A method for producing ultra-thin hot-rolled strip steel using a conventional hot rolling mill

By preparing reasonable rolling plans and process systems on conventional hot rolling production lines, the problem of producing extremely thin specification hot rolled strips with thicknesses of 0.8 to 1.2mm was solved, and the stable control of thickness and improvement of market competitiveness were achieved.

CN115301733BActive Publication Date: 2024-12-03ANGANG STEEL CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202211047733.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-30
Publication Date
2024-12-03
Estimated Expiration
2042-08-30

AI Technical Summary

Technical Problem

It is difficult for the prior art to produce extremely thin specification hot-rolled strip steel with a thickness of 0.8 to 1.2 mm on conventional hot-rolled production lines, which exceeds the minimum limit thickness of conventional hot-rolled production lines.

Method used

By preparing a reasonable rolling plan and heating and rolling process system, including rolling and transition material planning arrangement, heating temperature control, rough rolling and finishing rolling speed control, laminar cooling and coiler guide ruler opening setting, Ensure the temperature and shape stability of the slab during the rolling process, and achieve the production of low-carbon steel plates with a thickness of 0.8 to 1.2mm.

Benefits of technology

The product specifications of the hot continuous rolling production line have been successfully expanded, and the stable production of extremely thin strip steel with a thickness of 0.8~1.2mm has been achieved, which avoids the problem of head sleeves and improves the market competitiveness of the products.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a method for producing ultra-thin hot-rolled strip steel by using a conventional hot rolling mill, comprising: 1) arranging a hot roll material and a transition material plan; 2) heating; 3) rough rolling; 4) finishing rolling; 5) laminar cooling; 6) coiling; the present invention utilizes the existing equipment and technical advantages of a conventional hot rolling production line, and produces low-carbon steel plates with a thickness of 0.8 to 1.2 mm by compiling a reasonable rolling plan and heating and rolling process system, thereby broadening the product specifications of the hot rolling production line and providing a technical reserve for the development of ultra-thin strip steel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of strip steel production, and in particular to a method for producing ultra-thin hot-rolled strip steel using a conventional hot rolling mill, so as to enable a conventional hot rolling production line to produce low-carbon steel plates with a thickness range of 0.8 to 1.2 mm (exceeding the minimum limit thickness designed for the production line). Background Art

[0002] Hot rolled products have excellent properties such as high strength, good toughness, easy processing and forming, and good weldability, so they are widely used in manufacturing industries such as ships, automobiles, bridges, buildings, machinery, and pressure vessels. At present, hot rolled strip steel is generally produced by hot rolling technology. Hot rolling uses continuous casting slabs or initial rolling slabs as raw materials. After heating in a walking furnace and dephosphorization with high-pressure water, they enter the rough rolling mill. The rough rolled material is cut and then enters the finishing mill for computer-controlled rolling. After the final rolling, it is cooled by laminar flow (cooling rate is controlled by computer) and coiled by the coiler to become a straight coil.

[0003] Conventional hot rolling production lines have high equipment density and high automation, and can realize flexible production, fully automatic rolling, thin material production and high-quality surface control. The minimum limit thickness of strip steel produced by conventional hot rolling production lines is 1.2 mm. In order to develop ultra-thin specifications (0.8-1.2 mm) products that meet market demand and improve the market competitiveness of products, the present invention has developed a method for producing ultra-thin thickness specifications hot-rolled strip steel using conventional hot rolling production lines.

[0004] The Chinese patent application with publication number CN 107419191 A discloses an "ultra-thin weathering steel and its production method", which is a thin weathering steel with excellent performance produced by conventional hot rolling mills and traditional hot rolling production processes. The chemical composition weight percentage of the weathering steel is: C≤0.12%, Si: 0.25-0.45%, Mn: 0.20-0.45%, P: 0.060-0.090%, S≤0.015%, Cr: 0.30-0.40%, Ni: 0.15-0.20%, Cu: 0.25-0.30%, and the balance is Fe and unavoidable impurities. The production method includes the following steps: hot metal desulfurization → converter smelting → LF refining → slab continuous casting → hot rolling → laminar cooling → coiling → packaging and storage. However, the thickness of the ultra-thin weathering steel produced is 1.5-2.0 mm, which does not exceed the minimum limit thickness of the conventional hot rolling production line. It is not applicable to the ultra-thin hot-rolled strip steel with a thickness of 0.8 to 1.2 mm described in the present invention.

