A new type of protective slag for cold heading steel
By using magnesium chromite and other additives in cold heading steel protection slag, the heat control and lubrication performance is improved, the problems of high viscosity and poor heat control in the existing technology are solved, and low viscosity, high lubricity and stability are achieved The liquid layer effectively prevents longitudinal cracks and slag inclusions, improving the smoothness of continuous casting of cold heading steel and product quality.
Patent Information
- Application Number
- CN202210982640.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-16
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-08-16
AI Technical Summary
The protective slag viscosity of existing cold heading steel is too high, has poor heat control ability and poor lubrication effect, which leads to the problem of longitudinal cracks and slag inclusion on the surface of the casting billet.
Magnesium chromite is used as the raw material for protecting slag, which increases the content of Cr3+ and Mn2+, increases the surface tension, reduces infrared thermal radiation capacity, combines reducing bauxite, increases the content of borax and fluorite, reduces sodium carbonate in an appropriate amount, and improves the interface stability of steel slag , adjust the protective slag composition to improve heat control and lubrication performance.
It realizes the formation of liquid layers with low viscosity, high lubricity and stable, effectively prevents longitudinal cracks, reduces the slag inclusion rate on the surface of the casting billet, and improves the smoothness of cold-heading steel continuous casting and product quality.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to a novel cold heading steel protection slag, belonging to the field of steel metallurgy continuous casting. Background Art
[0002] Cold heading steel is widely used in the manufacture of high-strength screws, nuts and other fasteners. The carbon content of cold heading steel is between 0.39 and 0.42%, which belongs to medium carbon steel. Its solid-liquid phase region is about 1441~1495℃. According to the iron-carbon phase diagram, cold heading steel will undergo peritectic reaction (L+δ→γ) at 1479~1495℃; due to the high Cr content in cold heading steel, Cr and Fe will form a continuous solid solution, and the mutual substitution of Cr and Fe reduces the stability of austenite, thereby reducing the austenite phase region. In addition, due to the characteristics of the steel grade, medium and high carbon steels are in close contact with the wall of the crystallizer, and it is easy for the copper mold to bond with the solidified billet shell. Therefore, large longitudinal cracks often occur in the production of cold heading steel, and the cracks are often accompanied by protective slag. Protective slag plays a vital role in the continuous casting process, and its physical and chemical properties are closely related to the quality of the ingot. When the viscosity of the mold slag is too high, the amount of mold slag flowing into the mold and the solidified shell is reduced, which leads to a thin liquid slag layer, so that the ingot cannot be fully lubricated, resulting in disordered and distorted vibration marks and subcutaneous cracks. In order to solve the problems of thin primary shell at the meniscus of the mold, low high-temperature plasticity and strength at high temperature, low heat flow in the mold, and poor lubrication of the mold slag, an improved mold slag is needed.
[0003] The application publication number CN114101614A discloses a crystallizer protective slag for cold heading steel continuous casting and its preparation method. The invention aims at the quality defects such as corner chipping and non-metallic inclusions on the surface of the ingot that are prone to occur in the continuous casting process of cold heading steel. It reduces the Na element in the non-metallic inclusions that are prone to slag rolling, and at the same time increases the viscosity of the protective slag to ensure a sufficient liquid slag layer, enhance the lubrication effect and thus reduce slag rolling. The basicity of the protective slag of the invention is 0.65~1.05, the viscosity at 1300℃ is 1.16~1.45Pa·s, and the melting point is 1150~1178℃. The continuous casting protective slag in this melting point range cannot fill the gap between the solidified ingot shell and the crystallizer, resulting in poor lubrication effect, and the problem of longitudinal crack defects on the surface of the ingot is not well solved. There may also be a risk of bonding and steel leakage.
[0004] The application publication number CN109550912B discloses a low-reactivity protective slag for aluminum-containing medium-carbon steel; the invention selects a protective slag with low reactivity and more stable slag properties to solve the problem of slag-steel reaction from the source; the protective slag BaO / Al 2 O 3The ratio is controlled within 1.2~1.8, the viscosity at 1300℃ is 0.05~0.12Pa·s, and the melting point is 1140~1200℃. Although the protective slag ensures the lubrication effect of the slag on the casting, the BaO-Al 2 O 3 The crystallization performance of the protective slag is relatively weak, and the heat control effect is poor. For medium carbon steel such as cold heading steel, when undergoing the peritectic phase transformation from δ-Fe to γ-Fe, the mismatch of thermal shrinkage coefficient will cause additional stress on the initial solidified shell, resulting in phase transformation shrinkage and thus cracks.
