Polycrystalline diamond and preparation method thereof

By mixing 3 microns with fine single crystal diamond with a specific binding agent, dispersing and removing impurities, high temperature and high pressure synthesis under existing industrial conditions is achieved, which solves the problem of diamond resynthesis and improves diamond Performance and applicability.

CN115228373BActive Publication Date: 2024-11-15蒋向上
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210498284.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-09
Publication Date
2024-11-15
Estimated Expiration
2042-05-09

AI Technical Summary

Technical Problem

The prior art is difficult to effectively use 3 microns of fine single crystal diamond for high temperature and high pressure resynthesis, which leads to difficulties in industrial production and the problem of backlog of inventory.

Method used

By mixing 3 microns with fine single crystal diamond with a specific binding agent, dispersion treatment, impurity removal treatment and high-temperature and high-pressure synthesis, the environmental conditions of diamond atomic bond links are reduced, and high-temperature and high-pressure synthesis under existing industrial conditions is achieved, forming Polycrystalline diamond.

Benefits of technology

Successfully reduces the conditions for high-temperature and high-pressure synthesis, realizes bond links between diamond atoms, improves the hardness, wear resistance and impact strength of diamonds, and has unique grain arrangement and cutting capabilities, suitable for large-area tools and semiconductors. Preparation of components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115228373B_ABST
    Figure CN115228373B_ABST
Patent Text Reader

Abstract

The present invention discloses a polycrystalline diamond and a preparation method thereof. The present invention uses single crystal diamonds of 3 microns or less as raw materials, and combines single crystal diamonds of different particle sizes into a whole polycrystalline structure diamond through atomic bonds under high temperature and high pressure, so that single crystal diamonds of 3 microns or less can be resynthesized into a whole polycrystalline diamond. The color of the diamond prepared by the present invention is bright black, and it not only retains the high hardness, high wear resistance, high thermal conductivity, and corrosion resistance of traditional diamonds, but also has its own unique material properties: the grains are disorderly arranged, isotropic, have no cleavage plane, will not produce cracks, have high impact strength and hardness, have more crystal edges and grinding surfaces, and each crystal edge has cutting and grinding capabilities, which greatly increases the contact probability between the tool and the workpiece, greatly improves the working efficiency of the tool, and can prepare large-area diamond tools and diamond semiconductor components.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to polycrystalline diamond and a preparation method thereof, belonging to the technical field of diamond preparation. Background Art

[0002] In my country's artificial diamond industry, carbon atoms can be converted into diamonds with the help of catalysts through artificially given pressure and temperature, and have long been successfully applied to industrial production. Whether it is yellow-brown diamonds or white diamonds, whether it is a single-cavity production of hundreds of carats of diamonds or a single-cavity production of 10,000 carats of diamonds, it is inseparable from the basic principle of carbon atoms being converted into diamonds. The particle size of artificially synthesized diamonds is generally between 0.1 mm and 10 mm. Diamonds with a particle size of 3 microns to 100 microns are almost all made by crushing coarse-grained diamonds. Among the crushed diamonds, diamonds with a particle size of 3 microns or less account for 5% of the total. In my country, about 200 million carats of diamonds with a particle size of 3 microns or less are accumulated in stock every year. According to incomplete statistics, by the end of 2021, there were about 50 tons of diamonds with a particle size of 3 microns or less accumulated in warehouses across the country because they could not enter the sales market. Summary of the invention

[0003] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a polycrystalline diamond and a preparation method thereof. The present invention uses single crystal diamond of 3 microns or less as raw material, and combines single crystal diamonds of different sizes into a whole polycrystalline structure diamond through atomic bonds under high temperature and high pressure, so that the single crystal diamond of 3 microns or less can be resynthesized into a whole gold crystal diamond.

[0004] In order to achieve the above object, the present invention adopts the following technical solution:

[0005] The present invention provides a method for preparing polycrystalline diamond, comprising mixing a dispersed and impurity-removed single crystal diamond with a binder to obtain a mixed powder, pressing and molding the mixed powder to obtain a pressed green sheet, synthesizing the pressed green sheet on a hydraulic press to obtain a polycrystalline diamond rough sheet, and crushing and purifying the rough sheet to obtain the polycrystalline diamond;

[0006] The particle size of the single crystal diamond is ≤3 μm;

[0007] The purity of the single crystal diamond is ≧99.50%.

