Battery positive electrode sheet and preparation method thereof and battery
By dropping passivation liquid in the poor area of the active material layer of the battery electrode sheet, forming a composite layer and a passivation layer, and using materials such as polyethylene glycol to block the pores, the lithium-ionization and loss of battery caused by uneven thickness of the active material layer is solved. Material problems improve the circulation and safety performance of the battery.
Patent Information
- Application Number
- CN202110463752.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-04-27
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-04-27
AI Technical Summary
When preparing battery electrode sheets by batch coating method, uneven thickness of the edges of the active material layer leads to lithium extraction and material dropout of the battery, affecting the long-term use and safety performance of the battery.
Add passivation liquid dropwise to the poor areas of the active material layer to form a composite layer and a passivation layer. Polyethylene glycol and its derivatives are used as passivation materials to block pores and inhibit electrolyte infiltration and lithium ion detachment, improving the material layer Structural stability.
Effectively suppress lithium-ion excision of the battery negative electrode, improve the cycle performance and safety performance of the battery, while maintaining the energy density of the battery, ensuring excellent electrochemical performance.
Smart Images

Figure CN115249786B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a battery positive electrode sheet and a preparation method thereof, and a battery. Background Art
[0002] In the process of preparing battery pole pieces, intermittent coating is often used to prepare battery pole pieces because blank current collectors need to be reserved for welding pole ears. However, the thickness of the active material layer formed by the intermittent coating method is not uniform at the edge. The uneven thickness of the active material layer will cause lithium deposition and material loss in the pole piece, which is not conducive to the long-term use of the battery.
[0003] In order to reduce the impact of uneven thickness of the active material layer on the battery, the current method is to apply tape to the edge of the active material layer to inhibit lithium deposition and material loss in the battery. However, the adhesive in the tape easily diffuses into the electrolyte, reducing the performance of the battery; and after multiple charge and discharge cycles of the battery with the positive electrode taped, a large number of lithium dendrites will still precipitate on the negative electrode surface corresponding to the taped position. The formed lithium dendrites will reduce the battery safety performance on the one hand, and on the other hand, it will lead to a decrease in battery capacity and a decrease in battery cycle performance, which is not conducive to the use of the battery. Summary of the invention
[0004] In view of this, the present application provides a battery positive electrode sheet, which has good structural stability, is not easy to fall off, and can effectively inhibit lithium plating at the battery negative electrode. Applying it in a battery can effectively improve the battery's cycle performance and safety performance, and will not affect the battery's energy density, thereby ensuring that the battery has excellent electrochemical properties.
[0005] In a first aspect, the present application provides a positive electrode sheet of a battery, comprising a current collector and an active material layer arranged on the surface of the current collector; the active material layer comprises an active region and a passivation region located on opposite sides of the active region along a first direction; the active region comprises an active material; the passivation region comprises a composite layer and a passivation layer, the composite layer comprises the active material and a passivation material mixed with the active material; the passivation layer comprises the passivation material, and the passivation material comprises one or more of polyethylene glycol and polyethylene glycol derivatives.
[0006] At present, when the active material layer is coated on the surface of the current collector by an intermittent coating method, since the machine adopts segmented coating, the thickness of the active material layer formed by the machine at the start and end of coating is not uniform, which leads to unstable structure of the active material layer, easy material drop and easy lithium dendrites in the negative electrode. The area with uneven thickness is the bad area. The battery positive electrode sheet of the present application can effectively solve the above problems by passivating the bad area of the active material layer. The bad area forms a passivation area after passivation treatment. The passivation material and the active material in the passivation area are mixed with each other to form a composite layer, which can inhibit the electrolyte from wetting the active material in the passivation area. At the same time, the passivation material forms a passivation layer covering the surface of the composite layer, further inhibiting the electrolyte from wetting the passivation area and the release of lithium ions in the active material, reducing the kinetic ability of the active material in the passivation area, and improving the phenomenon of lithium dendrites formed by lithium precipitation at the negative electrode opposite to the passivation area.
[0007] Optionally, in the passivation region, the composite layer has a thickness of 1 μm-200 μm.
[0008] Optionally, in the composite layer, the mass ratio of the active material to the passivation material is 1:(0.001-0.03).
[0009] Optionally, the thickness of the passivation layer is less than or equal to 20 μm.
[0010] Optionally, the average molecular weight of the polyethylene glycol is 2000-8000.
[0011] Optionally, the width of the passivation area along the first direction is 3 mm-1.2 cm.
[0012] Optionally, the active material comprises a material capable of reversibly extracting and inserting lithium ions.
[0013] Optionally, the active material includes LiFePO4, Li3V2(PO4)3, LiMn2O4, LiMnO2, LiNiO2, LiCoO2, LiVPO4F, LiFeO2 or Li 1+x L 1-y-z M y N z One or more of O2, wherein -0.1≤x≤0.2, 0≤y≤1, 0≤z≤1, 0≤y+z≤1.0, and L, M, and N are selected from Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Al, Mg, and Ga, respectively.
[0014] Optionally, the composite layer further includes a conductive agent and a binder.