[0005] Cr is rarely added to industrial mold slag. Related studies have shown that Cr (Cr 2 O 3 ) As a transition metal oxide, it can increase the radiation absorption coefficient of the slag film, reduce the thermal radiation capacity of infrared rays, and improve the heat control capacity of the protective slag. The total heat transfer rate decreases with the increase of Cr. 2 O 3 For cold heading steel protection slag, it just fills the defect of poor heat control effect. my country has abundant reserves of magnesia-chromite, wide sources, easy to obtain and low price. Adding magnesia-chromite to the protection slag can simultaneously increase the electrostatic potential of the cationic Cr 3+ and Mg 2+ The content of MgO increases the surface tension of the protective slag, thereby solving the problem of too low interfacial tension between the original cold heading steel and its continuous casting protective slag, and effectively reducing slag inclusion on the surface of the ingot.
[0006] In addition to adding an appropriate amount of magnesia-chromite as a major innovation, the present invention also makes overall adjustments to the performance of the protective slag: it is planned to increase the basicity of the protective slag to increase the crystallization rate, reduce bauxite, increase borax and fluorite content to reduce the melting point and viscosity, and reduce sodium carbonate in an appropriate amount to improve the interface stability of the slag. The above adjustments are combined to achieve comprehensive regulation of the performance of the protective slag. Summary of the invention
[0007] The present invention aims to provide a new type of cold heading steel protective slag in view of the deficiencies of the prior art. In view of the problems of the original cold heading steel protective slag such as too high viscosity, poor heat control ability, and poor lubrication effect, a new type of cold heading steel protective slag is innovatively proposed. The protective slag of the present invention has stable composition and performance. The present invention is the first to try to use an appropriate amount of magnesia-chromite as one of the raw materials for the protective slag, which not only plays a good regulatory role in the heat control performance, but also reduces the cost. The innovative use of magnesia-chromite and pyrolusite as the raw materials for the protective slag improves Cr 3+ and Mn 2+ The content of Cr can increase the radiation absorption coefficient of the slag film, reduce the cut-off wavelength of infrared rays, reduce the thermal radiation capacity of infrared rays, and improve the thermal control capacity of protective slag. 3+ and Mn 2+They are all cations with large electrostatic potential, which can increase the surface tension of the protective slag, which is very beneficial to reducing the slag inclusion rate on the surface of the ingot; based on the original protective slag, the protective slag has increased basicity, reduced the proportion of bauxite, increased the content of borax and fluorite to lower the melting point and viscosity, appropriately reduced sodium carbonate, improved the stability of the slag interface, and ensured the smooth progress of continuous casting.
[0008] To achieve the above object, the technical solution of the present invention is:
[0009] The present invention discloses a novel cold heading steel protection slag, which is composed of the following components in percentage by mass:
[0010] Wollastonite 30%~45%, limestone 5%~12%, bauxite 10%~18%, pyrolusite 1%~6%, fluorite 1%~8%, magnesia 0%~5%, sodium carbonate 4%~13%, borax 1%~6%, carbon powder 9%~20%, magnesia-chromite 1%~4%.
[0011] The preferred addition amount of magnesia-chromite in the present invention is 1.5% to 4%. The protective slag within this range can well improve the ability to control heat transfer under the condition of controlling the crystallization temperature and melting temperature. The magnesia-chromite content should not be too high, otherwise it will lead to an increase in the melting temperature and crystallization temperature, which will reduce the lubrication performance of the protective slag and cause the ingot to be insufficiently lubricated.
[0012] As a preferred embodiment, the present invention provides a novel cold heading steel protection slag, wherein the protection slag is composed of the following components in percentage by mass:
[0013] Wollastonite 30%~43%, limestone 5.50%~12%, bauxite 11%~18%, pyrolusite 1%~5%, fluorite 2%~7%, magnesia 0%~3%, sodium carbonate 4%~12%, borax 1%~5%, carbon powder 10%~20%, magnesia-chromite 1.50%~4%.
[0014] As a further preferred embodiment, the present invention provides a novel cold heading steel protection slag, wherein the protection slag is composed of the following components in percentage by mass:
[0015] Wollastonite 36.38%~42.98%, limestone 8.03%~11.18%, bauxite 12.34%~17.18%, pyrolusite 1.42%~4.78%, fluorite 2.81%~6.88%, magnesia 0.10%~2.16%, sodium carbonate 5.12%~11.33%, borax 1.16%~4.58%, carbon powder 10.33%~16.38%, and magnesia-chromite 1.62%~3.48%.