[0008] The binder is composed of B powder, C powder, TiC powder, Ni powder, Mn powder, Co powder, Fe powder and Cu powder. In the mixed powder, the mass fraction of the binder is 4% to 12%; wherein the mass fraction of B powder in the mixture is 0.5% to 1%, the mass fraction of C powder in the mixture is 1% to 4%, the mass fraction of TiC powder in the mixture is 0.1% to 0.6%, the mass fraction of Ni powder in the mixture is 0.1% to 0.6%, the mass fraction of Mn powder in the mixture is 0.7% to 1.3%, the mass fraction of Co powder in the mixture is 1% to 6%, the mass fraction of Fe powder in the mixture is 1% to 5%, and the mass fraction of Cu powder in the mixture is 0.5% to 2.5%;

[0009] Diamond is an atomic crystal, which is composed of pure carbon, and carbon atoms are linked by tetravalent bonds, that is, the links between diamond atoms are combined into a whole in the form of carbon-carbon bonds, and each pair of diamond atoms is linked by more than four pairs. It is precisely because of the material structure characteristics of diamond atomic crystals that a theoretical basis is provided for the re-linking of diamond single crystals thinner than 3 microns into a whole crystal.

[0010] The prototype of diamond structure is diamond crystal. In diamond crystal, each carbon atom is in SP 3 The hybrid orbital forms covalent bonds with four other carbon atoms to form a regular tetrahedron. The strong CC covalent bonds give rise to the high hardness of diamond. The linking characteristics of multiple covalent bonds between atoms provide theoretical support for the original preparation process of synthesizing 3-micron diamonds into larger diamonds through high temperature and high pressure.

[0011] However, directly synthesizing diamonds thinner than 3 microns through high temperature and high pressure again requires a pressure as high as 28000MPa and a temperature as high as 2900℃, which makes industrial production impossible. The present invention has found through a large number of experiments that by first mixing single crystal diamond with the binder of the present invention, the environmental conditions for the atomic bonds of diamond can be reduced under the action of the binder of the present invention, thereby achieving high temperature and high pressure synthesis under existing industrial conditions. Finally, the synthesized rough diamond is purified and the binder is removed to obtain the overall polycrystalline diamond.

[0012] In a preferred embodiment, the dispersion treatment process is to place the single crystal diamond under a protective atmosphere for heat treatment, the heat treatment temperature is 600°C to 800°C, and the heat treatment time is 30min to 60min.

[0013] Further preferably, the protective atmosphere is selected from argon and / or nitrogen.

[0014] The inventors found that a considerable portion of the diamond single crystals with a particle size of less than 3 microns are nanometer-level, and the agglomeration phenomenon is quite serious. The particle size formed by the agglomeration is between 0.05 mm and 1 mm. After agglomeration, it is impossible to mix and disperse evenly with the binder, so that the single crystal diamonds cannot be bonded. The inventors found that by heat treating it at the above temperature, the dispersion problem can be well solved, so that the agglomerated particle size in the diamond single crystal with a particle size of less than 3 microns can be controlled to be less than 3 microns.

[0015] In a preferred embodiment, the impurity removal process is as follows: firstly, the single crystal diamond is placed in a solution containing nitric acid and hydrofluoric acid for acid treatment, and then the single crystal diamond is placed in a solution containing soda ash for acid treatment.

[0016] Further preferably, in the solution containing nitric acid and hydrofluoric acid, the mass ratio of nitric acid to hydrofluoric acid is 0.8 to 1.2:1;

[0017] More preferably, the temperature of the acid treatment is 60-70° C., and the time of the acid treatment is 80-120 h.

[0018] Further preferably, in the solution containing soda ash, the mass ratio of soda ash to water is 1:15-25.

[0019] More preferably, the alkali treatment is carried out at a temperature of 80 to 100° C. and for a time of 1 to 2 hours.

[0020] There are also various types of impurities such as graphite, silicon carbide, aluminum oxide, iron oxide, etc. in diamonds finer than 3 microns. According to detection and analysis, there are more than 20 impurities in diamonds finer than 3 microns. These impurities are harmful to the diamond's secondary synthesis and composite preparation process. The impurities in the diamond must be completely removed first. Through the above-mentioned impurity removal treatment, the purity of the diamond can reach 99.50%.

[0021] In a preferred embodiment, the particle size of the binder is 0.01 μm to 0.1 μm.

[0022] In the present invention, the particle size of the binder will have a certain influence on the high temperature and high pressure synthesis. If the particle size is too coarse, it will become a filler between the diamond atomic bonds, affecting the strength of the bonds between the diamond atoms. If the particle size is too fine, agglomerates will appear, which is more harmful than coarse particles.