[0015] Optionally, the binder includes one or more of polyvinylidene fluoride, polytetrafluoroethylene, polyhexafluoropropylene, styrene-butadiene rubber, sodium carboxymethyl cellulose, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polyamide, polyacrylonitrile and polyacrylate.
[0016] Optionally, the conductive agent includes one or more of acetylene black, carbon black, carbon nanotubes, carbon nanofibers, activated carbon and graphene.
[0017] Optionally, the mass percentage of the passivation material in the passivation area is 0.1%-3%.
[0018] Optionally, the mass percentage of the active material in the passivation region is 62%-99.7%.
[0019] Optionally, the mass percentage of the binder in the passivation area is 0.1%-15%.
[0020] Optionally, the mass percentage of the conductive agent in the passivation region is 0.1%-20%.
[0021] Optionally, the thickness of the current collector is 5 μm-100 μm. Further, the thickness of the current collector is 8 μm-20 μm.
[0022] Optionally, the active material layer has a thickness of 10 μm-200 μm.
[0023] In the battery positive electrode sheet provided in the first aspect of the present application, the passivation material can block the pores in the poor area of the active material layer, thereby inhibiting the electrolyte from infiltrating the poor area; and the passivation material can wrap the active material, which can inhibit the escape of lithium ions of the active material in the passivation area and reduce the concentration of lithium ions in the passivation area, thereby solving the problem of lithium plating at the negative electrode position corresponding to the poor area of the battery positive electrode and improving the battery's cycle performance and safety performance.
[0024] In a second aspect, the present application provides a method for preparing the above-mentioned battery positive electrode sheet, comprising the following steps:
[0025] Providing a current collector, coating a surface of the current collector with an active material layer to be passivated; the active material layer to be passivated includes an active region and regions to be passivated located on opposite sides of the active region along the first direction;
[0026] A passivation solution is dripped into the passivation area, and after drying, a passivation area is formed and an active material layer is obtained, and the active material layer is rolled to obtain the positive electrode sheet of the battery; the passivation solution includes a passivation material, and the passivation material includes one or more of polyethylene glycol and polyethylene glycol derivatives;
[0027] Optionally, the solvent of the passivation solution includes a volatile organic solvent, and the boiling point of the volatile organic solvent is less than or equal to 100°C.
[0028] Optionally, the volatile organic solvent includes one or more of ethanol, methanol, dichloromethane, chloroform and acetone.
[0029] Optionally, in the passivation solution, the mass percentage concentration of the passivation material is 1%-99.9%.
[0030] Optionally, the width of the area to be passivated along the first direction is 3 mm-1.2 cm.
[0031] Optionally, the rolling pressure is 1Mpa-10Mpa.
[0032] The preparation method of the battery positive electrode sheet provided in the present application has a simple and controllable process, is easy to operate, is conducive to realizing automated production, and the obtained battery positive electrode sheet has good structural stability. Applying it in a battery can make the battery have good cycle performance and safety performance.
[0033] In a third aspect, the present application provides a battery, comprising a positive electrode, a negative electrode, an electrolyte, and a separator located between the positive electrode and the negative electrode, wherein the positive electrode comprises the battery positive electrode sheet described in the first aspect of the present application or the battery positive electrode sheet obtained by the preparation method described in the second aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 is a schematic diagram of the structure of a battery;
[0035] Figure 2 A top view of a coated electrode prepared by an intermittent coating method;
[0036] Figure 3 This is a front view of a coated electrode prepared by an intermittent coating method;
[0037] Figure 4 Schematic diagram of bad areas of electrodes in a battery;
[0038] Figure 5 A top view of a positive electrode sheet of a battery provided in one embodiment of the present application;
[0039] Figure 6 A front view of a positive electrode sheet of a battery provided in one embodiment of the present application;
[0040] Figure 7 A schematic diagram of the passivation region layer structure provided in one embodiment of the present application. DETAILED DESCRIPTION
[0041] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0042] See also Figure 1 , Figure 1 The figure is a schematic diagram of the battery structure. The core components of the battery include the positive electrode sheet 10, the negative electrode sheet 20, the separator 30 and the electrolyte 40 as well as the corresponding connecting accessories and circuits. In the related art, since a blank area must be reserved on the current collector for welding the pole lugs, an intermittent coating method is often used to coat the active material layer to obtain the coated pole sheet, and then the coated pole sheet is cut and rolled to obtain the battery pole sheet. The intermittent coating method is to coat a section of slurry on the surface of the current collector and leave a blank section before coating the next section of slurry. Please refer to Figure 2 , Figure 2 The top view of the coated electrode sheet prepared by the intermittent coating method. The active material layer 102 is arranged on the surface of the current collector 101 at intervals, and the current collector 101 has an interval of blank areas. When the intermittent coating method is used, the thickness of the active material layer formed by the machine at the start and end of coating is not uniform, and the thickness at the edge of the active material layer will be greater. Please refer to Figure 3 , Figure 3 This is the front view of the coated electrode prepared by the intermittent coating method. Figure 3 In the embodiment, the thickness of the edge region of the active material layer 102 along the coating direction is greater than that of the middle region, and the thicker region is the defective region of the positive electrode sheet of the battery.
