A method for preparing aluminum alloy by low-temperature and high-speed extrusion
By using the method of high-pressure and high-speed flow out of profiles during the aluminum alloy extrusion process, the problem of uneven deformation in the high-strain rate extrusion of aluminum alloy is solved, and the rapid extrusion of low temperature is achieved, which improves production efficiency and saves energy.
Patent Information
- Application Number
- CN202210825550.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-14
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During the high strain rate extrusion process of aluminum alloy, uneven deformation problems such as pitting and cracks are prone to occur on the surface of the profile, resulting in low production efficiency and high energy consumption.
The profile flows out at high speed through high pressure, compensating for the increase of product temperature and achieving rapid low-temperature extrusion. Specific steps include alloy ingots, pretreatment, ingot extrusion, cooling and quenching, etc.
Under the condition of ensuring the temperature of the profile discharge port, the heating temperature of the aluminum rod is reduced, the extrusion speed is increased, the product temperature is compensated, the product temperature is increased, the product is rapidly extruded at low temperature, the production efficiency is improved, and energy saving is saved.
Smart Images

Figure CN115318859B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of aluminum alloy manufacturing, in particular to a method for preparing an aluminum alloy by low-temperature and high-speed extrusion. Background Art
[0002] Aluminum alloy has good thermoplasticity, excellent corrosion resistance, thermal conductivity and ideal processing performance, and is easy to oxidize and color. Therefore, it is widely used in construction, transportation, electronics, electrical heat dissipation, communications and other industries. It is currently the most widely used alloy.
[0003] As material processing develops towards high speed, energy saving and continuity, many aluminum extrusion manufacturers hope to adopt new low temperature rapid extrusion technology in recent years. Usually, the 6063 series aluminum alloy can reach a temperature rise of 32°C in less than 0.5 seconds under high strain rate conditions. It can be extruded at a low temperature (rod temperature is generally 400°C-430°C) at a high speed, and the outlet temperature can reach 500°C; the extrusion speed of solid profiles is between 15m / min-50m / min, and that of hollow profiles is between 10m / min-35m / min. If the extrusion speed is too fast, pitting and cracks will appear on the surface of the product, increasing the unevenness of metal deformation. Summary of the invention
[0004] To solve the above problems, the present invention uses high pressure to make the profile flow out at high speed to compensate for the increase in product temperature, so as to achieve the purpose of low-temperature rapid extrusion; this method is used to achieve rapid deformation of aluminum alloy billets.
[0005] In a first aspect, a method for preparing an aluminum alloy by low temperature and high speed extrusion comprises the following steps:
[0006] S1: Alloy ingot: The aluminum alloy raw material is cast into an ingot and refined to form a blank to be extruded;
[0007] S2: Pretreatment: Heat the billet to be extruded in S1 to 425°C to 450°C, and heat the extrusion die to 380°C to 450°C;
[0008] S3: Ingot extrusion: the billet to be extruded after S2 pretreatment is placed into the extrusion die after S2 pretreatment for extrusion; the outflow speed of the aluminum alloy profile after extrusion is ≥60m / min;
[0009] S4: Cooling and quenching: The aluminum alloy profiles generated in S3 are subjected to a forced cooling stage and then enter an artificial aging stage.
[0010] In an practicable manner, the pressure of the extrusion die in S3 when extruding the billet to be extruded is about 2000 MPa.
[0011] In an practicable manner, the outflow temperature of the aluminum profile in S3 is controlled to be 620°C-680°C.
[0012] In an practicable manner, the forced cooling stage in S4 uses water cooling treatment so that the cooling rate of the aluminum alloy profile after extrusion reaches 300°C / min.
[0013] In an practicable manner, the artificial aging in S4 is performed at 200° C. and kept warm for 4 hours to 4.5 hours.
[0014] In an operative manner, the Mg2Si precipitated particles in the aluminum alloy profile in S4 are smaller than 0.2 μm.
[0015] In an practicable manner, the extrusion die in S3 is a planar flow-dividing combined die, and the planar flow-dividing combined die has shuttle-shaped holes evenly and symmetrically distributed on a circular die plane.