[0005] The Chinese patent application with publication number CN112692056A discloses a "production process for ultra-thin hot-rolled checkered plates with a thickness of less than 1 mm". It uses a conventional hot rolling mill and formulates a special production plan to perform rough rolling and finish rolling on the slabs coming out of the heating furnace. During the rough rolling and finish rolling process, the process system is controlled, and the strip is cooled by head cooling and sparse cooling to roll out ultra-thin checkered plates with a thickness of less than 1.0 mm. It combines laminar cooling technology, that is, sparse cooling combined with head cooling and a sweeping device, to solve the problem of the difficulty of conventional rolling mills in producing thin-gauge checkered plates, and realizes stable batch production of checkered plates with a thickness of less than 1.0 mm. However, this technical solution mainly involves steel for checkered plate series, not conventional hot-rolled steel grades. Due to the pattern on the surface of the checkered plate, it is not easy to deviate during the strip production process, and the rolling difficulty during its production is less than that of strip steel with a smooth surface. Summary of the invention

[0006] The present invention provides a method for producing ultra-thin hot-rolled strip steel by using a conventional hot rolling mill. By utilizing the existing equipment and technical advantages of the conventional hot rolling production line, a reasonable rolling plan and heating and rolling process system are formulated to produce low-carbon steel plates with a thickness of 0.8 to 1.2 mm, thereby broadening the product specifications of the hot rolling production line and providing technical reserves for the development of ultra-thin strip steel.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] A method for producing ultra-thin hot-rolled strip steel using a conventional hot rolling mill comprises the following steps:

[0009] 1) Plan and arrange hot roll materials and transition materials; the strip steel shall be rolled within 45km of rolling mileage, and at least 3 groups of transition materials shall be arranged;

[0010] 2) Heating: The slab out-of-furnace temperature is controlled at 1250-1270°C, the soaking time is controlled at 40-50 minutes, and the total time in the furnace is controlled at 185-230 minutes;

[0011] 3) Rough rolling: the rough rolling outlet temperature is controlled at 1095-1120°C, and the finishing rolling inlet temperature is controlled at 1070-1085°C;

[0012] 4) Finishing rolling; the maximum rolling speed of finishing rolling is 14-17m / s; the reduction rate of the first stand of finishing rolling is controlled within 50%; the finishing rolling threading speed is controlled at 10-11m / s; the guide gauge margin of at least the last three stands is controlled at 40-85mm;

[0013] 5) Laminar cooling: The laminar cooling watering distance is controlled at 100-150m, and the head temperature is controlled at 70-120℃;

[0014] 6) Coiling: The guide gauge opening setting principle of 1# coiler to 3# coiler is: arrange them in an arithmetic sequence from small to large, and the difference of the arithmetic sequence is 30 to 100 mm.

[0015] Furthermore, the thickness of the finished strip steel is 0.8 to 1.2 mm.

[0016] Furthermore, during rough rolling, the rolling mode of the R1 rolling mill and the R2 rolling mill adopts the "N+R" mode, where N represents the rolling pass of the R1 rolling mill, and R represents the rolling pass of the R2 rolling mill; the rolling speeds of the first three passes of the R1 rolling mill are: 2.1-2.5 m / s for the first pass, 2.4-2.8 m / s for the second pass, and 2.4-2.8 m / s for the third pass; the rolling speeds of the first three passes of the R2 rolling mill are: 3.3-3.7 m / s for the first pass, 4.9-5.1 m / s for the second pass, and 4.9-5.1 m / s for the third pass.