[0023] According to a preferred solution, the pressed green body is assembled with the shielding material, the heat transfer and pressure transfer material, the heat generating and conductive material, and the insulating and pressure transfer material into a composite block, and then the composite block is synthesized by a hydraulic press.

[0024] In a preferred embodiment, the synthesis temperature is 1900° C. to 2500° C., and the synthesis pressure is 8000 MPa to 15000 MPa.

[0025] In the actual operation, the green compact is shaped into a cylinder, and then the cylindrical green compact is placed in a shielding material for sealing. Since the shielding material forms a sealed space, it is ensured that impurities will not penetrate into it during the synthesis process. The synthetic block is placed in a vacuum insulation box at a constant temperature of 100°C for storage.

[0026] The new polycrystalline diamond cylinder obtained after high temperature and high pressure synthesis is removed from the shielding material on the surface, crushed to the required particle size by a crusher, and then sieved and purified before being sold according to strength grade and particle size.

[0027] In a preferred embodiment, the purification process is as follows: firstly, the single crystal diamond is immersed in a solution containing nitric acid and hydrofluoric acid for acid treatment, then the single crystal diamond is immersed in a solution containing soda ash, and then the single crystal diamond is washed several times with clean water and then dried.

[0028] Further preferably, in the solution containing nitric acid and hydrofluoric acid, the mass ratio of nitric acid to hydrofluoric acid is 0.8 to 1.2:1.

[0029] More preferably, the temperature of the acid treatment is 60-70° C., and the time of the acid treatment is 80-120 h.

[0030] Further preferably, in the solution containing soda ash, the mass ratio of soda ash to water is 1:15-25.

[0031] More preferably, the alkali treatment is carried out at a temperature of 80 to 100° C. and for a time of 1 to 2 hours.

[0032] The present invention also provides polycrystalline diamond prepared by the above preparation method.

[0033] Principles and advantages

[0034] The present invention obtains fully dispersed and high-purity single crystal diamond by dispersing and removing impurities from single crystal diamonds with a size of 3 microns, and then combines it with the binder of the present invention. The binder of the present invention provides an environmental condition for reducing the atomic bond connection of diamond, thereby realizing high-temperature and high-pressure synthesis under existing industrial conditions. Finally, the synthesized rough diamond is purified and the binder is removed to obtain the overall polycrystalline diamond.

[0035] The color of the diamond prepared by the present invention is bright black. It not only retains the high hardness, high wear resistance, high thermal conductivity and corrosion resistance of traditional diamonds, but also has its own unique material properties:

[0036] 1. The grains are arranged in disorder, are isotropic, have no cleavage planes, and will not crack.

[0037] 2. High impact resistance, 3 to 4 times that of traditional diamonds.

[0038] 3. The hardness is 1.5 to 2 times higher than that of traditional diamonds, and its self-sharpening performance is better than that of traditional diamonds.

[0039] 4. There are more crystal edges and grinding surfaces. Each crystal edge has cutting and grinding capabilities, which greatly increases the contact probability between the tool and the workpiece, greatly improving the working efficiency of the tool.

[0040] 5. Larger area diamond tools and diamond semiconductor components can be produced. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 The green compact of the cylindrical structure in the present invention.

[0042] Figure 2 Schematic diagram of a cross-sectional view of a composite block assembled in the present invention.

[0043] Figure 3 The polycrystalline diamond prepared in Example 1 has a particle size of 1 mm to 5 mm.

[0044] Figure 4 The polycrystalline diamond prepared in Example 1 has a particle size of 100 μm to 1 mm.

[0045] Figure 5 The polycrystalline diamond with a particle size of ≦100 μm prepared in Example 1.

[0046] Figure 6 Macroscopic morphology of the polycrystalline diamond rough blank prepared in Example 1.

[0047] Figure 7 Macroscopic morphology of the polycrystalline diamond rough blank prepared in Comparative Example 1.

[0048] Figure 8 The polycrystalline diamond prepared in Comparative Example 2 still contained particles with a particle size of ≥8 mm after being crushed for 3 hours.

[0049] Fig. 9 The polycrystalline diamond prepared in Comparative Example 2 was crushed for 3 hours to produce particles with a particle size of ≤5 mm.

[0050] Fig.10 Macroscopic morphology of the polycrystalline diamond rough blank prepared in Example 3.

