperature decreases, the internal resistance of the manufactured battery increases, the capacity decreases, and the rate decreases slightly, showing the same rules as in Example 2; compared with Example 1, Example 4 is only changed from a single-sided 3μ coating to a double-sided 6μ coating, then the air permeability value increases and the porosity decreases. Although the 150°C thermal shrinkage rate of the product decreases and the membrane rupture temperature increases, the manufactured battery has the problems of increased internal resistance, decreased capacity, and poor rate.

[0100] Compared with Example 1, Comparative Example 1 lacks the anti-pore blocking solution and the first coating process, the air permeability of the product is significantly increased by 22%, the porosity and liquid absorption rate are reduced, the heat resistance is slightly worse, the internal resistance of the manufactured battery is significantly increased, the capacity is significantly reduced, and the rate is significantly worse;

[0101] Compared with Example 1, Comparative Example 2 lacks a penetrant, which is not conducive to the anti-pore blocking solution fully penetrating into the pore structure of the substrate, and easily causes the subsequent coated polymer solution to penetrate into the pores of the substrate, resulting in pore blocking. Therefore, similarly, the air permeability value of the manufactured high-performance lithium-ion battery separator increases, the porosity decreases, the liquid retention rate decreases, the 150°C thermal shrinkage rate increases and the membrane rupture temperature decreases slightly, the manufactured battery internal resistance increases, the capacity decreases, and the 3C rate deteriorates;

[0102] Comparative Example 3 Compared with Example 1, the polymer solution does not add a coagulant and an auxiliary agent, resulting in poor porosity of the coating. Therefore, the air permeability of the manufactured high-performance lithium-ion battery separator increases, the porosity decreases, the liquid retention rate decreases, the 150°C thermal shrinkage rate increases, and the membrane rupture temperature decreases slightly. The internal resistance of the manufactured battery increases, the capacity decreases, and the 3C rate deteriorates;

[0103] Comparative Example 4 directly uses 9μ wet PE substrate without any processing. The product shrinks nearly 100% at 150°C for 1.0h, that is, it almost shrinks into resin particles. The film breaking temperature is only 140°C, the heat resistance is insufficient, and the application safety performance is poor.

[0104] Comparative Example 5 is a lithium-ion battery coated diaphragm prepared by coating a polymer solution as a functional slurry. Compared with Example 1, the process is very different. A direct drying and solvent volatilization film-forming method is adopted. The material in the coating easily penetrates into the substrate and easily causes pore blockage, resulting in a significant decrease in the porosity of the diaphragm and a sharp increase in the air permeability. The battery manufactured using this lithium-ion battery coated diaphragm has a particularly large internal resistance and poor rate performance.

[0105] From the test results of the membranes prepared in the above embodiments and comparative examples, it can be seen that the selection and proportion of the thermosensitive functional resin and the pressure-sensitive functional resin, the amount of photoinitiator, whether the substrate is coated, hot pressing composite and UV curing will affect the physical and chemical properties and battery application performance of the multilayer composite lithium-ion battery membrane.

[0106] In summary, the present invention combines a unique formula with a unique process to produce a multilayer composite lithium-ion battery separator. While ensuring that the heat resistance of the separator is significantly improved by adding a new functional layer to the separator, the problems of substrate pore blocking and porosity reduction are effectively avoided, solving the pain points of such product applications, and effectively improving the transmission channel of lithium ions, thereby greatly improving the battery's rate charge and discharge performance.

[0107] The above-mentioned embodiments are only preferred embodiments of the present invention and cannot be used to limit the scope of protection of the present invention. Any non-substantial changes and substitutions made by technicians in this field on the basis of the present invention shall fall within the scope of protection required by the present invention.

Claims

1. A method for preparing a high-performance lithium-ion battery separator, Features: The following steps are involved: S1. Add the penetrant into a low boiling point solvent to prepare an anti-pore blocking solution; Pre-coating the anti-pore blocking solution on one or both sides of the polyolefin diaphragm substrate, allowing the anti-pore blocking solution to quickly penetrate into the pores of the substrate, and removing excess anti-pore blocking solution on the surface of the polyolefin substrate; wherein the penetrant is one of ethylene glycol, glycerol, tripropylene glycol, PEG-200, and PEG-400, or a combination of any two or more thereof; the low-boiling point solvent is an amphiphilic solvent having a boiling point of less than 100°C and containing polar groups and non-polar groups; S2, preparing a polymer solution; coating the polymer solution on one side of the polyolefin diaphragm substrate prepared in step S1 to obtain a coated diaphragm; S3, pre-drying the coating membrane with microwaves to form a film of the polymer solution on the polyolefin membrane substrate, and wet-coagulating the pre-dried coating membrane; S4, washing the coated separator after solidification and fixation with water, and drying it twice after washing to obtain the high-performance lithium-ion battery separator.

2. The method for preparing a high-performance lithium-ion battery separator according to claim 1, Features: The low boiling point solvent is selected from one of methanol, ethanol, isopropanol, dichloromethane, ethyl ether, acetone, butanone, tetrahydrofuran, ethyl acetate, and ethylene glycol dimethyl ether, or a combination of any two or more thereof.

3. The method for preparing a high-performance lithium-ion battery separator according to claim 1, Features: In step S1, the mass amount of the low boiling point solvent is 100 parts, and the mass amount of the penetrant is 0.5 to 5 parts.

4. The method for preparing a high-performance lithium-ion battery separator according to claim 1, Features: The polymer solution consists of the following components in parts by mass: 100 parts of a good solvent, 5 to 30 parts of a polymer resin, 1 to 10 parts of a coagulant, and 0.1 to 2 parts of an auxiliary agent.

5. The method for preparing a high-performance lithium-ion battery separator according to claim 4, Features: The good solvent is selected from one or a combination of any two or more of dimethylformamide, dimethylacetamide, N-methylpyrrolidone, dimethyl sulfoxide, m-cresol, dibutyl carbonate, ethyl acetate or water.

6. The method for preparing a high-performance lithium-ion battery separator according to claim 4, Features: The polymer resin is selected from one or a combination of any two or more of polyacrylonitrile, polyethylene terephthalate, polyarylether, polyarylate, polyamide, polyimide, aromatic polyamide, polyetheretherketone or polyvinyl alcohol.

7. The method for preparing a high-performance lithium-ion battery separator according to claim 4, Features: The coagulant is selected from one or a combination of any two or more of methanol, ethanol, isopropanol, isobutanol, ethylene glycol, glycerol or water; the auxiliary agent is one or a combination of any two or more of fatty alcohol polyoxyethylene ether, multi-branched alcohol modified polyoxyethylene ether, acetylene glycol modified polyoxyethylene ether, polydimethylsiloxane, polyethylene glycol 200-400.

8. The method for preparing a high-performance lithium-ion battery separator according to claim 1, Features: In step S3, the power of microwave drying is 500-900W, the temperature is 20-60°C, and the drying time is 1-5min; the processing temperature of wet coagulation is 30-50°C, and the processing time is 1-10min.

9. The method for preparing a high-performance lithium-ion battery separator according to claim 1, Features: In step S4, the water washing treatment temperature is 20-40° C., and the water washing time is 1-10 minutes; the drying temperature of the secondary drying is 40-100° C., and the drying time is 0.5-5 minutes.