A Co3Fe7 alloy / C composite CDI active material and its preparation and application in ion electrosorption

Through the non-hydrothermal oxidation-reduction preparation method of Co3Fe7 alloy/C composite materials, the stability and dispersion problems of cobalt-iron alloy materials in CDI are solved, and efficient electrosorption performance is achieved, which is suitable for industrial wastewater treatment.

CN115312741BActive Publication Date: 2024-10-15CENT SOUTH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211076360.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-05
Publication Date
2024-10-15
Estimated Expiration
2042-09-05

AI Technical Summary

Technical Problem

Existing cobalt-iron alloy materials have ion dissolution and stability problems in electrochemical desalination and electrosorption (CDI), which are difficult to meet the requirements of industrial applications. The preparation process is complex and the product dispersion is not ideal, which affects the adsorption capacity and cycle stability.

Method used

Co3Fe7 alloy/C composite material is used, and through a non-hydrothermal oxidation-reduction preparation method of low-temperature pretreatment and organic carbon source roasting, Co3Fe7 alloy particles with spherical morphology and ultra-fine grains are formed to improve the dispersion and adsorption performance of the material.

Benefits of technology

It significantly improves CDI electrosorption stability and capacity, reduces metal ion dissolution, and enhances the material's cycle performance. It reaches an industry-leading adsorption capacity of 72mg/g and a stability of 109%, making it suitable for industrial wastewater purification treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115312741B_ABST
    Figure CN115312741B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of wastewater electrosorption, and specifically relates to a Co3Fe7 alloy / C composite CDI active material, including a carbon material, and spherical Co3Fe7 alloy particles uniformly dispersed and coated in the carbon material, wherein the particle size of the spherical Co3Fe7 alloy particles is less than or equal to 10 nm. The present invention also provides the preparation of the material and its application in CDI electrosorption. The present invention provides a new material with a spherical morphology and high dispersion and ultrafine crystal cell particle size. Studies have found that when the material with the structure and morphology is applied to CDI ion adsorption, it can unexpectedly and significantly improve the CDI electrosorption stability and improve the CDI electrosorption capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of wastewater treatment, and specifically relates to the technical field of electric adsorption active materials. Background Art

[0002] Electrochemical methods have been increasingly used in industrial wastewater treatment. In order to achieve high-capacity removal of pollutants by electrode materials, in addition to traditional carbon-based non-Faraday electrode materials, a variety of Faraday electrode materials have been developed. This material stores ions through reversible redox reactions and has superior ion adsorption capacity compared to traditional electrostatic storage. Therefore, Faraday electrode materials have received widespread attention. Cobalt metal is considered to be one of the best anode choices in the field of electrochemistry due to its high specific capacity and abundance. For example, the theoretical specific capacity of Co3O4 is as high as 890mAh·g -1 , which is more than twice that of commercial graphite electrodes, which means that large-capacity adsorption of pollutants in the electrochemical field can be achieved. However, the significant ion dissolution problem in long-term cycles remains a challenge for the application of this system in aquatic environments. Actual research has found that cobalt-based materials can achieve significant ion dissolution in the electrochemical field, causing secondary pollution to the water environment. To achieve application in aquatic environments, it is crucial to improve the stability of cobalt electrode materials.

[0003] In order to improve the stability of cobalt-based electrode materials, a variety of methods have been used. These include surface coating methods, such as sol-gel coating and carbon coating; in addition, there is also microstructural regulation of cobalt, adjusting cobalt to a stable crystal phase, such as the (220) crystal plane. But even so, the electrochemical stability is still poor under long electric field cycles. Existing studies have shown that high-efficiency multifunctional electrodes based on bimetallic materials are very ideal, and using multi-component regulation to increase the stability of the original electrode is an effective method with high research value and broad application prospects. However, there is still the problem of multi-component phase separation.

