A photovoltaic N-type TOPCon cell ALD passivation film manufacturing process
In the ALD process, O3 gas is first used to remove wet residues on the silicon wafer surface and a SiO2 film is prepared, and then H2O and TMA are used to alternately deposit Al2O3 films. This solves the problem of poor passivation effect in the existing technology and significantly improves photovoltaic efficiency. The open circuit voltage and conversion efficiency of the battery.
Patent Information
- Application Number
- CN202210856578.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-20
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-07-20
AI Technical Summary
When the existing ALD process is used to manufacture the Al2O3 passivation film of photovoltaic N-type TOPCon cells, the wet residue on the surface of the silicon wafer cannot be completely cleaned, resulting in a weakened passivation effect and an impact on the open circuit voltage.
In the ALD process chamber, O3 gas is first introduced to remove wet process residues and a SiO2 film is prepared, and then H2O vapor is introduced to form a passivation interface. TMA and H2O are then alternately introduced to grow an Al2O3 film, and the passivation is improved through the dynamic balance of O3 and H2O. Effect.
Effectively removes wet residues on the silicon wafer surface, reduces interface recombination, improves open circuit voltage and conversion efficiency, and simplifies the process without increasing costs.
Smart Images

Figure CN115274923B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of photovoltaic cell manufacturing, in particular to a photovoltaic N-type TOPCon cell ALD passivation film manufacturing process. Background Art
[0002] Atomic layer deposition (ALD) is a technology that forms a deposited film by alternately passing gaseous precursors into a reactor and causing chemical reactions. This technology can coat the material on the substrate surface layer by layer in the form of a single atomic layer. After the precursors are deposited on the substrate surface, they will chemically adsorb on the substrate surface, and then the reactor needs to be purged with an inert gas to remove the remaining precursors that are not adsorbed on the substrate surface to ensure that the chemical reaction only occurs on the substrate surface. In the field of photovoltaic cells, ALD is used to manufacture Al2O3 passivation films. Different processes during the ALD film growth process affect the quality of the passivation effect.
[0003] The existing ALD atomic layer deposition technology is to place the silicon wafer in a vacuum reaction chamber, alternately introduce TMA and H2O when the chamber temperature reaches 200-250℃, and use N2 to purge the remaining gas after introducing one gas and waiting for the deposition time. The desired Al2O3 film thickness is achieved according to the number of cycles of alternately introducing the gas. The traditional PERC cell passivation film manufacturing process is used on N-type TOPCon cells. Due to the uneven velvet surface, the chemical additives remaining in the wet process cannot be completely cleaned, forming a composite center on the silicon wafer, thereby weakening the passivation effect of Al2O3 in the ALD process. Summary of the invention
[0004] In view of the above shortcomings in existing production, the applicant provides a photovoltaic N-type TOPCon cell ALD passivation film manufacturing process, thereby solving the problem of cleaning the silicon wafer surface residue before ALD aluminum oxide coating of the N-type TOPCon cell, reducing recombination, improving the passivation effect, and further increasing the open circuit voltage.
[0005] The technical solution adopted by the present invention is as follows:
[0006] A photovoltaic N-type TOPCon cell ALD passivation film manufacturing process comprises the following steps:
[0007] Step S1, placing the substrate processed by the wet process in the process chamber, forming a vacuum constant temperature environment in the process chamber, and the target temperature is 200-300° C.;
[0008] Step S2, circulating O3 gas in the process chamber to remove wet process residues on the surface of the silicon wafer and prepare a SiO2 film;
[0009] Step S3, introducing H2O vapor into the process chamber to deposit on the SiO2 surface to form a passivation interface;
[0010] Step S4, alternately introducing TMA and H2O vapor into the process chamber to grow a highly passivated Al2O3 film;
[0011] Step S5, purging and breaking the vacuum to complete the process.
[0012] As a further improvement of the above technical solution:
[0013] The substrate in step S1 is a silicon wafer.
[0014] Step S1 further includes: heating the process chamber for 200s, with a target temperature of 200-300°C, and evacuating the process chamber to a low pressure of 0.05-0.3 mTorr, thereby forming a vacuum constant temperature environment in the process chamber.
[0015] Step S1 further includes: after a vacuum constant temperature environment is formed in the process chamber, the duration is 200-600 seconds.
[0016] Step S2 further includes: a method of circulating O3 gas into the process chamber includes introducing O3 gas for a duration of 30-200 seconds, then introducing N2 for purging, the purging time is 0-100 seconds, and performing 1-5 cycles.