[0016] As a further preferred embodiment, the present invention provides a novel cold heading steel protection slag, wherein the protection slag is composed of the following components in percentage by mass:
[0017] Wollastonite 38.98%~41.83%, limestone 9.63%~10.28%, bauxite 14.34%~15.68%, pyrolusite 2.12%~3.18%, fluorite 5.81%~6.88%, magnesia 0.10%~0.21%, sodium carbonate 6.02%~9.03%, borax 1.16%~2.58%, carbon powder 11.3%~15.18%, and magnesia-chromite 2.02%~3.18%.
[0018] As a further preferred embodiment, the present invention provides a novel cold heading steel protection slag, wherein the protection slag is composed of the following components in percentage by mass:
[0019] Wollastonite 40.94%, limestone 10.19%, bauxite 14.50%, pyrolusite 2.50%, fluorite 6.64%, magnesia 0.10%, sodium carbonate 6.89%, borax 1.90%, carbon powder 13.30%, and magnesia-chromite 3.03%.
[0020] The content of MgCr2O4 in the magnesium-chromite ore used is 80-98%.
[0021] The invention discloses a novel cold heading steel protective slag, wherein the melting temperature of the protective slag is between 1027°C and 1131°C.
[0022] The invention discloses a novel cold heading steel protection slag, wherein the viscosity of the protection slag is 0.221-0.422 Pa•s at 1300°C.
[0023] The invention discloses a novel cold heading steel protection slag, wherein the wetting angle of the protection slag is 36.62°-45.6°.
[0024] The invention discloses a novel cold heading steel protective slag, wherein the protective slag is composed of the following components in percentage by mass: 40.94% wollastonite, 10.19% limestone, 14.50% bauxite, 2.50% pyrolusite, 6.64% fluorite, 0.10% magnesia, 6.89% sodium carbonate, 1.90% borax, 13.30% carbon powder and 3.03% magnesia-chromite.
[0025] When the content of MgCr2O4 in the magnesia-chromite is 84-86%, the melting temperature of the protective slag is between 1123-1125°C; the viscosity of the protective slag is 0.37-0.38 Pa•s at 1300°C; and the wetting angle of the protective slag is 45.4°-45.6°.
[0026] The invention discloses an application of a novel cold heading steel protection slag, wherein the protection slag is used for continuous casting of cold heading steel; in the cold heading steel, the content of Mn is 0.50wt%-0.88wt%, the content of Cr is 0.90wt%-1.28wt%, and the content of aluminum is 0.01wt%-0.6wt%.
[0027] In the present invention, the continuous casting of cold heading steel includes continuous casting using existing technology.
[0028] The present invention uses traditional wollastonite and limestone as the main base materials of the protective slag, which is a traditional CaO-SiO 2 It is a protective slag with good chemical composition stability.
[0029] In the present invention, borax and fluorite are used as additives of protective slag and have the function of controlling the melting temperature.
[0030] In the present invention, magnesia chromite and pyrolusite are used as colorants to reduce radiation heat transfer. At the same time, magnesia chromite can also increase the electrostatic potential of cations Cr 3+ and Mg 2+ The content of can increase the surface tension of the protective slag, thereby improving the surface quality of the casting and reducing defects such as dents and cracks.
[0031] In the present invention, C serves as a skeleton and can adjust the melting speed of the protective slag. In the present invention, the carbon powder content is controlled within the range of 13-20%.
[0032] Advantages of the present invention:
[0033] 1) The cold heading steel protection slag innovatively selects magnesium chromite as the protection slag raw material for the first time. 2 O 3 The radiation absorption coefficient of the slag film is improved, and the heat control ability of the protective slag is improved, which solves the problem of slag inclusion on the surface of the ingot caused by the small wetting angle and poor heat control effect of the original cold heading steel protective slag. It not only plays a good regulatory role in the heat control performance, but also reduces the cost. Magnesium chromite can simultaneously increase the electrostatic potential of the cationic Cr 3+ and Mg 2+ The content of can improve the surface tension of the protective slag, improve the surface quality of the ingot, and reduce defects such as dents and cracks. The invention has obvious advantages and broad application prospects, and can provide reliable academic and theoretical support for academic research and production practice. 2) The cold heading steel protective slag belongs to the traditional CaO-SiO 2 It is a protective slag with no slag-steel reaction. Compared with the traditional cold heading steel protective slag, it has high component stability, solves the problem of uneven slag penetration, has stable physical and chemical properties, and stable ingot quality. It can provide reliable and stable academic and theoretical support for academic research and production practice. In particular, it provides the necessary conditions for continuous industrial application.