[0004] Cobalt-iron alloy materials have excellent saturation magnetization and catalytic activity similar to that of precious metals. They are widely used in electromagnetic wave absorption and electrocatalysis, but cobalt-iron alloy materials are still a blank in the industry in terms of CDI adsorption. In addition, the preparation of common cobalt-iron alloy materials is relatively complicated, and due to certain lattice differences between metals, it is a great challenge to directly replace cobalt atoms with other metal atoms instead of physically depositing them on the surface of cobalt. For example, the existing Co3Fe7 alloy material is mainly synthesized by hydrothermal reaction to synthesize iron-cobalt oxide, and then reduced to obtain the material of the required phase. The products of the existing preparation principles and methods are mainly cubic phases, and are prone to Austenitic nano-welding and large grain size. Not only that, they are also prone to agglomeration and have unsatisfactory dispersion. Such materials are difficult to adapt to the requirements of CDI use, affecting the CDI electrical adsorption capacity and cycle stability. Summary of the invention

[0005] The first object of the present invention is to provide a Co3Fe7 alloy / C composite CDI active material, aiming to provide a new material with excellent CDI adsorption capacity and adsorption stability.

[0006] The second object of the present invention is to provide a method for preparing the Co3Fe7 alloy / C composite CDI active material and its application in ion electrosorption.

[0007] The third object of the present invention is to provide the Co3Fe7 alloy / C composite CDI active material and its application in electrosorption.

[0008] The fourth object of the present invention is to provide a CDI electrode material, a CDI electrode and a method for using the same for electrosorption, comprising the Co3Fe7 alloy / C composite CDI active material.

[0009] A Co3Fe7 alloy / C composite CDI active material comprises a carbon material and spherical Co3Fe7 alloy particles uniformly dispersed and / or coated in the carbon material, wherein the particle size of the spherical Co3Fe7 alloy particles is less than or equal to 10 nm.

[0010] The present invention provides a new material with a spherical morphology and high dispersion and ultrafine grain size. Studies have found that when the material with the structure and morphology is applied to CDI ion adsorption, it can unexpectedly significantly improve the CDI electrical adsorption stability and improve the CDI electrical adsorption capacity.

[0011] In the present invention, the spherical morphology, good dispersion and ultrafine grain size are the key to synergistically improving the CDI adsorption capacity and cyclic adsorption performance of the material.

[0012] Preferably, the Co3Fe7 alloy / C composite CDI active material has a carbon material as a substrate, in which spherical Co3Fe7 alloy particles are uniformly dispersed; and / or contains uniformly dispersed active particles, wherein the active particles have a core-shell structure, wherein the shell is a carbon material and the core is the spherical Co3Fe7 alloy particles.

[0013] In the present invention, the spherical Co3Fe7 alloy particles are highly dispersed and have no Austrones nano-welding bonding and agglomeration.

[0014] In the present invention, the spherical Co3Fe7 alloy particles have an ultrafine lattice size. For example, the particle size of the spherical Co3Fe7 alloy particles is 4 to 6 nm, preferably 4 to 5 nm.

[0015] Preferably, in the composite CDI active material, the content of Co3Fe7 alloy is 30-50wt.%.

[0016] The present invention also provides a method for preparing a Co3Fe7 alloy / C composite CDI active material, the steps comprising:

[0017] Step (1):

[0018] Pre-treating a solution containing iron salt, cobalt salt, surfactant and alkali to obtain a pre-treated product: wherein the pre-treatment temperature is 70-95° C.; in the starting solution of the pre-reaction, the molar ratio of Co:Fe element is 1:1.2-2;

[0019] Step (2):

[0020] The pre-treated product is compounded with an organic carbon source, and then calcined at a temperature of 480 to 800° C. to obtain;

[0021] The weight ratio of the organic carbon source to the pretreatment product is 5 to 15:1.