[0016] Compared with the prior art, the present invention has the following beneficial effects: the present scheme adopts low-temperature rapid extrusion, which means that the extrusion temperature is lower than 450°C and the discharge speed is higher than 60m / min, that is, under the condition that the temperature of the profile outlet reaches the direct air-cooling quenching temperature, the heating temperature of the aluminum rod is reduced as much as possible, and the extrusion speed is increased to compensate for the increase in the product temperature, so as to achieve the purpose of low-temperature rapid extrusion, which not only improves production efficiency but also saves energy. Compared with the ordinary extrusion method, the low-temperature rapid extrusion method has its outstanding advantages: due to the low temperature during extrusion, the heating time of the billet is correspondingly shortened, and the deformation speed is fast, and the billet deformation time is short, which not only saves energy consumption but also greatly improves production efficiency.
[0017] Extrusion temperature has a great impact on product quality, production efficiency, die life, energy consumption, etc. The extrusion metal temperature control speed of the present application is relatively fast, and from the heating of the aluminum rod to the quenching of the extruded profile, it is necessary to ensure that the soluble phase structure does not precipitate from the solid solution or precipitate in the form of small particles. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 It is a schematic plan view of a circular die of an extrusion die; DETAILED DESCRIPTION
[0019] The following specific implementations are provided to further illustrate the present invention. It should be understood that the technical solutions including but not limited to the technical solutions shown in the following specific implementations are only used to illustrate the present invention and are not used to limit the scope of the present invention.
[0020] Embodiment 1
[0021] A method for preparing an aluminum alloy by low-temperature and high-speed extrusion, comprising the following steps:
[0022] S1: Alloy ingot: The aluminum alloy raw material is cast into an ingot and refined to form a blank to be extruded;
[0023] S2: Pretreatment: Heat the billet to be extruded in S1 to 425°C and heat the extrusion die to 380°C;
[0024] S3: Ingot extrusion: the billet to be extruded after the S2 pretreatment is placed into the extrusion die after the S2 pretreatment for extrusion; the outflow speed of the aluminum alloy profile after extrusion is 60m / min, and the outflow temperature of the aluminum alloy profile is 620°C.
[0025] The pressure of the extrusion die when extruding the billet to be extruded is 2000MPa.
[0026] S4: Cooling and quenching: The aluminum alloy profile generated in S3 is subjected to a forced cooling stage, and water cooling treatment is adopted so that the cooling rate of the aluminum alloy profile after extrusion reaches 300°C / min.
[0027] Then it enters the artificial aging stage, using 200℃, keeping temperature for 4 hours, and the Mg in the aluminum alloy profile is finally formed. 2 Si precipitated particles are 0.15 μm.
[0028] In an practicable manner, the extrusion die in S3 is a planar flow-dividing combined die, and the planar flow-dividing combined die has the following features: Figure 1 The shuttle-shaped holes 1 are evenly and symmetrically distributed on the plane of the circular mold.
[0029] The diverter bridge in the plane diverter combination mold adopts a teardrop shape with a width of 15mm; the welding chamber adopts a butterfly-shaped welding chamber. Since the pressure of this application is relatively large, the depth of the welding chamber is 11mm; because high-speed molding is required, the mold core adopts a conical mold core structure. To match the depth of the welding chamber, the mold core height is 19mm.
[0030] Embodiment 2
[0031] A method for preparing an aluminum alloy by low-temperature and high-speed extrusion, comprising the following steps:
[0032] S1: Alloy ingot: The aluminum alloy raw material is cast into an ingot and refined to form a blank to be extruded;
[0033] S2: Pretreatment: heating the billet to be extruded in S1 to 410°C and the extrusion die to 450°C;
[0034] S3: Ingot extrusion: The billet to be extruded after S2 pretreatment is placed into the extrusion die after S2 pretreatment for extrusion; the outflow speed of the aluminum alloy profile after extrusion is 60m / min; the outflow temperature of the aluminum profile is 680°C.
[0035] The pressure of the extrusion die when extruding the billet to be extruded is 2000MPa.