[0051] Fig.11 Macroscopic morphology of the polycrystalline diamond rough blank prepared in Comparative Example 3. DETAILED DESCRIPTION

[0052] Example 1

[0053] The single crystal diamond with a diameter of 3 microns was placed in nitrogen for heat treatment at a temperature of 600° C. for 60 minutes to obtain dispersed single crystal diamond.

[0054] A solution containing nitric acid and hydrofluoric acid is prepared in a ratio of 1:1:20 to water, and the single crystal diamond is first immersed in the solution containing nitric acid and hydrofluoric acid and treated at 60°C for 100 hours. Then, a solution containing soda ash is prepared in a ratio of 1:20 to water, and the single crystal diamond is immersed in the solution containing soda ash and treated at 80°C for 2 hours to obtain a single crystal diamond with a purity of 99.6%, which is mixed with a binder to obtain a mixed powder, which is pressed under a pressure of 200MPa to obtain a cylindrical compact, and the cylindrical compact is combined with a shielding material, a heat transfer and pressure transfer material, a heat-generating conductive material, and an insulating and pressure transfer material. The resulting product is assembled into a synthetic block, and then placed in a six-sided hydraulic press to apply a pressure of 8000 MPa to the synthetic block, and subjected to high temperature and high pressure at 1900°C for 5 hours to obtain a polycrystalline diamond rough blank. The rough blank is crushed, and the crushed product is mixed with a solution containing nitric acid and hydrofluoric acid in a mass ratio of 1:1:20 between nitric acid, hydrofluoric acid and water. The single crystal diamond is first immersed in the solution containing nitric acid and hydrofluoric acid and treated at 60°C for 100 hours, and then a solution containing soda ash is mixed in a mass ratio of soda ash to water of 1:20, and the single crystal diamond is immersed in the solution containing soda ash and treated at 80°C for 1 hour to obtain polycrystalline diamond.

[0055] The binder is composed of B powder, C powder, TiC powder, Ni powder, Mn powder, Co powder, Fe powder and Cu powder all with particle sizes ranging from 0.01 to 0.1 μm, wherein the mass fraction of B powder in the mixture is 0.5%, the mass fraction of C powder in the mixture is 1%, the mass fraction of TiC powder in the mixture is 0.6%, the mass fraction of Ni powder in the mixture is 0.6%, the mass fraction of Mn powder in the mixture is 0.7%, the mass fraction of Co powder in the mixture is 1%, the mass fraction of Fe powder in the mixture is 5%, and the mass fraction of Cu powder in the mixture is 2.5%.

[0056] The polycrystalline diamond prepared in this embodiment is screened. Figure 3 It is polycrystalline diamond with a particle size of 1mm to 5mm. Figure 4 It is polycrystalline diamond with a particle size of 100μm to 1mm. Figure 5 The polycrystalline diamond has a particle size of ≤100 μm, wherein the polycrystalline diamond with a particle size of 300 μm to 200 μm is tested to have a static pressure strength of ≥12 Kg / particle and a thermal shock strength of ≥90 J / m.

[0057] Example 2

[0058] The single crystal diamond with a diameter of 3 microns was placed in nitrogen for heat treatment at a temperature of 700° C. for 45 minutes to obtain dispersed single crystal diamond.

[0059] A solution containing nitric acid and hydrofluoric acid is prepared in a ratio of 1:1:20 to water, and the single crystal diamond is first immersed in the solution containing nitric acid and hydrofluoric acid and treated at 65°C for 100 hours. Then, a solution containing soda ash is prepared in a ratio of 1:20 to water, and the single crystal diamond is immersed in the solution containing soda ash and treated at 90°C for 1.5 hours to obtain a single crystal diamond with a purity of 99.7%, which is mixed with a binder to obtain a mixed powder, which is pressed under a pressure of 250MPa to obtain a cylindrical compact, and the cylindrical compact is combined with a shielding material, a heat transfer and pressure transfer material, a heat-generating conductive material, and an insulating and pressure transfer material. The product is assembled into a synthetic block, and then placed in a six-sided hydraulic press to apply a pressure of 10000 MPa to the synthetic block, and subjected to high temperature and high pressure at 2200°C for 3 hours to obtain a polycrystalline diamond rough blank. The rough blank is crushed, and the crushed product is mixed with a solution containing nitric acid and hydrofluoric acid in a mass ratio of 1:1:20 between nitric acid, hydrofluoric acid and water. The single crystal diamond is first immersed in the solution containing nitric acid and hydrofluoric acid and treated at 60°C for 100 hours, and then a solution containing soda ash is mixed in a mass ratio of soda ash to water of 1:20, and the single crystal diamond is immersed in the solution containing soda ash and treated at 80°C for 1.5 hours to obtain polycrystalline diamond.