[0022] The existing Co3Fe7 alloy material is mainly synthesized by hydrothermal reaction of iron cobalt oxide, and then reduced to obtain the material of the required phase. The products of the existing preparation principle and method are mainly cubic phase, and are prone to austenitic nano-welding, and the grain size is large. Not only that, it is also easy to agglomerate and the dispersibility is not ideal; such materials are difficult to play a good electrical adsorption capacity and cyclic adsorption performance in CDI. In response to this problem, the present invention innovatively provides a new non-hydrothermal oxidation-reduction preparation principle and idea, which pre-treats iron salts, cobalt salts, surfactants, and alkalis at the low temperature to achieve atomic-level hybrid contact of Fe-Co, and then directly performs subsequent organic carbon source-assisted roasting treatment, and further cooperates with the joint control of the preparation process to achieve synergy, so that the Co3Fe7 alloy particle phase can be synthesized, and nano-welding can be effectively reduced, and the dispersibility and grain size of the alloy particles can be improved, which may unexpectedly avoid the problems of unsatisfactory CDI adsorption performance and unsatisfactory cyclic stability caused by conventional fine-grained materials. In the present invention, based on the combination of the new preparation principles, ideas, processes and parameters, synergy can be achieved, and new materials with spherical morphology, ultrafine grains and high dispersion performance can be unexpectedly prepared. Moreover, the materials prepared by this preparation method have unexpected electrical adsorption capacity and adsorption stability in CDI electrical adsorption.

[0023] In the present invention, low-temperature pretreatment assisted by alkali and surfactant and direct subsequent calcination treatment as well as joint control of pre-reaction and calcination conditions are the key to successfully preparing the highly dispersed, ultrafine grain and spherical morphology materials and improving the CDI adsorption capacity and adsorption stability.

[0024] Preferably, the cobalt source is at least one salt of divalent cobalt and trivalent cobalt, preferably one or more of cobalt chloride, cobalt nitrate and cobalt acetate;

[0025] In the present invention, the iron source is a trivalent iron salt, preferably one or more of ferric chloride, ferric sulfate and ferric nitrate.

[0026] Preferably, the alkali is at least one of alkali metal hydroxide and ammonia water. The alkali metal hydroxide is at least one of sodium hydroxide and potassium hydroxide. The amount of the alkali can be adjusted according to the preparation needs. For example, the weight ratio of the alkali to the cobalt element in the cobalt source is 0.1 to 15:1; more preferably 5 to 10:1.

[0027] Preferably, the surfactant is a water-soluble or alcohol-soluble surfactant, preferably at least one of sodium dodecyl sulfate, hexadecyl trimethyl ammonium bromide, and polyvinyl pyrrolidone. The amount of the surfactant can be adjusted based on the preparation needs, for example, the weight ratio of the surfactant to the cobalt element in the cobalt source is 0.1 to 10:1; preferably 1 to 5:1.

[0028] Preferably, in step (1), the solvent of the solution comprises an alcohol, preferably a C1-C4 mono- or polyol;

[0029] More preferably, the solvent also contains water.

[0030] The present invention has found that further controlling the Co:Fe element molar ratio and temperature in the pretreatment stage, combined with subsequent direct carbon roasting, can help to further synergistically improve phase purity, reduce nano-welding, improve dispersion and grain size, and further improve the CDI adsorption performance of the material.

[0031] Preferably, in the pre-reaction starting solution, the molar ratio of Co:Fe is 1:1.5-2; more preferably 1:1.5-1.8. Studies have found that the preferred ratio is more conducive to the phase purity, reducing nano-welding, improving dispersibility and grains, and improving CDI capacity and cycle stability.

[0032] Preferably, the pre-reaction temperature is 80-90° C. Studies have found that low-temperature pre-reaction at this preferred temperature, followed by subsequent calcination treatment, helps to synergistically improve Co3Fe7 alloy, reduce nano-welding, improve dispersibility and grains, and improve CDI capacity and cycle stability.

[0033] In the present invention, there is no particular requirement for the pre-reaction time. Considering the processing efficiency, the pre-reaction processing time is 6 to 24 hours, and more preferably 18 to 22 hours.

[0034] In the present invention, the pretreated product is directly subjected to carbonization and roasting, which is conducive to preparing a material that meets the use requirements and performance of CDI.

[0035] In the present invention, the pretreatment product and the organic carbon source are compounded and then subjected to a calcination treatment. In the present invention, the pretreatment product and the organic carbon source can be compounded based on an existing method.