[0034] 3) The cold heading steel protective slag has a low melting point and viscosity, and can form a stable liquid layer, which can lubricate the ingot very well, control heat, and ensure the smooth progress of continuous casting.
[0035] In summary, the present invention is the first to try to use an appropriate amount of magnesium-chromite as one of the raw materials for protective slag, which plays a good role in regulating thermal performance and reduces costs. 3+ and Mn 2+ The content of slag can be increased to improve the radiation absorption coefficient of the slag film and reduce the thermal radiation capacity of infrared rays, thereby achieving the purpose of improving the heat control ability of the protective slag. In addition, the content of bauxite is reduced, and the content of borax and fluorite is increased to reduce the melting point and viscosity, and the sodium carbonate is appropriately reduced to improve the stability of the steel slag interface and inhibit slag rolling. The new cold heading steel protective slag has good lubricity and can control heat transfer well, ensuring the smooth continuous casting process of cold heading steel, and can effectively prevent the occurrence of longitudinal cracks, with good social and economic benefits. DETAILED DESCRIPTION
[0036] The present invention is further described below in conjunction with the examples, which are only used to illustrate the present invention and are not intended to limit the present invention in any form.
[0037] The melting temperature and viscosity at 1300°C of the protective slag of the present invention are measured by metallurgical industry standards YB / T186 and YB / T185, respectively. The crystallization temperature is measured by the hot wire method commonly used in the industry. During the test, the protective slag raw materials are first weighed and mixed according to the target composition, and then melted in a medium frequency induction furnace to make the composition uniform. The molten slag is then poured into water and quenched to obtain a glassy protective slag block. Finally, the block protective slag is ground into powder and subjected to a hot wire experiment. In the process of measuring the crystallization temperature of the protective slag by the hot wire method, the thermocouple carrying the protective slag is first heated to 1500°C, and then cooled at a cooling rate of 30°C / s after keeping warm for 3 minutes. The time for crystal precipitation in the protective slag is observed and recorded by a camera connected to an optical microscope, and then the protective slag temperature collected by the computer is searched according to the time, so as to accurately obtain the crystallization temperature of the protective slag.
[0038] Preparation process: 1) Use industrial raw materials such as limestone, wollastonite, bauxite, fluorite, etc. to weigh the content of the above-mentioned protective slag components; mix the weighed raw materials and stir them mechanically to make the components evenly mixed; 2) Pour the mixed sample into a graphite crucible and put them into a medium frequency induction furnace for heating and melting, and keep warm for a period of time to remove volatiles and uniform slag components; 3) Pour the molten slag into water and quench to obtain a glassy sample; 4) After the glassy sample is crushed, add the required amount of carbonaceous material and cellulose binder to make a slurry; 5) Send the obtained slurry into a spray particle drying tower for drying and granulation. The product requires moisture content less than 0.5% and particle size in the range of 0.01~2mm, and seal it in bags for use.
[0039] The proportion of magnesia-chromite components in the protective slag is shown in Table 1, and the main physical properties of the protective slag are shown in Table 1.
[0040] In the embodiments and comparative examples, the magnesia-chromite has the following components in mass percentage: the content of MgCr2O4 in the magnesia-chromite used in the embodiments and comparative examples is about 85%.
[0041] Ingredients: The ingredients are shown in Table 1.
[0042] Preparation process: Same as Example 1.
[0043] The main physical properties of mold slag are shown in Table 1.
[0044] Table 1 Chemical composition (wt%) and physical properties of mold slags of Examples 1 to 3 and Comparative Examples 1 to 3
[0045]
[0046] It can be seen from Table 1 that the melting temperatures of Examples 1 to 3 are 1124°C, 1052°C, and 1229°C, respectively, and the viscosities at 1300°C are 0.373 Pa•s, 0.241 Pa•s, and 0.472 Pa•s, respectively, and the wetting angles of the protective slag are 45.56°, 43.21°, and 36.62°, respectively.
[0047] Ingredients: The ingredients are shown in Table 1.
[0048] Preparation process: Same as Example 1.
[0049] The main physical properties of mold slag are shown in Table 1.