[0017] Furthermore, the thickness of the rough-rolled intermediate billet is 35 to 38 mm.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] 1) By utilizing the existing equipment and technical advantages of conventional hot rolling production lines, the production of ultra-thin hot-rolled strip steel (thickness of 0.8 to 1.2 mm, exceeding the minimum limit thickness specification designed for conventional hot rolling production lines) is realized, which broadens the product specifications of the hot rolling production lines and provides technical reserves for the production of ultra-thin strip steel below 1.2 mm on conventional hot rolling production lines.

[0020] 2) By formulating a reasonable rolling plan, the stable shape control of extremely thin strip steel is guaranteed.

[0021] 3) Through the heating and rolling process system, the starting rolling temperature required for ultra-thin specifications is guaranteed, providing a guarantee for the stable rolling of ultra-thin specifications.

[0022] 4) By reasonably controlling the finishing rolling threading speed within the range of 10-11m / s and the laminar cooling head watering distance within the range of 100-150m, the problem of head lifting that is prone to occur in hot-rolled strips with a thickness of less than 1.2mm is well solved. DETAILED DESCRIPTION

[0023] The method of producing ultra-thin hot-rolled strip steel by using a conventional hot rolling mill of the present invention comprises the following steps:

[0024] 1) Plan and arrange hot roll materials and transition materials; the strip steel shall be rolled within 45km of rolling mileage, and at least 3 groups of transition materials shall be arranged;

[0025] 2) Heating: The slab out-of-furnace temperature is controlled at 1250-1270°C, the soaking time is controlled at 40-50 minutes, and the total time in the furnace is controlled at 185-230 minutes;

[0026] 3) Rough rolling: the rough rolling outlet temperature is controlled at 1095-1120°C, and the finishing rolling inlet temperature is controlled at 1070-1085°C;

[0027] 4) Finishing rolling; the maximum rolling speed of finishing rolling is 14-17m / s; the reduction rate of the first stand of finishing rolling is controlled within 50%; the finishing rolling threading speed is controlled at 10-11m / s; the guide gauge margin of at least the last three stands is controlled at 40-85mm;

[0028] 5) Laminar cooling: The laminar cooling watering distance is controlled at 100-150m, and the head temperature is controlled at 70-120℃;

[0029] 6) Coiling: The guide gauge opening setting principle of 1# coiler to 3# coiler is: arrange them in an arithmetic sequence from small to large, and the difference of the arithmetic sequence is 30 to 100 mm.

[0030] Furthermore, the thickness of the finished strip steel is 0.8 to 1.2 mm.

[0031] Furthermore, during rough rolling, the rolling mode of the R1 rolling mill and the R2 rolling mill adopts the "N+R" mode, where N represents the rolling pass of the R1 rolling mill, and R represents the rolling pass of the R2 rolling mill; the rolling speeds of the first three passes of the R1 rolling mill are: 2.1-2.5 m / s for the first pass, 2.4-2.8 m / s for the second pass, and 2.4-2.8 m / s for the third pass; the rolling speeds of the first three passes of the R2 rolling mill are: 3.3-3.7 m / s for the first pass, 4.9-5.1 m / s for the second pass, and 4.9-5.1 m / s for the third pass.

[0032] Furthermore, the thickness of the rough-rolled intermediate billet is 35 to 38 mm.

[0033] The design principle of the method for producing ultra-thin hot-rolled strip steel by using a conventional hot rolling mill described in the present invention is as follows:

[0034] 1. Plan arrangement;

[0035] In order to ensure the stable control of the strip production process, it is necessary to prepare a reasonable plan for hot roll materials and transition materials. At the same time, in order to ensure the stable control of the plate shape, it is necessary to roll when the thermal crown of the roll is stable. Therefore, the strip is arranged to be rolled within 45km of rolling kilometers, and 3 groups of transition materials with a thickness of less than 2.0mm are used. The thickness of the transition materials is 1.65-2.0mm, 1.4-1.6mm, and 1.05-1.35mm respectively.

[0036] 2. Heating;

[0037] Taking into account the large temperature drop in the rough rolling area of ​​conventional rolling mills (generally in the range of 170-200°C), in order to ensure that the finishing rolling has sufficient temperature, the slab temperature out of the heating furnace is required to be controlled within the range of 1250-1270°C, the soaking time is controlled within the range of 40-50 minutes, and the total time in the furnace is controlled within the range of 185-230 minutes.