[0060] The binder is composed of B powder, C powder, TiC powder, Ni powder, Mn powder, Co powder, Fe powder and Cu powder all with particle sizes ranging from 0.01 to 0.1 μm, wherein the mass fraction of B powder in the mixture is 0.8%, the mass fraction of C powder in the mixture is 2%, the mass fraction of TiC powder in the mixture is 0.4%, the mass fraction of Ni powder in the mixture is 0.4%, the mass fraction of Mn powder in the mixture is 0.9%, the mass fraction of Co powder in the mixture is 3%, the mass fraction of Fe powder in the mixture is 3%, and the mass fraction of Cu powder in the mixture is 1.5%.

[0061] The polycrystalline diamond prepared in this embodiment was screened, and the polycrystalline diamond with a particle size of 300 μm to 200 μm was tested to have a static pressure strength of ≥12 Kg / particle and a thermal shock strength of ≥90 J / m. The overall quality of the polycrystalline diamond met the requirements.

[0062] Example 3

[0063] The single crystal diamond with a diameter of 3 microns was placed in nitrogen for heat treatment at a temperature of 800° C. for 30 minutes to obtain dispersed single crystal diamond.

[0064] A solution containing nitric acid and hydrofluoric acid is prepared in a ratio of 1:1:20 to water, and the single crystal diamond is first immersed in the solution containing nitric acid and hydrofluoric acid and treated at 70°C for 100 hours. Then, a solution containing soda ash is prepared in a ratio of 1:20 to water, and the single crystal diamond is immersed in the solution containing soda ash and treated at 100°C for 1 hour to obtain a single crystal diamond with a purity of 99.8% and mixed with a binder to obtain a mixed powder, which is pressed at a pressure of 300MPa to obtain a cylindrical compact, and the cylindrical compact is mixed with a shielding material, a heat transfer and pressure transfer material, The heating conductive material and the insulating pressure transmitting material are subjected to a pressure of 15000MPa at 2500℃ for 3h to obtain a polycrystalline diamond rough blank. The rough blank is crushed and the crushed product is mixed with a solution containing nitric acid and hydrofluoric acid in a mass ratio of 1:1:20 between nitric acid, hydrofluoric acid and water. The single crystal diamond is first immersed in the solution containing nitric acid and hydrofluoric acid and treated at 70℃ for 100h. Then, a solution containing soda ash is mixed in a mass ratio of soda ash to water of 1:20. The single crystal diamond is immersed in the solution containing soda ash and treated at 100℃ for 2h to obtain polycrystalline diamond.

[0065] The binder is composed of B powder, C powder, TiC powder, Ni powder, Mn powder, Co powder, Fe powder and Cu powder all with particle sizes ranging from 0.01 to 0.1 μm, wherein the mass fraction of B powder in the mixture is 1%, the mass fraction of C powder in the mixture is 4%, the mass fraction of TiC powder in the mixture is 0.1%, the mass fraction of Ni powder in the mixture is 0.1%, the mass fraction of Mn powder in the mixture is 1.3%, the mass fraction of Co powder in the mixture is 6%, the mass fraction of Fe powder in the mixture is 1%, and the mass fraction of Cu powder in the mixture is 0.5%.

[0066] The polycrystalline diamond prepared in this embodiment was screened, and the polycrystalline diamond with a particle size of 300 μm to 200 μm was tested to have a static pressure strength of ≥12 Kg / particle and a thermal shock strength of ≥90 J / m.

[0067] Comparative Example 1.

[0068] The other conditions are the same as those in Example 1, except that the particle size of the additive is ≥ 0.15 μm. Figure 6 and Figure 7 are the polycrystalline diamond synthetic rough blanks prepared in Example 1 and Comparative Example 1, respectively. Figure 7 The white substance in the rough is metal, which means that the metal in flakes cannot directly participate in the bonding of diamond atoms, resulting in uneven bonding of polycrystalline diamond in the rough, and the overall quality of polycrystalline diamond is reduced.

[0069] Comparative Example 2.