[0036] S4: Cooling and quenching: The aluminum alloy profile generated in S3 is subjected to a forced cooling stage, and water cooling treatment is adopted so that the cooling rate of the aluminum alloy profile after extrusion reaches 300°C / min.
[0037] Then it enters the artificial aging stage, using 200℃, keeping temperature for 4.5 hours, and the Mg in the aluminum alloy profile is finally formed. 2 Si precipitated particles are 0.13 μm.
[0038] In an practicable manner, the extrusion die in S3 is a planar diversion combined die, and the specific structure is referred to Implementation 2.
[0039] The aluminum alloy profiles formed in the above-mentioned embodiment 2 and embodiment 4 achieve low-temperature and high-speed extrusion because the alloy composition and extrusion process are well controlled, thereby improving the production efficiency by more than 40%.
[0040] The surface quality and Webster hardness HW of the aluminum alloy profiles in Example 1 and Example 2 are shown in Table 1.
[0041]
[0042] Table 1
[0043] The parts of the embodiments herein that are not exhaustive of the midpoint values of the technical scope claimed for protection by the present invention and the new technical solutions formed by equivalent replacement of single or multiple technical features in the technical solutions of the embodiments are also within the scope claimed for protection by the present invention; at the same time, in all the listed or unlisted embodiments of the scheme of the present invention, each parameter in the same embodiment merely represents an example of its technical solution (i.e., a feasible solution), and there is no strict coordination and limitation relationship between the parameters, wherein the parameters can be replaced with each other without violating the axioms and the claims of the present invention, unless otherwise stated.
[0044] The technical means disclosed in the scheme of the present invention are not limited to the technical means disclosed in the above technical means, but also include technical schemes composed of any combination of the above technical features. The above is a specific implementation of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications are also regarded as the protection scope of the present invention.
Claims
1. A method for preparing an aluminum alloy by low-temperature and high-speed extrusion, characterized in that: The following steps are involved: S1: Alloy ingot: The aluminum alloy raw material is cast into an ingot and refined to form a blank to be extruded; S2: Pretreatment: Heat the billet to be extruded in S1 to 425°C~450°C, and heat the extrusion die to 380°C~450°C; S3: Ingot extrusion: the billet to be extruded after the S2 pretreatment is placed in the extrusion die after the S2 pretreatment for extrusion; The pressure of the extrusion die when extruding the billet is 2000MPa; the outflow speed of the aluminum alloy profile after extrusion is ≥60m / min; S4: Cooling and quenching: The aluminum alloy profiles generated in S3 are subjected to a forced cooling stage and then enter an artificial aging stage.
2. The method for preparing a low-temperature and high-speed extruded aluminum alloy according to claim 1, characterized in that: The outflow temperature of the aluminum profile in S3 is controlled to be 620℃-680℃.
3. The method for preparing a low-temperature and high-speed extruded aluminum alloy according to claim 1, characterized in that: In the forced cooling stage of S4, water cooling is used to achieve a cooling rate of 300°C / min for the aluminum alloy profile after extrusion.
4. The method for preparing a low-temperature and high-speed extruded aluminum alloy according to claim 3, characterized in that: The artificial aging in S4 is carried out at 200℃ and kept warm for 4H~4.5H.
5. The method for preparing a low-temperature and high-speed extruded aluminum alloy according to claim 3 or 4, characterized in that: The Mg2Si precipitated particles in the aluminum alloy profile of S4 are smaller than 0.2μm.
6. The method for preparing a low-temperature and high-speed extruded aluminum alloy according to claim 1, characterized in that: The extrusion die in S3 is a planar flow-dividing combined die, and the planar flow-dividing combined die has shuttle-shaped holes evenly and symmetrically distributed on the circular die plane.
Citation Information
Patent Citations
Beam aluminum profile production process
CN102397904A
Method for achieving rapid low-temperature extrusion formation of 6063 aluminum alloy
CN104353689A
Material for thermal-insulating aluminum alloy doors and windows and manufacturing method thereof
CN105735831A
Method for producing aluminum alloy profiles for doors and windows of high-speed trains
CN106694591A
Extrusion technology for aluminum alloy profile
CN107008763A