[0036] Preferably, the organic carbon source is compounded in the pretreatment product by solid phase compounding, liquid phase compounding or in situ polymerization. The solid phase compounding is, for example, directly mixing the pretreatment product and the organic carbon source solid. The liquid phase compounding is, for example, dispersing the pretreatment product in a solution in which the organic carbon source is dissolved, followed by solid-liquid separation. The in situ polymerization refers to in situ polymerization of the polymerizable carbon source on the pretreatment product under necessary polymerization conditions.

[0037] Preferably, the small molecule carbon source is a viscous carbon source and / or a polymerizable carbon source, such as at least one of glucose, citric acid, and dopamine;

[0038] Preferably, the weight ratio of the organic carbon source to the pretreatment product is 5 to 10: 1. Under the preferred conditions, it is helpful to further synergistically improve the performance of the prepared material.

[0039] In the present invention, the calcination stage is carried out under a protective atmosphere;

[0040] Preferably, the temperature of the calcination stage is 500-650°C, most preferably 500-550°C; studies have found that at the preferred calcination temperature, it helps to further improve the phase purity of the Co3Fe7 alloy, reduce nano-welding, improve dispersibility and grain size, and improve CDI adsorption capacity and stability.

[0041] Preferably, the calcination temperature is 2 to 4 hours.

[0042] The present invention also provides an application of the Co3Fe7 alloy / C composite CDI active material, which is used as a CDI active material for electrical adsorption of ions;

[0043] Preferably, the ion is an anion, more preferably Cl - 、SO4 2- 、NO3 - At least one of .

[0044] The present invention also provides a CDI electrode material, comprising an active material, a binder and a conductive agent, wherein the active material comprises the Co3Fe7 alloy / C composite CDI active material.

[0045] In the present invention, the binder and the conductive agent may be components known in the field of CDI electrodes, for example, the binder may be at least one of PVDF and CMC. The conductive agent may be conductive carbon black, for example.

[0046] In the present invention, the contents of the binder and the conductive agent can be adjusted as required. For example, in the CDI electrode material, the contents of the binder and the conductive agent are 5 to 15 wt. %, respectively.

[0047] The present invention also provides a CDI electrode, comprising an electrode plate and the CDI electrode material compounded on the surface of the electrode plate.

[0048] The present invention also provides a CDI adsorption method for ions in an aqueous solution, using the CDI electrode to electrically adsorb ions in the aqueous solution;

[0049] Preferably, the ions in the aqueous solution are anions, more preferably Cl - 、SO4 2- 、NO3 - At least one of .

[0050] The CDI adsorption method of ions in aqueous solution of the present invention may use the electrode of the CDI active material of the present invention, and other operations and parameters may be known.

[0051] Compared with the prior art, the present invention has the following advantages:

[0052] 1. The present invention provides a new small-particle, highly dispersed spherical Co3Fe7 / carbon composite material, which has excellent CDI electrical adsorption capacity and electrical adsorption stability;

[0053] 2. The present invention provides a new preparation principle and idea of ​​non-hydrothermal oxidation-reduction, which is pre-treated at low temperature with the assistance of alkali and surfactant, and then the Co3Fe7 phase and carbon structure are synchronously constructed with the carbon source at the said temperature, which is beneficial to improve the phase purity, dispersion degree and grain size of the product, and is beneficial to obtain materials with new structures and morphologies. The present invention successfully constructs small-particle, highly dispersed Co3Fe7 / C alloy nanomaterials, reduces metal ion dissolution, reduces phase separation, and ultimately improves the CDI adsorption stability of the obtained material.

[0054] For example, in the present invention, the stability level can reach 109%, and the electrical adsorption capacity can reach 72 mg / g, reaching the leading level in the industry and being suitable for industrial wastewater purification. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] Figure 1TEM image of the Co3Fe7 / C alloy nanomaterial prepared in Example 1;

[0056] Figure 2 SAED diagram of the Co3Fe7 / C alloy nanomaterial prepared in Example 1;

[0057] Figure 3 The XRD pattern of the Co3Fe7 / C alloy nanomaterial in Example 1;

[0058] Figure 4 The Co3Fe7 / C alloy nanomaterial prepared in Example 1 is - Conduct electrochemical adsorption performance diagram;