[0038] 3. Rough rolling;

[0039] (1) During rough rolling, the rolling mode of R1 and R2 mills adopts the "N+R" mode, where N represents the required rolling passes of R1 mill and R represents the required rolling passes of R2 mill. Considering the large temperature drop in the rough rolling area, in order to ensure the start rolling temperature of finishing rolling, the rolling speed of each rough rolling pass needs to be increased, as shown in Table 1.

[0040] Table 1 Rough rolling speed

[0041] Rolling Mill First pass, m / s Second pass, m / s The third pass, m / s R1 2.1~2.5 2.4~2.8 2.4~2.8 R2 3.3~3.7 4.9~5.1 4.9~5.1

[0042] (2) When producing ultra-thin strip steel, the temperature control in the rough rolling area is mainly to reduce the regional temperature drop, specifically to control the outlet temperature of the rough rolling R2 to ensure the start temperature of the finishing rolling. The present invention controls the outlet temperature of the R2 rolling mill within the range of 1095-1120°C and the inlet temperature of the finishing rolling within the range of 1070-1085°C.

[0043] (3) The thickness of the rough rolling intermediate billet is controlled within the range of 35 to 38 mm.

[0044] 4. Finish rolling;

[0045] (1) To ensure the final rolling temperature, the maximum rolling speed is 14-17 m / s, and the first and second accelerations of the finishing rolling speed are 0.05-0.12 m / s respectively. 2 , 0.015~0.25m / s 2 At the same time, the reduction rate of the finishing rolling F1 stand is controlled within 50%.

[0046] (2) To avoid the problem of strip lifting after the strip head leaves the F7 stand, the finishing rolling speed is controlled within the range of 10 to 11 m / s.

[0047] (3) When rolling extremely thin strip steel, if the last stand deviates, it is very easy to scrape the finishing rolling guide and cause a strip break accident. Therefore, the finishing rolling F5~F7 guide gauge excess is controlled within the range of 40~85mm.

[0048] 5. Laminar cooling;

[0049] In order to avoid the accumulation of laminar rollers during the production of extremely thin specifications, the laminar cooling head watering distance is controlled within the range of 100-150m, and the head temperature is controlled within the range of 70-120℃.

[0050] 6. Coil up;

[0051] In order to ensure that the strip head enters the coiler smoothly, the guide opening of the 1# to 3# coilers is arranged in an arithmetic sequence from small to large, and the difference is controlled within the range of 30 to 100 mm.

[0052] The following embodiments are implemented on the premise of the technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following embodiments.

[0053] [Example 1]

[0054] In this embodiment, a conventional 1580 hot rolling production line is used to produce hot rolled steel strip with a thickness of 1.0 mm. The specific process is as follows:

[0055] 1. Plan arrangement;

[0056] The 1.0mm thickness specification is planned to be arranged when the rolling mileage is 40km. Three groups of transition materials with thickness below 2.0mm are used. The thickness of the three groups of transition materials are 1.8mm, 1.5mm and 1.2mm respectively, and 3 pieces are arranged for each thickness specification.

[0057] 2. Heating;

[0058] The temperature of the slab out of the heating furnace is controlled at 1250℃, the soaking time is controlled at 40min, and the total time in the furnace is 190min.

[0059] 3. Rough rolling;

[0060] (1) The rolling mode of the R1 and R2 mills is the “3+3” mode. The rolling speed of each pass of the rough rolling is shown in Table 1.

[0061] Table 1 Rough rolling speed

[0062] Rolling Mill First pass, m / s Second pass, m / s The third pass, m / s R1 2.3 2.6 2.6 R2 3.5 5.1 5.1

[0063] (2) The outlet temperature of R2 rolling mill is controlled at 1110℃, and the inlet temperature of finishing rolling is controlled at 1075℃.

[0064] (3) The thickness of the rough rolling intermediate billet is set to 35 mm.