[0043] During the use of the battery, since there are more active materials in the bad area of the positive electrode, the lithium ion concentration in the bad area of the positive electrode will be higher during the battery charging process, and the corresponding lithium ion concentration in the negative electrode area will also be higher, which makes it easy for lithium dendrites to form in this area of the negative electrode. Figure 4 , Figure 4 Schematic diagram of the bad area of the electrode in the battery. Figure 4In the figure, area a represents the bad area with high lithium ion concentration in the positive electrode of the battery, that is, area a is the bad area with thick positive active material layer, and area b is the area of the negative electrode of the battery corresponding to area a. After long-term use of the battery, area b is very likely to produce a large number of lithium dendrites. The hazards of lithium dendrites are mainly in three aspects: first, they will puncture through the diaphragm to cause short circuits and cause serious safety accidents; second, lithium dendrites can react with the electrolyte in situ to form an electronic insulation film on the surface, which will cause mutual electronic insulation between lithium dendrites. Once the root system is broken, the entire lithium dendrite loses its electrochemical activity, resulting in a rapid decrease in battery capacity; third, the spatial volume of lithium dendrites is large, which can easily lead to battery volume expansion and battery cycle performance attenuation. In addition, the bad area of the active material layer of the positive electrode is prone to material shedding, which is also not conducive to the battery's cycle performance and safety performance.
[0044] To solve the above problems, the relevant technology is to stick tape on the edge of the active material layer coating. However, the tape contains polyurethane adhesives, and the main components are polyisocyanate, polyether, alcohol, etc. The above components are easy to diffuse into the electrolyte, which is not conducive to the electrochemical performance and safety performance of the battery. In addition, after multiple charge and discharge cycles of the battery with positive electrode glue, the negative electrode position corresponding to the tape will still have relatively serious lithium dendrite precipitation, which cannot solve the problem well.
[0045] In order to improve the electrochemical performance and safety performance of the battery, the present application provides a battery positive electrode sheet, which passivates the undesirable areas with high lithium ion concentration, inhibits the infiltration of the electrolyte into the passivated area, slows down the escape rate of lithium ions, thereby effectively inhibiting the formation of lithium dendrites, and at the same time improves the structural stability of the battery positive electrode sheet. Applying it in the battery can effectively enhance the battery's cycle performance and safety performance.
[0046] See also Figure 5 , Figure 5 A top view of a positive electrode sheet of a battery provided in one embodiment of the present application. Figure 5 In the embodiment, the positive electrode sheet 10 of the battery includes a current collector 101 and an active material layer 102 disposed on the surface of the current collector 101; the active material layer 102 includes an active region c and a passivation region d; the passivation region d is located on two opposite sides of the active region c along the first direction. For further explanation of the position of the passivation region of the present application, please refer to Figure 6 , Figure 6 This is a front view of a positive electrode sheet of a battery provided in one embodiment of the present application. Figure 6In the invention, the active material layer 102 includes an active region c and a passivation region d located on opposite sides of the active region c along a first direction. In the present application, the first direction refers to a direction parallel to the coating direction of the battery pole piece. Since the battery pole piece is coated in sections, the thickness of the edge portion of the active material layer along the coating direction is relatively thick. The present application can effectively solve the problem caused by the uneven thickness of the active material by passivating the above-mentioned region. It can be understood that in the present application, the shape of the active material layer is a rectangle, the shape of the active region is a rectangle, and the two opposite sides of the active region are parallel to the first direction, and the other two opposite sides of the active region are perpendicular to the first direction; the shape of the passivation region is a rectangle, and the two opposite sides of the passivation region are parallel to the first direction, and the other two opposite sides of the passivation region are perpendicular to the first direction.
[0047] In the embodiments of the present application, the active region includes an active material, and the active material refers to a material that can reversibly release and embed lithium ions. In the present application, there is no special limitation on the active material, and the active material can be any active material known in the art. In some embodiments of the present application, the active material includes LiFePO4, Li3V2(PO4)3, LiMn2O4, LiMnO2, LiNiO2, LiCoO2, LiVPO4F, LiFeO2 or Li 1+x L 1-y-z M y N z One or more of O2, wherein -0.1≤x≤0.2, 0≤y≤1, 0≤z≤1, 0≤y+z≤1.0, and L, M, and N are selected from Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Al, Mg, and Ga, respectively.
[0048] In the embodiment of the present application, the passivation region includes a passivation material and an active material, the passivation material and the active material are mixed to form a composite layer, and the passivation material includes one or more of polyethylene glycol and polyethylene glycol derivatives. In the present application, the passivation material can wrap the active material and block the pores between the active materials, making it difficult for the electrolyte to infiltrate the passivation region, thereby inhibiting the release of lithium ions in the passivation region and reducing the concentration of lithium ions in the passivation region; and the passivation material of the present application is insoluble in the electrolyte of the battery, on the one hand, it can firmly wrap the active material, so that the positive electrode sheet of the battery has good stability, and on the other hand, it has no effect on the electrochemical performance of the battery. In some embodiments of the present application, polyethylene glycol is used as a passivation material. Polyethylene glycol has a good affinity for active materials, can fully wrap the active materials, and block the pores in the passivation region, so that the lithium ions in the passivation region are difficult to escape normally, and polyethylene glycol is incompatible with the electrolyte and has no side effects on the battery. In the embodiment of the present application, the average molecular weight of polyethylene glycol is 2000-8000. The average molecular weight of polyethylene glycol may be, but is not limited to, 2000, 3000, 4000, 5000, 6000 or 8000.