[0050] Comparative Examples 1 to 3 are general cold heading steel protective slags, wherein the wollastonite content of Comparative Examples 1 to 3 is >44%, and their melting temperatures are 1244°C, 1250°C, and 1280°C, respectively; their viscosities at 1300°C are 0.477 Pa•s, 0.525 Pa•s, and 0.508 Pa•s, respectively; and their wetting angles are 34.21°, 31.24°, and 44.39°, respectively.
[0051] The melting temperatures of Comparative Examples 1 to 3 are too high, resulting in a small slag film thickness, which is not conducive to lubrication of the ingot, and the viscosity is too high, so the ingot is prone to cracks.
[0052] The melting temperature and viscosity of Examples 1 to 3 are lower than those of Comparative Examples 1 to 3, which is conducive to the formation of a liquid slag layer and lubrication of the casting.
[0053] The protective slag of the above embodiment is used for continuous casting of cold heading steel; in the cold heading steel, the content of Mn is 0.60wt%, the content of Cr is 1.10wt%, and the content of aluminum is 0.02wt%. The effects are shown in Table 2:
[0054] Table 2: Slag consumption and slag inclusion rate of Examples 1 to 3 and Comparative Examples 1 to 3
[0055]
[0056] From the perspective of slag inclusion rate, the slag inclusion defect rate of the casting mold slag of Examples 1 to 3 is significantly lower than that of Comparative Examples 1 to 3. Compared with Comparative Examples 1 to 3, Examples 1 to 3 have improved the stability of the steel slag interface, strong ability to inhibit slag rolling, and good lubrication performance, and can well control heat transfer, ensure the smooth progress of the cold heading steel continuous casting process, and effectively prevent the generation of longitudinal cracks. From the perspective of raw material cost, since the slag consumption of Examples 1 to 3 is less than that of Comparative Examples 1 to 3, the mold slag cost is reduced to a certain extent.
Claims
1. A new type of cold heading steel protection slag, characterized by: The protective slag is composed of the following components in percentage by mass: Wollastonite 30%~43%, limestone 5.50%~12%, bauxite 11%~18%, pyrolusite 1%~5%, fluorite 2%~7%, magnesia 0%~3%, sodium carbonate 4%~12%, borax 1%~5%, carbon powder 10%~20%, magnesia chromite 1.50%~4%; The viscosity of the protective slag at 1300° C. is 0.221-0.422 Pa•s; The wetting angle of the protective slag is 36.62°~45.6°.
2. The protective slag according to claim 1, characterized in that: The protective slag is composed of the following components in percentage by mass: Wollastonite 36.38%~42.98%, limestone 8.03%~11.18%, bauxite 12.34%~17.18%, pyrolusite 1.42%~4.78%, fluorite 2.81%~6.88%, magnesia 0.10%~2.16%, sodium carbonate 5.12%~11.33%, borax 1.16%~4.58%, carbon powder 10.33%~16.38%, and magnesia-chromite 1.62%~3.48%.
3. The protective slag according to claim 2, characterized in that: The protective slag is composed of the following components in percentage by mass: Wollastonite 38.98%~41.83%, limestone 9.63%~10.28%, bauxite 14.34%~15.68%, pyrolusite 2.12%~3.18%, fluorite 5.81%~6.88%, magnesia 0.10%~0.21%, sodium carbonate 6.02%~9.03%, borax 1.16%~2.58%, carbon powder 11.3%~15.18%, and magnesia-chromite 2.02%~3.18%.
4. The protective slag according to claim 3, characterized in that: The protective slag is composed of the following components in percentage by mass: Wollastonite 40.94%, limestone 10.19%, bauxite 14.50%, pyrolusite 2.50%, fluorite 6.64%, magnesia 0.10%, sodium carbonate 6.89%, borax 1.90%, carbon powder 13.30%, and magnesia-chromite 3.03%.
5. The protective slag according to claim 4, characterized in that: When the content of MgCr2O4 in the magnesia-chromite is 84-86%, the melting temperature of the protective slag is between 1123-1125°C; The viscosity of the protective slag at 1300° C. is 0.37-0.38 Pa•s; The wetting angle of the protective slag is 45.4°~45.6°.
6. An application of the novel cold heading steel protection slag as claimed in any one of claims 1 to 5, characterized in that: The protective slag is used for continuous casting of cold heading steel; in the cold heading steel, the content of Mn is 0.50wt%~0.88wt%, the content of Cr is 0.90wt%~1.28wt%, and the content of aluminum is 0.01wt%~0.6wt%.