[0059] Figure 5 The Co3Fe7 / C alloy nanomaterial prepared in Example 1 is - Conduct electrochemical cycling performance graphs;

[0060] Figure 6 This is the XRD pattern of the material prepared in Comparative Example 2. DETAILED DESCRIPTION

[0061] The present invention also provides an application of a small-particle-size, highly dispersed Co3Fe7 / C alloy nanomaterial as an electrode material, which is used on an electrode of a capacitive deionization device. The capacitive deionization device is used to perform an electrosorption treatment on a salt solution with an initial concentration of 50-300 mg / L; wherein the applied voltage of the capacitive deionization device is 0-1.2V.

[0062] Specifically, as an optional solution, the small-particle, highly dispersed Co3Fe7 / C alloy nanomaterial, polyvinylidene fluoride and carbon black can be mixed in a mass ratio of 8:1:1, N-methylpyrrolidone can be added, ground into slurry and then applied to a titanium plate for use in a capacitive deionization device.

[0063] CDI electrode preparation and electrosorption:

[0064] The Co3Fe7 / C alloy nanomaterial described in the present invention is formed by attaching the active material Co3Fe7 / C alloy nanomaterial obtained in each case to a titanium plate. The preparation steps are, for example: 80wt% Co3Fe7 / C alloy nanomaterial, 10wt% conductive carbon black, 10wt% polyvinylidene fluoride binder, then adding a certain amount of N-methylpyrrolidone and continuing to grind until a uniform black slurry is formed and mixed to obtain a uniform slurry; then, the solid slurry is evenly coated on the titanium plate, dried overnight at 60°C, and a CDI electrode is obtained. The preparation method of the cobalt-iron hybrid material electrode is similar to that of the Co3Fe7 / C alloy nanomaterial electrode, the difference being that the Co3Fe7 / C alloy nanomaterial is used as the active material, and the content of the active material in the electrode is the same.

[0065] The high-stability CDI module described in the present invention comprises: two acrylic electrode fixing plates, two groups of silica gel plates, anion and cation exchange membranes, and two titanium plates, which are sealed and fixed to each other at the edges using sealing materials; two oppositely arranged electrode fixing plates with a plane electrode between them, and two electrodes are located between the two electrode fixing plates, wherein one electrode is a Co3Fe7 / C alloy nanomaterial electrode, and the other electrode is an activated carbon electrode.

[0066] The applied voltage of the capacitive deionization device was set to 1.2 V, and a 100-h cyclic electrochemical experiment was performed. The solution was driven through the electrodes by a peristaltic pump at a flow rate of 10 mL / min. - The initial solution concentration was 500 mg / L, and the change in ion concentration was detected using a conductivity meter.

[0067] In the present invention, the cycle stability, unless otherwise stated, refers to the percentage of the adsorption capacity after 100 cycles compared to the initial adsorption capacity.

[0068] Example 1

[0069] A method for preparing large and small particle size and highly dispersed Co3Fe7 / C alloy nanomaterials for achieving high performance of electrode materials

[0070] Step 1: Weigh cobalt nitrate hexahydrate (9.6 mmol) and ferric nitrate nonahydrate (Co / Fe molar ratio of 2:3) and place them in a 500 mL beaker, add 300 mL of ethanol, and stir magnetically to completely dissolve the cobalt salt and iron salt powders; measure saturated ammonia water (21 mL, the weight ratio of ammonia to cobalt element is 8.4:1) and place it in a beaker, and add 1.58 g of PVP to the solution to form a uniform solution, react at 80°C for 20 hours;

[0071] Step 2: Cool the reaction sample prepared above to room temperature, wash it with anhydrous ethanol and deionized water, and then dry it at 60° C. to obtain a cobalt-iron hybrid material;

[0072] Step 3: The material prepared in step 2 was dispersed in 80 mL of 10 mM Tris solution with a dopamine concentration of 33% (wherein the weight ratio of dopamine to cobalt-iron hybrid material was 10:1), magnetically stirred for 24 hours, washed and dried, and carbonized at 500 ° C for 2 hours in an Ar atmosphere. The obtained black powder was the small-particle, highly dispersed alloy nanomaterial. It was named Co3Fe7 / C alloy nanomaterial. TEM, SAED and XRD patterns are shown in Figure 1. Figure 1 to Figure 3 As can be seen from the accompanying drawings, the preparation method can prepare a carbon composite alloy material with a spherical shape, a small particle size (average size is 4.81 nm), and high dispersion, and its physical phase purity is high.