[0017] Step S3 further includes: the method of introducing H2O steam into the process chamber includes introducing H2O steam for a duration of 5-30 seconds, and then introducing N2 for purging for 0-100 seconds.
[0018] Step S4 further includes: a method of alternately introducing TMA and H2O vapor into the process chamber includes first introducing TMA for a duration of 0.5-5s, then introducing N2 for purging for a duration of 1-10s, pausing for 0.5-5s, then introducing H2O for a duration of 2-7s, pausing for 0.5-5s, then introducing N2 for purging for a duration of 1-10s, pausing for 0.5-5s, this is one cycle, and the cycle is performed continuously for 20-70 times.
[0019] The beneficial effects of the present invention are as follows:
[0020] The present invention introduces O3 gas before the ALD process, which can effectively remove the wet residue on the surface of the silicon wafer and prepare the SiO2 film, which has both the effect of interface passivation and the effect of improving anti-PID. After the SiO2 film is prepared, H2O vapor is introduced for a certain period of time and deposited on the surface of the silicon wafer, so that the SiO2 film forms a good contact with the subsequent Al2O3 film. During sintering, H+ (hydrogen ions) overflow, reduce interface recombination and thus increase the open circuit voltage; and form a dynamic balance with the subsequent alternating introduction of TMA and H2O. The above steps have a significant effect on improving the battery Eta (conversion efficiency). BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a schematic diagram of the process of the present invention. DETAILED DESCRIPTION
[0022] The specific implementation of the present invention will be described below in conjunction with the accompanying drawings.
[0023] like Figure 1 As shown, the photovoltaic N-type TOPCon cell ALD passivation film manufacturing process of the present invention comprises the following steps:
[0024] Step S1, placing a substrate processed by a wet process in a process chamber, the substrate being a silicon wafer, etc., heating the process chamber for 200 seconds, the target temperature being 200-300° C., evacuating the process chamber to a low pressure of 0.05-0.3 mTorr, forming a vacuum constant temperature environment in the process chamber, the duration being 200-600 seconds, and the target temperature being 200-300° C.;
[0025] Step S2, introducing O3 gas into the process chamber to remove wet process residues on the surface of the silicon wafer and prepare a SiO2 film, the duration is 30-200 seconds, and then introducing N2 for purging, the purge time is 0-100 seconds, and performing 1-5 cycles;
[0026] Step S3, introducing H2O vapor into the process chamber to deposit on the SiO2 surface to form a passivation interface for 5-30 seconds, and then introducing N2 to purge for 0-100 seconds;
[0027] Step S4, alternately introducing TMA (trimethylaluminum) and H2O vapor into the process chamber to grow a highly passivated Al2O3 film, including first introducing TMA for a duration of 0.5-5s, then introducing N2 for purging for a duration of 1-10s, pausing for 0.5-5s, then introducing H2O for a duration of 2-7s, pausing for 0.5-5s, then introducing N2 for purging for a duration of 1-10s, pausing for 0.5-5s, this is one cycle, and the cycle is performed continuously for 20-70 times;
[0028] Step S5, purging and breaking the vacuum to complete the process.
[0029] The invention firstly introduces O3 gas to remove wet process residues on the surface of the silicon wafer and prepare a SiO2 film. On the one hand, chemical liquid in the wet process penetrates into the bottom of the velvet pyramid, which may not be completely removed by water cleaning itself. The introduction of O3 can effectively clean the wet process residues on the surface of the silicon wafer. O3 has a strong oxidizing effect and is in a gaseous state, so it can effectively oxidize and blow away the chemical components at the bottom of the velvet pyramid. On the other hand, the introduced O3 can react with the silicon wafer to form a SiO2 film of a certain thickness. The film has both the effect of interface passivation and the effect of improving anti-PID.
[0030] After the SiO2 film is prepared, H2O vapor is introduced for a certain period of time and deposited on the surface of the silicon wafer. On the one hand, this allows the SiO2 film to form good contact with the subsequent Al2O3 film, and H+ (hydrogen ions) overflow during sintering, reducing interface recombination and thereby increasing the open circuit voltage. On the other hand, the introduced H2O is deposited on the surface and reacts quickly with the subsequently introduced TMA (usually the amount of TMA introduced for the first time in the ALD process is too much), achieving one cycle and one TMA introduction, forming a dynamic balance with the subsequent alternating introduction of TMA and H2O.