[0049] In an embodiment of the present application, the mass ratio of the active material to the passivation material in the composite layer is 1:(0.001-0.03). The mass ratio of the active material to the passivation material in the composite layer may be, but is not limited to, 1:0.001, 1:0.005, 1:0.01, 1:0.001, 1:0.005, 1:0.01 or 1:0.03. When the mass ratio of the active material to the passivation material in the composite layer of the passivation region is 1:(0.001-0.03), the passivation material can fully block the pores between the active materials, thereby effectively inhibiting the electrolyte from wetting the passivation region. In an embodiment of the present application, the thickness of the composite layer is 1 μm-200 μm, wherein the thickness of the composite layer refers to the maximum thickness of the composite layer. The thickness of the composite layer may be, but is not limited to, 1 μm, 5 μm, 10 μm, 50 μm, 100 μm, 150 μm or 200 μm.
[0050] In the embodiment of the present application, the passivation region further includes a passivation layer disposed on the surface of the composite layer, and the passivation layer includes a passivation material. Figure 7 , Figure 7 A schematic diagram of the layer structure of the passivation region provided in one embodiment of the present application. Figure 7, the passivation region d includes a composite layer B and a passivation layer A disposed on the surface of the composite layer B. In an embodiment of the present application, the thickness of the passivation layer is less than or equal to 20 μm, wherein the thickness of the passivation layer refers to the maximum thickness of the passivation layer. The thickness of the passivation layer may be, but is not limited to, 0.1 μm, 0.5 μm, 1 μm, 5 μm, 10 μm, 15 μm or 20 μm. In the present application, the passivation layer can isolate the passivation region from the electrolyte, thereby inhibiting the electrolyte from infiltrating the passivation region, reducing the diffusion rate of lithium ions and the concentration of lithium ions in the passivation region, and reducing the risk of lithium plating at the negative electrode.
[0051] In the implementation manner of the present application, the active region also includes a conductive agent and a binder, and the passivation region also includes a conductive agent and a binder. In the present application, the binder and the conductive agent can be any binder and conductive agent known in the art. In some implementation manners of the present application, the binder includes one or more of polyvinylidene fluoride, polytetrafluoroethylene, polyhexafluoropropylene, styrene-butadiene rubber, sodium carboxymethyl cellulose, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polyamide, polyacrylonitrile and polyacrylate. In some implementation manners of the present application, the conductive agent includes one or more of acetylene black, carbon black, carbon nanotubes, carbon nanofibers, activated carbon and graphene.
[0052] In the embodiment of the present application, the mass percentage of the passivation material in the passivation region is 0.1-3%. The mass percentage of the passivation material in the passivation region may be, but is not limited to, 0.1%, 0.3%, 0.5%, 1%, 1.5% or 3%. In the embodiment of the present application, the mass percentage of the active material in the passivation region is 62%-99.7%. The mass percentage of the active material in the passivation region may be, but is not limited to, 62%, 80%, 90% or 99.7%.
[0053] In the embodiment of the present application, the mass percentage of the binder in the passivation region is 0.1%-15%. The mass percentage of the binder in the passivation region can be, but not limited to, 0.1%, 0.5%, 1%, 2%, 5%, 7%, 10% or 15%. In the embodiment of the present application, the mass percentage of the conductive agent in the passivation region is 0.1%-20%. The mass percentage of the conductive agent in the passivation region can be, but not limited to, 0.1%, 0.5%, 1%, 2%, 5%, 10%, 15% or 20%.
[0054] In an embodiment of the present application, the width of the passivation region along the first direction is 1 mm-2 cm. In some embodiments of the present application, the width of the passivation region along the first direction is 3 mm-1.2 cm. The width of the passivation region along the first direction may be, but is not limited to, 1 mm, 3 mm, 5 mm, 7 mm, 1 cm, 1.2 cm or 2 cm. Within the above width range, the passivation region can effectively cover the bad area of the electrode, thereby alleviating the problem of negative electrode lithium plating.
[0055] In an embodiment of the present application, the thickness of the active material layer is 10 μm-200 μm. The thickness of the active material layer may be, but is not limited to, 10 μm, 20 μm, 50 μm, 100 μm, 150 μm or 200 μm. In an embodiment of the present application, the thickness of the current collector is 5 μm-100 μm. In some embodiments of the present application, the thickness of the current collector is 8 μm-20 μm. The thickness of the current collector may be, but is not limited to, 5 μm, 10 μm, 20 μm, 50 μm, 70 μm, 90 μm or 100 μm.
[0056] The battery positive electrode sheet provided in the present application can effectively inhibit the electrolyte from wetting the passivation area of the positive electrode by passivating the positive electrode, hinder the escape of lithium ions in the passivation area, and reduce the transmission rate of lithium ions in the passivation area, thereby alleviating the problem of lithium precipitation at the negative electrode position corresponding to the passivation area, and at the same time effectively improve the structural stability of the battery positive electrode sheet.