[0073] The CDI results are shown in Figure 4 ,pass Figure 4 It can be seen that the prepared material has a strong affinity for Cl - The electrical adsorption capacity can reach 73 mg / g.

[0074] The obtained material was subjected to CDI adsorption cycle treatment, and the figure of 100 cycles is shown in Figure 5 ,pass Figure 5 It can be seen that after 100 cycles, the adsorption retention rate can still reach 109%, indicating that the material of the present invention has excellent adsorption-desorption and elution-desorption cycle stability.

[0075] Using the same Cl - The determination method is to mix the sulfate ion (SO4 2- ) replaced the Cl-, and the adsorption capacity of sulfate ions of the material was measured. The results were: the adsorption capacity was 50.5 mg / g; and the stability after 100 cycles was 94%.

[0076] Example 2

[0077] Compared with Example 1, the only difference is that in step 2, the amount of cobalt remains unchanged, and the molar ratio of cobalt to iron is controlled to be: A: 1: 1; B: 2: 1. Other operations and parameters are the same as in Example 1.

[0078] The CDI performance was measured by the method of Example 1. The results showed that - The electrosorption stability and capacity are:

[0079] A: 78%, 52 mg / g;

[0080] B: 69%, 62 mg / g.

[0081] Example 3

[0082] Compared with Example 1, the only difference is that in step 2, the high-temperature carbonization temperatures of step 3 are controlled to be: A: 450°C; B: 650°C. Other operations and parameters are the same as in Example 1.

[0083] The CDI performance was measured by the method of Example 1. The results showed that - The electrosorption stability and capacity are:

[0084] A: 69%, 55mg / g;

[0085] B: 92%, 59 mg / g.

[0086] It can be seen that the target product can be obtained at a calcination temperature above 450°C, but at 500-650°C, an alloy material with lower nano-welding, excellent dispersion performance and fine grains can be obtained, which can show better CDI adsorption capacity and cycle stability.

[0087] Embodiment 4:

[0088] Compared with Example 1, the only difference is that the temperature of the pretreatment reaction is set to 90° C. Thus, the material with the structure described in the present invention is prepared.

[0089] The method of Example 1 was used to prepare 500 mg / L Cl - The CDI performance was measured and the results showed that the CDI adsorption capacity was 60 mg / g and the stability was 93%.

[0090] Comparative Example 1:

[0091] Compared with Example 1, the only difference is that no surfactant (PVP) is added. The ultra-fine size and highly dispersed composite material of the present invention is not obtained.

[0092] Carry out Cl according to the method of Example 1 - The performance of the product was measured, and the final adsorption capacity was 36 mg / g and the stability was 72%.

[0093] Comparative Example 2:

[0094] Compared with Example 1, the only difference is that no alkaline environment is constructed (no ammonia water is added). No product of the target phase is obtained. Figure 6 .

[0095] The Cl- performance was measured according to the method of Example 1, and the final adsorption capacity was 5 mg / g, and the stability was 23%. There was basically no CDI adsorption performance.

[0096] Comparative Example 3:

[0097] Compared with Example 1, the only difference is that the temperature of the pretreatment reaction is set to 60° C. Thus, the material with the structure described in the present invention is prepared.

[0098] The method of Example 1 was used to prepare 500 mg / L Cl - The CDI performance was measured and the adsorption capacity was 35 mg / g. The adsorption performance was poor.

[0099] Comparative Example 4:

[0100] Compared with Example 1, the only difference is that step (3) is omitted and the cobalt-iron hybrid particles obtained in step (2) are directly used as CDI materials.

[0101] The method of Example 1 was used to prepare 500 mg / L Cl - The CDI performance was measured and the adsorption capacity was 21 mg / g. The adsorption performance was poor.