[0065] 4. Finish rolling;

[0066] (1) The maximum rolling speed is 14 m / s, and the first and second accelerations of the finishing rolling speed are 0.05 m / s respectively2 , 0.015m / s 2 The reduction rate of the finishing rolling F1 stand is 50%.

[0067] (2) The finishing rolling threading speed is set to 10.4 m / s.

[0068] (3) The guide gauge allowances for finishing rolling F5~F7 are 45mm, 60mm, and 60mm respectively.

[0069] 5. Laminar cooling;

[0070] In order to avoid the accumulation of laminar rollers during the production of extremely thin specifications, the laminar cooling head watering distance is 120m and the head temperature is 80℃.

[0071] 6. Coil up;

[0072] The guide gauge opening of the 2# coiler and the 3# coiler is 30mm and 60mm larger than that of the 1# coiler respectively.

[0073] [Example 2]

[0074] In this embodiment, a conventional 1580 hot rolling production line is used to produce hot rolled steel strip with a thickness of 0.85 mm. The specific process is as follows:

[0075] 1. Plan and arrange hot roll materials and transition materials;

[0076] When the 0.85mm thickness strip is arranged to have a rolling mileage of 45km, three groups of transition materials with a thickness of less than 2.0mm are used. The thicknesses of the three groups of transition materials are 1.65mm, 1.4mm, and 1.05mm respectively, and three pieces are arranged for each thickness specification.

[0077] 2. Heating;

[0078] The temperature of the slab out of the heating furnace is controlled at 1265℃, the soaking time is controlled at 45min, and the total time in the furnace is 200min.

[0079] 3. Rough rolling;

[0080] (1) The rolling mode of the R1 and R2 mills is the “1+5” mode. The rolling speed of each pass of the rough rolling is shown in Table 2.

[0081] Table 2 Rough rolling speed

[0082] Rolling Mill First pass, m / s Second pass, m / s The third pass, m / s Fourth pass, m / s The fifth pass, m / s R1 2.35 - - - - R2 3.1 4.0 4.5 5.1 5.1

[0083] (2) The outlet temperature of the R2 rolling mill is controlled at 1120°C, and the inlet temperature of the finishing rolling mill is controlled at 1085°C.

[0084] (3) The thickness of the rough rolling intermediate billet is 35 mm.

[0085] 4. Finish rolling;

[0086] (1) The maximum rolling speed is 16 m / s, and the first and second accelerations of the finishing rolling speed are 0.10 m / s respectively 2 , 0.025m / s 2 The reduction rate of the finishing rolling F1 stand is 48%.

[0087] (2) The finishing rolling speed is set to 10.0 m / s.

[0088] (3) The guide gauge allowances for finishing rolling F5~F7 are 50mm, 75mm, and 75mm respectively.

[0089] 5. Laminar cooling;

[0090] In order to avoid the accumulation of laminar rollers during the production of extremely thin specifications, the laminar cooling head watering distance is 135m and the head temperature is 100℃.

[0091] 6. Coil up;

[0092] The guide gauge opening of the 2# coiler and the 3# coiler is 60mm and 120mm larger than that of the 1# coiler respectively.

[0093] [Example 3]

[0094] In this embodiment, a conventional 1580 hot rolling production line is used to produce a hot-rolled steel strip with a thickness of 1.15 mm. The specific process is as follows:

[0095] 1. Plan arrangement;

[0096] When the 1.15mm thick strip steel is arranged to have a rolling mileage of 35km, three groups of transition materials with a thickness of less than 2.0mm are used. The thicknesses of the three groups of transition materials are 1.8mm, 1.55mm, and 1.35mm respectively, and three pieces are arranged for each thickness specification.

[0097] 2. Heating;

[0098] The temperature of the slab out of the heating furnace is controlled at 1250℃, the soaking time is controlled at 38min, and the total time in the furnace is 185min.

[0099] 3. Rough rolling;

[0100] (1) The rolling mode of the R1 and R2 mills is the “0+5” mode. The rolling speed of each pass of the rough rolling is shown in Table 3.