[0057] The present application also provides a method for preparing the above-mentioned battery positive electrode sheet, comprising the following steps:
[0058] Step 100: providing a current collector, and coating a surface of the current collector to form an active material layer to be passivated, wherein the active material layer to be passivated includes an active region and regions to be passivated located on opposite sides of the active region along a first direction;
[0059] Step 200: dripping a passivation liquid into the area to be passivated, forming a passivation area after drying and obtaining an active material layer, and rolling the active material layer to obtain a positive electrode sheet of a battery.
[0060] In step 100 of the present application, the first direction is parallel to the coating direction. The active material layer to be passivated can be formed by coating the current collector surface with any preparation method known in the art. In the embodiment of the present application, the active material layer to be passivated is formed by coating with an intermittent coating method, and the drying temperature after coating is 50°C-150°C.
[0061] In step 200 of the present application, the area to be passivated refers to the bad area of the electrode, and the bad area includes the area where the thickness of the electrode active material layer is uneven. When preparing the passivation area, a passivation solution is dripped into the area to be passivated, and the passivation solution can penetrate into the area to be passivated. After the passivation solution is dried, the passivation material will form a solid film wrapped on the surface of the active material, and at the same time block the gaps in the active material layer, thereby inhibiting the electrolyte from infiltrating the passivation area, wherein the part infiltrated by the passivation solution forms a composite layer of the passivation area after drying, and part of the passivation material will adhere to the surface of the composite layer to form a passivation layer. In the present application, the thickness of the composite layer is related to the volume of the passivation solution dripped, the concentration of the passivation solution, and the type of passivation material. In some embodiments of the present application, the passivation solution completely penetrates the active material layer of the area to be passivated, that is, the thickness of the composite layer is equal to the thickness of the active material layer of the passivation area. In some embodiments of the present application, the passivation solution partially penetrates the active material layer of the area to be passivated, that is, the thickness of the composite layer is less than the thickness of the active material layer of the passivation area. In the present application, when the passivation solution completely penetrates the active material layer in the area to be passivated, the passivation effect is optimal. In the embodiment of the present application, the temperature at which the passivation solution is dried is 50°C-150°C. The temperature at which the passivation solution is dried can be, but is not limited to, 50°C, 60°C, 70°C, 80°C, 100°C, 120°C or 150°C.
[0062] In an embodiment of the present application, the solute of the passivation solution includes a passivation material, and the passivation material includes one or more of polyethylene glycol and polyethylene glycol derivatives. Polyethylene glycol and polyethylene glycol derivatives have good solubility, which is conducive to obtaining a passivation solution with uniform components, thereby promoting the passivation solution to penetrate into the bad area of the active material layer and realize the passivation of the bad area. In an embodiment of the present application, the average molecular weight of polyethylene glycol is 2000-8000. The average molecular weight of polyethylene glycol can be specifically but not limited to 2000, 3000, 4000, 5000, 6000 or 8000. When the average molecular weight of polyethylene glycol is too high, the solubility of polyethylene glycol is low, and it is not easy to prepare a high concentration coating solution; when the average molecular weight of polyethylene glycol is too low, the fluidity of the coating solution is high, and it is easy to contaminate the normal area. In an embodiment of the present application, the solvent of the passivation solution includes a volatile organic solvent, and the boiling point of the volatile organic solvent is less than or equal to 100°C. When a volatile organic solvent is used, the passivation liquid can evaporate quickly after penetrating into the bad area, thereby inhibiting the passivation liquid from penetrating into the normal area of the electrode and ensuring the effective capacity of the battery. In the embodiment of the present application, the boiling point of the volatile organic solvent can be specifically but not limited to 50°C, 60°C, 65°C, 70°C, 78°C, 85°C or 100°C. In some embodiments of the present application, the volatile organic solvent includes one or more of ethanol, methanol, dichloromethane, chloroform and acetone. In some embodiments of the present application, an ethanol solution of polyethylene glycol is used as a passivation liquid. Polyethylene glycol can effectively block the pores between the active materials, and polyethylene glycol has a high solubility in ethanol. A small amount of passivation liquid can be used to complete the passivation of the bad area, thereby reducing the penetration of the passivation liquid in the direction of the active area and effectively controlling the position of the passivation area.
[0063] In the implementation mode of the present application, the mass percentage concentration of the passivation material in the passivation solution is 1%-99.9%. The mass percentage concentration of the passivation material in the passivation solution can be, but is not limited to, 1%, 5%, 10%, 20%, 40%, 50%, 60%, 70%, 90% or 99.9%. In some implementation modes of the present application, the mass percentage concentration of the passivation material in the passivation solution is 50%-70%. When the concentration of the passivation material is too low, the solvent volatilization time is long, and the passivation solution is easy to penetrate into the normal area of the electrode. When the concentration of the passivation material is too high, the passivation solution is not easy to penetrate the passivation area, which will reduce the passivation effect. Within the concentration range of the present application, the passivation solution can not only fully passivate the bad area of the electrode, making it difficult for lithium ions in the bad area to escape, but also has little effect on the normal area of the electrode.
