A wide temperature range low friction composite coating and its preparation method and application

By depositing a multi-layer structural coating with alternate stacks of VAlN/Ag on the substrate surface, the problems of high friction coefficient and poor wear resistance in the wide temperature range are solved, and the coating performance with low friction coefficient and long wear life is achieved. Suitable for high temperature environments.

CN115354288BActive Publication Date: 2024-11-19QIANWAN INST OF CNITECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210985117.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-16
Publication Date
2024-11-19
Estimated Expiration
2042-08-16

AI Technical Summary

Technical Problem

The prior art is difficult to provide solid lubricating materials with low friction and high thermal stability in a wide temperature range. Traditional coatings have high friction coefficient and short wear resistance in high temperature environments, and the preparation conditions for the multiple phase components are complex and the performance is not good.

Method used

The VAlN/Ag alternate stack is deposited on the substrate surface using DC reactive magnetron sputtering technology and high-power pulse magnetron sputtering technology to form a wide temperature domain low friction composite coating with multi-layer structure. The VAlN layer provides support and hardness, Ag The layer provides lubricity and induces the formation of a lubricating phase at high temperatures.

Benefits of technology

It achieves a low friction coefficient and long wear-resistant life in a wide temperature range of 25 to 650℃. The coating has not failed in a high-temperature environment and is suitable for key moving parts of aerospace engines and industrial machinery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115354288B_ABST
    Figure CN115354288B_ABST
Patent Text Reader

Abstract

The present invention discloses a wide temperature range low-friction composite coating and its preparation method and application. The wide temperature range low-friction composite coating comprises: a transition layer and a VAlN / Ag alternating laminate formed on the surface of a substrate in sequence, wherein the VAlN / Ag alternating laminate is a nano multilayer coating formed by alternating VAlN layers and Ag layers, and the outermost layer of the VAlN / Ag alternating laminate is an Ag layer; the VAlN layer is composed of a VN phase with a crystal plane index of (111) and (220) and a w-AlN phase with a crystal plane index of (101); the Ag layer is composed of an Ag phase with a crystal plane index of (200) and (220). The wide temperature range low-friction composite coating prepared by the present invention has tribological properties of low friction coefficient and long wear life within 25 to 650°C, and has broad application prospects in the fields of aerospace engines, key moving parts of industrial machinery, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of solid lubricating materials, and in particular relates to a low-friction composite coating with a wide temperature range and a preparation method and application thereof. Background Art

[0002] Aircraft engines are gradually developing towards high flow ratio and high thrust-to-weight ratio, and they are faced with bottleneck technical problems such as lubrication and wear resistance in a wide temperature range during service. In particular, key components such as blade crowns, foil bearings, brush wire comb teeth, etc., experience frequent start-stop, high-speed and heavy-load conditions during service in a wide temperature range, which increases their service temperature, causes friction between the two contact surfaces, and causes severe wear, shortening the life of the components and eventually causing failure, which in turn affects the safety and stability of the entire operating system. Traditional solid lubricating materials can no longer meet the performance requirements of the above-mentioned harsh working conditions, and there is an urgent need to develop wide-temperature range wear-resistant and friction-reducing coating material technology with excellent low friction and high thermal stability.

[0003] Single lubricating materials often have specific use environment requirements and applicable temperature ranges. For example, MoS2 is suitable for dry or vacuum environments, and the use temperature cannot exceed 350°C. Nitride coatings such as VN, CrN, and MoN have applicable temperatures of 500-700°C, and the friction coefficient is higher in other temperature ranges. In the design and preparation of low-friction coatings with a wide temperature range, researchers prepared composite coatings by compounding multi-phase components, including the addition of soft metals, to meet the needs of lubrication applications. For example, patent CN202010581856.8 discloses a VN-Ag2MoO4 composite material, which has good self-lubricating properties from room temperature to 700°C, but the preparation conditions are harsh and the preparation method is relatively complicated. The friction coefficient from room temperature to 300°C is higher than 0.62, and the friction coefficients at 500 and 700°C are higher than 0.35 and 0.25, respectively. Therefore, the friction coefficient is high in a wide temperature range; patent CN201910549021.1 discloses a VAlCN / VN-Ag multilayer structure coating prepared by multi-arc ion plating technology, which is mainly used for high-temperature protection, but the controllable preparation of Ag single layer cannot be achieved. The tribological properties of the coating such as friction coefficient, wear life, wear rate in a wide temperature range need to be further improved.