[0102] Comparative Example 5

[0103] Compared with Example 1, the only difference is that the solution of step 1 is placed in a sealed container, heated to 150° C. for hydrothermal treatment for 5 h, then cooled to room temperature, washed with anhydrous ethanol and deionized water, and dried at 60° C. to obtain a precursor;

[0104] The obtained precursor is treated in step 3 to obtain the catalyst; a catalyst with a cubic morphology and large size is obtained.

[0105] The CDI performance was measured using the method of Example 1. The results showed that the adsorption capacity was 56 mg / g and the stability after 100 cycles was 76%.

[0106] Comparative Example 6:

[0107] Compared with Example 1, the only difference is that the mass ratio of the organic carbon source to the cobalt-iron hybrid nanoparticles is 1:1.

[0108] The method of Example 1 was used to prepare 500 mg / L Cl - The CDI performance was measured and the result was: 62 mg / g, stability: 65.3%.

Claims

1. A Co3Fe7 alloy / C composite CDI active material, characterized in that: It comprises a carbon material, and spherical Co3Fe7 alloy particles uniformly dispersed and / or coated in the carbon material, wherein the particle size of the spherical Co3Fe7 alloy particles is less than or equal to 10 nm; In the Co3Fe7 alloy / C composite CDI active material, a carbon material is used as a substrate, in which spherical Co3Fe7 alloy particles are uniformly dispersed; Alternatively, it comprises uniformly dispersed active particles, wherein the active particles have a core-shell structure, wherein the shell is a carbon material and the core is the spherical Co3Fe7 alloy particle; The particle size of the spherical Co3Fe7 alloy particles is 4-6 nm; In the composite CDI active material, the content of Co3Fe7 alloy is 30~50Wt.%.

2. A method for preparing the Co3Fe7 alloy / C composite CDI active material according to claim 1, characterized in that the steps include: Step (1): Pre-treating a solution containing an iron salt, a cobalt salt, a surfactant, and an alkali to obtain a pre-treated product: wherein the pre-treatment temperature is 70-95° C.; in the pre-treated starting solution, the molar ratio of Co:Fe elements is 1:1.2-2; Step (2): The pre-treated product is compounded with an organic carbon source, and then calcined at a temperature of 480-800°C to obtain; The weight ratio of the organic carbon source to the pretreatment product is 5-15:

1.

3. The method for preparing the Co3Fe7 alloy / C composite CDI active material according to claim 2, characterized in that: The cobalt salt is at least one of divalent cobalt and trivalent cobalt.

4. The method for preparing the Co3Fe7 alloy / C composite CDI active material according to claim 2, characterized in that: The iron salt is a trivalent iron salt.

5. The method for preparing the Co3Fe7 alloy / C composite CDI active material according to claim 2, characterized in that: In the pretreated starting solution, the molar ratio of Co:Fe elements is 1:1.5-2.

6. The method for preparing the Co3Fe7 alloy / C composite CDI active material according to claim 2, characterized in that: The base is at least one of alkali metal hydroxide and ammonia water.

7. The method for preparing the Co3Fe7 alloy / C composite CDI active material according to claim 2, characterized in that: The weight ratio of the alkali to the cobalt element in the cobalt salt is 0.1 to 15:

1.

8. The method for preparing the Co3Fe7 alloy / C composite CDI active material according to claim 2, characterized in that: The weight ratio of the alkali to the cobalt element in the cobalt salt is 5 to 10:

1.

9. The method for preparing the Co3Fe7 alloy / C composite CDI active material according to claim 2, characterized in that: The weight ratio of the surfactant to the cobalt element in the cobalt salt is 0.1~10:

1.

10. The method for preparing the Co3Fe7 alloy / C composite CDI active material according to claim 2, characterized in that: The weight ratio of the surfactant to the cobalt element in the cobalt salt is 1-5:

1.

11. The method for preparing the Co3Fe7 alloy / C composite CDI active material according to claim 2, characterized in that: The surfactant is a water-soluble or alcohol-soluble surfactant.