[0064] In the present application, rolling the active material layer means rolling the entire active material layer, that is, the rolling position includes the active area and the passivation area of the active material layer. In the embodiment of the present application, the pressure of rolling the active material layer is 1Mpa-10Mpa. The rolling pressure can be but not limited to 1Mpa, 3Mpa, 5Mpa or 10Mpa. Under the above pressure range, a structurally stable active material layer can be formed.
[0065] The present application also provides a lithium-ion battery, which includes a positive electrode, a negative electrode, an electrolyte, and a separator located between the positive electrode and the negative electrode, wherein the positive electrode includes the battery positive electrode sheet provided in the present application.
[0066] In the present application, the negative electrode of the lithium-ion battery can be any negative electrode known in the art. In the embodiment of the present application, the negative electrode may include one or more of a carbon-based negative electrode, a silicon-based negative electrode, a tin-based negative electrode, a lithium negative electrode, a sodium negative electrode, a potassium negative electrode, a magnesium negative electrode, a zinc negative electrode and an aluminum negative electrode. Among them, the carbon-based negative electrode may include graphite, hard carbon, soft carbon, graphene, etc.; the silicon-based negative electrode may include silicon, silicon carbon, silicon oxygen, silicon metal compounds, etc.; the tin-based negative electrode may include tin, tin carbon, tin oxygen, tin metal compounds; the lithium negative electrode may include metallic lithium or a lithium alloy. The lithium alloy may specifically be at least one of a lithium silicon alloy, a lithium sodium alloy, a lithium potassium alloy, a lithium aluminum alloy, a lithium tin alloy and a lithium indium alloy. In some embodiments of the present application, the current collector of the negative electrode is a copper foil, which can be a porous structure or a common copper foil, and the thickness of the copper foil is 5μm-100μm, and further, the thickness of the copper foil is 10μm-20μm; the negative electrode active material includes one or more of natural graphite, artificial graphite, hard carbon, soft carbon, lithium titanate, iron oxide, lithium titanium phosphate, titanium dioxide, silicon, silicon oxide, aluminum, tin and antimony; the binder includes one or more of polyacrylic acid (PAA), polyvinylidene fluoride (PVDF), carboxymethyl cellulose (CMC) and styrene butadiene latex (SBR); the conductive agent includes one or more of acetylene black, Ketjen black, Super-P, carbon nanotubes, carbon nanofibers, activated carbon and graphene. In the present application, the preparation method of the negative electrode can adopt any method known in the art.
[0067] In the present application, the separator of the lithium-ion battery can be any separator known to those skilled in the art, for example, the separator can be one or more of polyolefin microporous membrane, polyethylene terephthalate, polyethylene felt, glass fiber felt or ultrafine glass fiber paper.
[0068] In the present application, the electrolyte of the lithium ion battery includes a solution of an electrolyte lithium salt in a non-aqueous solvent. In an embodiment of the present application, the electrolyte lithium salt includes lithium hexafluorophosphate (LiPF6), lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium hexafluorosilicate (LiSiF6), lithium tetraphenylborate (LiB(C6H5)4), lithium chloride (LiCl), lithium bromide (LiBr), lithium chloroaluminate (LiAlCl4), lithium fluoroalkylsulfonate (LiC(SO2CF3)3), LiCH3SO3, LiN(SO2CF3)2 and LiN(SO2C2F5)2. In some embodiments of the present application, the non-aqueous solvent includes one or more of a chain acid ester and a cyclic acid ester. In some embodiments of the present application, the chain acid ester includes one or more of dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methyl propyl carbonate (MPC) and dipropyl carbonate (DPC). In some embodiments of the present application, the chain acid ester includes chain organic esters containing fluorine, sulfur or unsaturated bonds. In some embodiments of the present application, the cyclic acid ester includes one or more of ethylene carbonate (EC), propylene carbonate (PC), vinylene carbonate (VC), γ-butyrolactone (γ-BL) and sultone. In some embodiments of the present application, the cyclic acid ester includes cyclic organic esters containing fluorine, sulfur or unsaturated bonds. In some embodiments of the present application, the non-aqueous solvent includes one or more of chain ethers and cyclic ether solutions. In some embodiments of the present application, the cyclic ether includes one or more of tetrahydrofuran (THF), 2-methyltetrahydrofuran (2-MeTHF), 1,3-dioxolane (DOL) and 4-methyl-1,3-dioxolane (4-MeDOL).
[0069] In some embodiments of the present application, the cyclic ether includes a fluorine-containing, sulfur-containing or unsaturated bond-containing cyclic organic ether. In some embodiments of the present application, the chain ether includes one or more of dimethoxymethane (DMM), 1,2-dimethoxyethane (DME), 1,2-dimethoxypropane (DMP) and diethylene glycol dimethyl ether (DG).
[0070] In some embodiments of the present application, the chain ether includes a chain organic ether containing fluorine, sulfur or unsaturated bonds. In some embodiments of the present application, the concentration of the electrolyte lithium salt in the electrolyte is 0.1 mol / L-15 mol / L. In some embodiments of the present application, the concentration of the electrolyte lithium salt is 1 mol / L-10 mol / L.