[0031] Before atomic layer deposition, an O3 oxidation step and a H2O passivation compensation step are added to improve the passivation effect. This two-step process directly has a significant effect on improving the battery Eta (conversion efficiency). The process method of the present invention is simple and does not require additional machine costs and labor costs. It only requires the addition of an O3 preparation machine and related pipelines to achieve the above process on an ALD machine. The process principle is simple and easy to promote and use.
[0032] In order to verify the beneficial effects of the present invention, the present invention also carried out actual experiments, and the relevant test contents and results are as follows:
[0033] An atomic layer deposition furnace was used to conduct verification tests on the deposition of Al2O3 films under different processes in a photovoltaic cell workshop. The target Al2O3 film thickness was 4nm (30 cycles), and the process chamber temperature was controlled at 275°C. The test was divided into 4 groups, Group A (no introduction of O3 and H2O, direct ALD deposition), Group B (first introduction of O3, then ALD deposition), Group C (first introduction of H2O, then ALD deposition), and Group D (the solution of the present invention, first introduction of O3 and H2O, then ALD deposition). The electrical performance data are shown in Tables 1 and 2 below:
[0034] Table 1
[0035]
[0036] Note: BSL is the control group, Lifetime is the minority carrier lifetime, the unit is us, Jo is the interface recombination, the unit is A / cm2, iVoc is the simulated open circuit voltage, the unit is V. Full process passivation verification, no printing process.
[0037] Table 2
[0038]
[0039] Note: voc open circuit voltage, unit is V, Isc short circuit current, unit is A, Eta conversion efficiency, unit is %, FF fill factor, unit is %, Rs series resistance, unit is Ω, Rsh parallel resistance, unit is Ω, IRev2 leakage current, unit is A.
[0040] It can be seen from Tables 1 and 2 that (1) after adding H2O and O3 processes, the Lifetime of the cell is significantly increased, J0 is significantly reduced, and iVoc is also significantly improved;
[0041] (2) After adding H2O and O3 processes, the Eta of the battery cell was significantly improved. The efficiency Eta of the O3+H2O process in group D increased by 0.13%, mainly due to the significant improvement in Voc.
[0042] The above description is an explanation of the present invention, not a limitation of the present invention. The present invention may be modified in any form without violating the spirit of the present invention.
Claims
1. A photovoltaic N-type TOPCon cell ALD passivation film manufacturing process, characterized by: The method comprises the following steps: Step S1, placing a substrate processed by a wet process in a process chamber, forming a vacuum constant temperature environment in the process chamber, and the target temperature is 200-300° C.; Step S2, circulating O3 gas into the process chamber for a duration of 30-200 seconds, then passing N2 for purging for a duration of 0-100 seconds, performing 1-5 cycles to remove wet process residues on the surface of the silicon wafer and prepare a SiO2 film; Step S3, introducing H2O vapor into the process chamber for a duration of 5-30 seconds, and then introducing N2 for 0-100 seconds to form a passivation interface by deposition on the SiO2 surface; Step S4, alternately introducing TMA and H2O vapor into the process chamber to grow a highly passivated Al2O3 film; Step S5, purging and breaking the vacuum to complete the process.
2. The photovoltaic N-type TOPCon cell ALD passivation film manufacturing process according to claim 1, characterized in that: The substrate in step S1 is a silicon wafer.
3. The photovoltaic N-type TOPCon cell ALD passivation film manufacturing process according to claim 1, characterized in that: Step S1 further includes: heating the process chamber for 200s, with a target temperature of 200-300°C, and evacuating the process chamber to a low pressure of 0.05-0.3 mTorr, thereby forming a vacuum constant temperature environment in the process chamber.
4. The photovoltaic N-type TOPCon cell ALD passivation film manufacturing process according to claim 1, characterized in that: Step S1 further includes: after a vacuum constant temperature environment is formed in the process chamber, the duration is 200-600 seconds.
5. The photovoltaic N-type TOPCon cell ALD passivation film manufacturing process according to claim 1, characterized in that: Step S4 further includes: a method of alternately introducing TMA and H2O vapor into the process chamber includes first introducing TMA for a duration of 0.5-5s, then introducing N2 for purging for a duration of 1-10s, pausing for 0.5-5s, then introducing H2O for a duration of 2-7s, pausing for 0.5-5s, then introducing N2 for purging for a duration of 1-10s, pausing for 0.5-5s, this is one cycle, and the cycle is performed continuously for 20-70 times.