[0070] The proportion of diamond cylinder blank is: diamond 89%, Ni1%, Mn2%, Co8%, synthesis chamber temperature 1900℃, synthesis chamber pressure 9000MPa, the hardness of the synthesized polycrystalline diamond blank is ≥HRC50. During the crushing process, due to the high hardness, long crushing time, and large wear of crushing tools, the particle size distribution after crushing is 200 mesh fine and 300 mesh coarse, accounting for 30%, which seriously restricts the production efficiency of polycrystalline diamond and increases the manufacturing cost. Figure 8 , Fig. 9 .from Figure 8 It can be seen that after four hours of crushing, the particle size is still between 6 and 15 mm. As the difficulty of crushing the rough blank increases, the industrial production cost of polycrystalline diamond is greatly increased.

[0071] Comparative Example 3.

[0072] All other conditions were the same as those in Example 3, except that the temperature was 2600°C. During the synthesis, the polycrystalline diamond rough blank could not meet the quality requirements for practical applications and suffered great losses due to breakage. Fig.11 . This means that whether the manufacturing of polycrystalline diamond is successful or not, in addition to the ratio of additives, the particle size has strict requirements, and the optimal matching value of pressure and temperature in the synthesis chamber is also extremely critical. According to the different quality requirements of polycrystalline diamond, different synthesis processes need to be designed and formulated, that is, a reasonable pressure value and temperature value need to be given in the synthesis chamber. If the pressure is too large or too small, and the temperature is too high or too low, the rough polycrystalline diamond cannot be formed during synthesis, which is easy to cause loss and waste, increasing production costs.

Claims

1. A method for preparing polycrystalline diamond, characterized in that: The single crystal diamond which has been dispersed and impurity-removed is mixed with a binder to obtain a mixed powder, which is pressed into a compact to obtain a green compact, which is synthesized on a hydraulic press to obtain a polycrystalline diamond rough blank, which is crushed and purified to obtain a polycrystalline diamond; The dispersion treatment process is to place the single crystal diamond in a protective atmosphere for heat treatment, the heat treatment temperature is 600° C. to 800° C., and the heat treatment time is 30 min to 60 min; The particle size of the single crystal diamond is ≤3µm; The purity of the single crystal diamond is ≥99.50%; The binder is composed of B powder, C powder, TiC powder, Ni powder, Mn powder, Co powder, Fe powder and Cu powder. In the mixed powder, the mass fraction of the binder is 4% to 12%; wherein the mass fraction of B powder in the mixture is 0.5% to 1%, the mass fraction of C powder in the mixture is 1% to 4%, the mass fraction of TiC powder in the mixture is 0.1% to 0.6%, the mass fraction of Ni powder in the mixture is 0.1% to 0.6%, the mass fraction of Mn powder in the mixture is 0.7% to 1.3%, the mass fraction of Co powder in the mixture is 1% to 6%, the mass fraction of Fe powder in the mixture is 1% to 5%, and the mass fraction of Cu powder in the mixture is 0.5% to 2.5%; The particle size of the binder is 0.01µm~0.1µm; The synthesis temperature is 1900° C. to 2500° C., and the synthesis pressure is 8000 MPa to 15000 MPa.

2. The method for preparing polycrystalline diamond according to claim 1, characterized in that: The process of the impurity removal treatment is: firstly, the single crystal diamond is placed in a solution containing nitric acid and hydrofluoric acid for acid treatment, and then the single crystal diamond is placed in a solution containing soda ash.

3. The method for preparing polycrystalline diamond according to claim 2, characterized in that: In the solution containing nitric acid and hydrofluoric acid, the mass ratio of nitric acid to hydrofluoric acid is 0.8-1.2:1; the temperature of the acid treatment is 60-70° C., and the time of the acid treatment is 80-120 hours; In the solution containing soda ash, the mass ratio of soda ash to water is 1:15-25; the treatment temperature is 80-100° C., and the treatment time is 1-2 hours.

4. The method for preparing polycrystalline diamond according to claim 1, characterized in that: The purification process is as follows: firstly, the single crystal diamond is immersed in a solution containing nitric acid and hydrofluoric acid for acid treatment, then the single crystal diamond is immersed in a solution containing soda ash, then the single crystal diamond is washed with clean water for several times and then dried.

5. The method for preparing polycrystalline diamond according to claim 4, characterized in that: In the solution containing nitric acid and hydrofluoric acid, the mass ratio of nitric acid to hydrofluoric acid is 0.8-1.2:1; the temperature of the acid treatment is 60-70°C, and the time of the acid treatment is 80-120h; in the solution containing soda ash, the mass ratio of soda ash to water is 1:15-25; the treatment temperature is 80-100°C, and the time is 1-2h.