[0071] In the embodiments of the present application, the battery can be prepared by using either a lamination process or a winding process. In some embodiments of the present application, the battery is prepared by using a lamination process.
[0072] The lithium-ion battery provided in the present application has good cycle performance and safety performance due to the use of the battery positive electrode sheet of the present application.
[0073] The present application also provides a power vehicle, which includes the above-mentioned lithium-ion battery.
[0074] The technical solution of the present application is further described below with reference to a number of embodiments.
[0075] Example 1
[0076] 1) Preparation of battery positive electrode:
[0077] Weigh 1kg of positive electrode active material (LiCoO2), 20g of conductive agent (carbon nanotubes) and 20g of binder (vinylidene fluoride, PVDF) and add them to 1kg of N-methylpyrrolidone, stir in a mixer for 30 minutes to form a stable and uniform slurry; evenly coat the slurry on the surface of the current collector aluminum foil, put it in an oven and dry it at 80°C to obtain an active material layer; drip the passivation liquid in the 1cm area of the edge of the active material layer so that the droplets evenly cover the edge surface of the active material layer, dry the solution in an oven at 80°C, and then press the active material layer at a pressure of 2Mpa, roll it to obtain a battery positive electrode sheet, and spot weld the pole ear to obtain a battery positive electrode. Among them, the passivation liquid is a PEG ethanol solution with a mass percentage of 60%, the average molecular weight of PEG is 4000, and the thickness of the active material layer of the obtained battery positive electrode is 95μm, that is, the thickness of the active area in the active material layer is 95μm.
[0078] 2) Preparation of battery negative electrode:
[0079] Weigh 1 kg of negative electrode active material (composite negative electrode material of natural graphite and artificial graphite with a particle size of 15 μm, and the mass ratio of natural graphite to artificial graphite is 1:9), 10 g of conductive agent (acetylene black), and binder (30 g of styrene-butadiene rubber, 20 g of sodium carboxymethyl cellulose) and add them to 1 kg of deionized water. After stirring, coating, drying, rolling, and spot welding the pole ears, the battery negative electrode is obtained.
[0080] 3) Preparation of batteries:
[0081] The battery positive electrode, battery negative electrode and polyolefin microporous membrane separator prepared above were wound into a battery core, and after packaging, 1 mol / L lithium hexafluorophosphate electrolyte (solvent is 1:1:1 EC:DMC:DPC) was injected to obtain a battery. The battery of Example 1 was named DS-1.
[0082] Example 2
[0083] The difference from Example 1 is that the passivation solution in Example 2 is a PEG ethanol solution with a mass percentage of 30%. The battery in Example 2 is named DS-2.
[0084] Example 3
[0085] The difference from Example 1 is that the passivation solution in Example 3 is a PEG ethanol solution with a mass percentage of 80%. The battery in Example 3 is named DS-3.
[0086] Example 4
[0087] The difference from Example 1 is that the average molecular weight of PEG in Example 4 is 2000, and the battery of Example 4 is named DS-4.
[0088] Example 5
[0089] The difference from Example 1 is that the average molecular weight of PEG in Example 4 is 8000, and the battery of Example 5 is named DS-5.
[0090] Example 6
[0091] The difference from Example 1 is that the passivation solution in Example 6 is added to an area 1 mm from the edge of the active material layer. The battery of Example 5 is named DS-6.
[0092] Comparative Example 1
[0093] The difference from Example 1 is that in Comparative Example 1, the active material layer after drying is directly rolled to obtain the positive electrode sheet of the battery. The battery of Comparative Example 1 is named DS-7.
[0094] Comparative Example 2
[0095] The difference from Example 1 is that in Comparative Example 2, a tape is pasted on the 1-2 cm area at the edge of the active material layer after drying. The tape used is an existing commercial BOPP film substrate tape. The battery of Comparative Example 2 is named DS-8.
[0096] Effect Example
[0097] In order to verify the structure and performance of the battery positive electrode sheet prepared in the present application, the present application also provides an effect embodiment.
[0098] 1) The passivation region and the composite layer and the passivation layer of the battery positive electrode sheets of Examples 1-6 were measured by SEM, and the content of the composite layer in the passivation region of the battery positive electrode sheets of Examples 1-5 and 1-6 was analyzed by calculation. Please refer to Table 1, which is a table of structural parameters and content parameters of the battery positive electrode sheets of Examples 1-6, wherein m 活 / m 钝 is the mass ratio of the active material of the composite layer to the passivation material in the passivation region.