[0101] Table 3 Rough rolling speed

[0102] Rolling Mill First pass, m / s Second pass, m / s The third pass, m / s Fourth pass, m / s The fifth pass, m / s R1 - - - - - R2 2.35 3.2 4.3 5.1 5.1

[0103] (2) The outlet temperature of the R2 rolling mill is controlled at 1110°C, and the inlet temperature of the finishing rolling mill is controlled at 1070°C.

[0104] (3) The thickness of the rough rolling intermediate billet is set to 38 mm.

[0105] 4. Finish rolling;

[0106] (1) The maximum rolling speed is 14 m / s, and the first and second accelerations of the finishing rolling speed are 0.05 m / s respectively 2 , 0.020m / s 2 The reduction rate of the finishing rolling F1 stand is 50%.

[0107] (2) The finishing rolling threading speed is set to 10.8 m / s.

[0108] (3) The guide gauge allowances for finishing rolling F5~F7 are 45mm, 60mm, and 60mm respectively.

[0109] 5. Laminar cooling;

[0110] In order to avoid the accumulation of laminar rollers during the production of extremely thin specifications, the laminar cooling head watering distance is 100m and the head temperature is 70℃.

[0111] 6. Coil up;

[0112] The guide gauge opening of the 2# coiler and the 3# coiler is 30mm and 60mm larger than that of the 1# coiler respectively.

[0113] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for producing ultra-thin hot-rolled strip steel using a conventional hot rolling mill, It is characterized in that The steps include: 1) Arrangement of hot roll materials and transition materials; the strip steel shall be rolled within 45 km of rolling mileage, and at least 3 groups of transition materials shall be arranged; 2) Heating: The slab out-of-furnace temperature is controlled at 1250-1270°C, the soaking time is controlled at 40-50 minutes, and the total time in the furnace is controlled at 185-230 minutes; 3) Rough rolling: the rough rolling outlet temperature is controlled at 1095-1120°C, and the finishing rolling inlet temperature is controlled at 1070-1085°C; 4) Finishing rolling; the maximum rolling speed of finishing rolling is 14-17m / s; the reduction rate of the first stand of finishing rolling is controlled within 50%; the threading speed of finishing rolling is controlled at 10-11m / s; the guide gauge margin of at least the last three stands is controlled at 40-85mm; 5) Laminar cooling: The laminar cooling allows the head watering distance to be controlled at 100-150m, and the head temperature to be controlled at 70-120℃; 6) Coiling: The guide gauge opening of 1# coiler to 3# coiler is set in the principle of arranging them in an arithmetic sequence from small to large, and the difference of the arithmetic sequence is 30 to 100 mm; The thickness of the finished strip steel is 0.8 to 1.2 mm.

2. A method for producing ultra-thin hot-rolled strip steel using a conventional hot rolling mill according to claim 1, It is characterized in that During rough rolling, the rolling mode of R1 mill and R2 mill adopts "N+R" mode, N represents the rolling pass of R1 mill, and R represents the rolling pass of R2 mill; the rolling speeds of the first three passes of R1 mill are: 2.1-2.5 m / s for the first pass, 2.4-2.8 m / s for the second pass, and 2.4-2.8 m / s for the third pass; the rolling speeds of the first three passes of R2 mill are: 3.3-3.7 m / s for the first pass, 4.9-5.1 m / s for the second pass, and 4.9-5.1 m / s for the third pass.

3. A method for producing ultra-thin hot-rolled strip steel using a conventional hot rolling mill according to claim 1, It is characterized in that The thickness of the rough rolling intermediate billet is 35 to 38 mm.

Citation Information

Patent Citations

  • Extremely-thin specification weathering resistant steel and production method thereof

    CN107419191A

  • Production process of ultrathin hot-rolled checkered plate with thickness of 1 mm or below

    CN112692056A

  • Thin material threading control method for guide rulers of hot rolling coiler

    CN103008359A

  • Method for producing low-strength steel strip with thickness<=2.0mm in CSP production line by speed-up rolling process

    CN106269871A

  • Method for using thin slab continuous casting and rolling technology for producing thin-specification, low-alloy and high-strength steel

    CN106734201A