12. The method for preparing the Co3Fe7 alloy / C composite CDI active material according to claim 11, characterized in that: The surfactant is at least one of sodium dodecyl sulfate, hexadecyltrimethylammonium bromide and polyvinyl pyrrolidone.

13. The method for preparing the Co3Fe7 alloy / C composite CDI active material according to claim 11, characterized in that: In step (1), the solvent of the solution contains alcohol.

14. The method for preparing the Co3Fe7 alloy / C composite CDI active material according to claim 13, characterized in that: In step (1), the alcohol is a C1-C4 unit or polyol.

15. The method for preparing the Co3Fe7 alloy / C composite CDI active material according to claim 13, characterized in that: In step (1), the solvent further comprises water.

16. The method for preparing the Co3Fe7 alloy / C composite CDI active material according to claim 2, characterized in that: The pretreatment temperature is 80-90°C.

17. The method for preparing the Co3Fe7 alloy / C composite CDI active material according to claim 2, characterized in that: The pretreatment time is 6 to 24 hours.

18. The method for preparing the Co3Fe7 alloy / C composite CDI active material according to claim 2, characterized in that: The organic carbon source is compounded in the pretreatment product by solid phase compounding, liquid phase compounding or in-situ polymerization.

19. The method for preparing the Co3Fe7 alloy / C composite CDI active material according to claim 18, characterized in that: The organic carbon source is at least one of a high molecular weight polymer and a small molecular weight carbon source.

20. The method for preparing the Co3Fe7 alloy / C composite CDI active material according to claim 19, characterized in that: The small molecule carbon source is a viscous carbon source and / or a polymerizable carbon source.

21. The method for preparing the Co3Fe7 alloy / C composite CDI active material according to claim 20, characterized in that: The small molecule carbon source is at least one of glucose, citric acid and dopamine.

22. The method for preparing the Co3Fe7 alloy / C composite CDI active material according to claim 20, characterized in that: The weight ratio of the organic carbon source to the pretreatment product is 5-10:

1.

23. The method for preparing the Co3Fe7 alloy / C composite CDI active material according to claim 2, characterized in that: The calcination stage is carried out under a protective atmosphere.

24. The method for preparing the Co3Fe7 alloy / C composite CDI active material according to claim 2, characterized in that: The temperature in the calcination stage is 500~650℃.

25. The method for preparing the Co3Fe7 alloy / C composite CDI active material according to claim 2, characterized in that: The temperature in the calcination stage is 500~550℃.

26. The method for preparing the Co3Fe7 alloy / C composite CDI active material according to claim 2, characterized in that: The calcination temperature is 2 to 4 hours.

27. Use of the Co3Fe7 alloy / C composite CDI active material according to claim 1 or the Co3Fe7 alloy / C composite CDI active material prepared by any one of the preparation methods of claims 2 to 26, characterized in that: It is used as CDI active material for the electrical adsorption of ions.

28. The use according to claim 27, characterized in that The ions are anions.

29. The use according to claim 28, characterized in that The ion is Cl - 、SO4 2- 、NO3 - At least one of .

30. A CDI electrode material, comprising an active material, a binder and a conductive agent, characterized in that: The active material comprises the Co3Fe7 alloy / C composite CDI active material according to claim 1 or the Co3Fe7 alloy / C composite CDI active material prepared by any one of the preparation methods of claims 2 to 26.

31. The CDI electrode material according to claim 30, characterized in that In the CDI electrode material, the contents of the binder and the conductive agent are 5-15wt.% respectively.

32. A CDI electrode, characterized in that: It comprises an electrode plate, and the CDI electrode material according to claim 30 or 31 compounded on the surface of the electrode plate.

33. A CDI adsorption method for ions in aqueous solution, characterized in that: The CDI electrode according to claim 32 is used to electro-adsorb ions in an aqueous solution.

34. The CDI adsorption method of ions in aqueous solution according to claim 33, characterized in that: The ions in the aqueous solution are anions.

35. The CDI adsorption method of ions in aqueous solution according to claim 34, characterized in that: The ions in the aqueous solution are Cl - 、SO4 2- 、NO3 - At least one of .