[0099] Table 1 Structural parameters and content parameters of the positive electrode sheets of the batteries of Examples 1-6
[0100]
[0101] 2) The batteries of Examples 1-6 and Comparative Examples 1-2 were subjected to charge and discharge tests. The specific test conditions were as follows: using a blue electric test system, the positive electrode and the negative electrode were connected, and the battery was subjected to two stages of charge and discharge tests. The first stage of the charge and discharge system was: standing for 1 minute, constant current charging to 4.45V at 8mA current, then constant voltage charging at 4.45V, with a cut-off current of 2mA, then standing for 10 minutes, 8mA constant current discharge, with a cut-off voltage of 2V, and standing for 50 hours. The first stage of the test is used to form the SEI film in the battery formation and to reduce the polarization of the battery. The second stage of the charge and discharge system was: 60mA constant current charging, with a cut-off voltage of 4.45V; 4.45V constant voltage charging, with a cut-off current of 2mA; after standing for 10 minutes, 60mA constant current discharge, with a cut-off voltage of 2V, and then the second stage of the charge and discharge cycle was stopped after 800 cycles. The second stage of the test is used to test the cycle performance of the battery. The first cycle charging refers to the battery after the first test, first 60mA constant current charging to 4.45V, and then 4.45V constant voltage charging to a cut-off current of 2mA; the first cycle discharge capacity refers to the capacity discharged by the battery when the voltage is 2V at 60mA constant current. And the discharge capacity after the subsequent 800 cycles is calculated with the discharge capacity of the first cycle as the reference 100%. Please refer to Table 2, which shows the change value of the discharge capacity retention rate of the batteries of Examples 1-6 and Comparative Examples 1-2 during 800 cycles of charge and discharge.
[0102] Table 2 Cyclic performance test table of the batteries of Examples 1-6 and Comparative Examples 1-2
[0103]
[0104]
[0105] It can be seen from the test results of Table 2 that compared with the battery composed of the untreated positive electrode of Comparative Example 1 and the positive electrode treated with glue in Comparative Example 2, the battery obtained by using the positive electrode sheet of the battery in the embodiment of the present application has a higher capacity retention rate and a better cycle performance. In the embodiment of the present application, after the bad positive electrode area is passivated, the discharge capacity retention rate of the battery is significantly improved, and with the increase of the concentration of the passivation solution, the capacity retention rate of the battery gradually increases. When the concentration is 60%, the capacity retention rate of the DS-3 battery reaches 99%, proving that the passivation treatment of the present application can effectively improve the battery performance. At the same time, it was found that the molecular weight of PEG affects the fluidity of the passivation solution. Compared with PEG with a molecular weight of 2000 and PEG with a molecular weight of 8000, when PEG with a molecular weight of 4000 is used as the solute, the fluidity of the obtained passivation solution is moderate, the blocking effect is better, and the battery has a higher capacity retention rate.
[0106] The above experimental results show that when the surface of the battery positive electrode is covered with tape, the battery will have obvious lithium deposition after multiple cycles, which reduces the battery capacity retention rate. However, after the passivation treatment is performed using the method of the present application, when the obtained battery positive electrode is assembled into a battery, the phenomenon of lithium deposition at the negative electrode is greatly reduced, thereby enhancing the battery's cycle performance and safety performance.
[0107] The above is a preferred embodiment of the present application, but it should not be understood as limiting the scope of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present application, and these improvements and modifications are also considered to be within the scope of protection of the present application.
Claims
1. A positive electrode sheet for a battery, It is characterized in that It includes a current collector and an active material layer arranged on the surface of the current collector; the active material layer includes an active area and a passivation area located on opposite sides of the active area along a first direction; the active area includes an active material; the passivation area includes a composite layer and a passivation layer, the composite layer includes the active material and a passivation material mixed with the active material; the passivation layer is arranged on the surface of the composite layer; the passivation layer includes the passivation material, and the passivation material includes one or more of polyethylene glycol and polyethylene glycol derivatives.
2. The positive electrode sheet of a battery as claimed in claim 1, It is characterized in that The thickness of the composite layer is 1 μm-200 μm.
3. The positive electrode sheet of a battery as claimed in claim 1, It is characterized in that, In the composite layer, the mass ratio of the active material to the passivation material is 1:(0.001-0.03). The battery positive electrode sheet according to claim 1 , wherein the thickness of the passivation layer is less than or equal to 20 μm.
5. The positive electrode sheet of a battery as claimed in claim 1, It is characterized in that The average molecular weight of the passivation material is 2000-8000.
6. The positive electrode sheet of a battery as claimed in claim 1, It is characterized in that The width of the passivation region along the first direction is 3 mm-1.2 cm.
7. A method for preparing a positive electrode sheet of a battery as claimed in any one of claims 1 to 6, It is characterized in that The following steps are involved: Providing a current collector, and coating the surface of the current collector with a layer of active material to be passivated; The active material layer to be passivated includes an active region and regions to be passivated located on opposite sides of the active region along the first direction; A passivation liquid is dripped into the area to be passivated, and after drying, a passivation area is formed and an active material layer is obtained, and the active material layer is rolled to obtain the battery positive electrode sheet; the passivation liquid includes a passivation material, and the passivation material includes one or more of polyethylene glycol and polyethylene glycol derivatives.
8. The preparation method according to claim 7, It is characterized in that The solvent of the passivation solution includes a volatile organic solvent; the boiling point of the volatile organic solvent is less than or equal to 100°C.
9. A battery, It is characterized in that It comprises a positive electrode, a negative electrode, an electrolyte and a separator located between the positive electrode and the negative electrode, wherein the positive electrode comprises the battery positive electrode sheet as described in any one of claims 1 to 6 or the battery positive electrode sheet obtained by the preparation method as described in claim 7 or 8.