[0004] Compounding multi-phase components to prepare a low-friction coating with a wide temperature range requires solving several key technical problems, such as difficult interface matching, uncontrollable element content, and difficult regulation of multi-phase components. At the same time, the sputtering yield of soft metal targets (taking Ag targets as an example) is high. When using a DC power supply to sputter the Ag target, the Ag element content in the coating is too high, the coating is loose, and there is insufficient support during the friction process, resulting in increased wear rate and failure; when using an RF power supply to sputter the Ag target, the discharge is unstable and trace uniform doping is difficult to achieve. Therefore, providing a composite coating with a wide temperature range, low friction coefficient, and long wear life is an urgent problem to be solved. Summary of the invention

[0005] The main purpose of the present invention is to provide a wide temperature range low friction composite coating and a preparation method and application thereof, so as to overcome the shortcomings of the prior art.

[0006] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:

[0007] The embodiment of the present invention provides a wide temperature range low friction composite coating, which comprises: a transition layer and a VAlN / Ag alternating laminate formed on the surface of a substrate in sequence, wherein the VAlN / Ag alternating laminate is a nano multilayer coating formed by alternatingly laminating a VAlN layer as a support layer and an Ag layer as a lubricating layer, and the outermost layer of the VAlN / Ag alternating laminate is an Ag layer;

[0008] The VAlN layer is composed of a VN phase with crystal plane indices (111) and (220) and a w-AlN phase with a crystal plane index (101); and the Ag layer is composed of an Ag phase with crystal plane indices (200) and (220).

[0009] The embodiment of the present invention further provides a method for preparing the aforementioned wide temperature range low friction composite coating, which comprises:

[0010] providing a substrate;

[0011] A DC reactive magnetron sputtering technique is used to deposit a transition layer on the surface of the substrate;

[0012] Furthermore, a DC reactive magnetron sputtering composite high-power pulsed magnetron sputtering technology is used to deposit VAlN / Ag alternating layers on the surface of the transition layer until the wide temperature range low-friction composite coating is formed.

[0013] The embodiment of the present invention also provides the use of the aforementioned wide temperature range low friction composite coating in the field of solid lubrication protection.

[0014] Compared with the prior art, the present invention has the following beneficial effects:

[0015] (1) The present invention adopts DC reactive magnetron sputtering combined with high-power pulsed magnetron sputtering technology to prepare a wide temperature range low-friction composite coating. The prepared wide temperature range low-friction composite coating is a multilayer structure and is composed of three main phases of VN, w-AlN and Ag. Strong interaction occurs between the ionic bond compound VN and the covalent bond compound w-AlN to form a VAlN layer with a hardness greater than 35 GPa, and the VAlN layer is a dense columnar crystal structure, which plays a supporting role and inhibits the rapid diffusion of the underlying Ag element during the wide temperature range friction process, thereby preventing the coating from failing quickly and increasing the wear resistance of the coating. A flat and smooth Ag lubricating layer is prepared by high-power pulsed magnetron sputtering technology, and a strong bonding force is formed between the Ag lubricating layer and the VAlN layer, thereby increasing the toughness of the coating, providing lubrication during the friction process in medium and low temperature environments, and inducing the generation of a high-temperature lubricating phase during the high-temperature friction process.

[0016] (2) During the low-temperature friction process of 25°C, the Ag layer on the surface of the wide-temperature low-friction composite coating prepared by the present invention plays a major lubricating role, and the friction coefficient is 0.4-0.51; during the medium-temperature friction process of 300°C, an oxide lubricating phase is formed on the surface of the Ag layer, and the friction coefficient is 0.36-0.31; during the high-temperature friction process of 650°C, the friction of the coating induces the generation of layered AgVO3 and Ag3VO4 lubricating phases, interlayer slip occurs, and the friction coefficient is reduced to 0.13-0.22; the coating does not fail after a long-distance friction of 180 meters, thereby making the composite coating have tribological properties of low friction coefficient and long wear life in a wide temperature range of 25-650°C; the composite coating can be used as a new wide-temperature solid lubricating coating, which can be applied to the fields of aerospace engines, key moving parts of industrial machinery, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0018] Figure 1 is the XRD diagram of the wide temperature range low friction composite coating in Example 1 of the present invention at different temperatures;

[0019] Figure 2a-2b They are respectively the surface and cross-sectional SEM images of the wide temperature range low friction composite coating in Example 1 of the present invention;

[0020] Figure 3 is a diagram of the tribological performance of the wide temperature range low friction composite coating at different temperatures in Example 1 of the present invention;

[0021] Figure 4 This is a long friction distance life graph of the wide temperature range low friction composite coating at high temperature in Example 1 of the present invention;

[0022] Figure 5 is a cross-sectional SEM image of the wide temperature range low friction composite coating in Comparative Example 2 of the present invention;

[0023] Figure 6 is a cross-sectional SEM image of the wide temperature range low friction composite coating in Comparative Example 3 of the present invention;

[0024] Figure 7a-Figure 7b It is a schematic diagram of the structure of a wide temperature range low friction composite coating in a typical embodiment of the present invention. DETAILED DESCRIPTION

[0025] In view of the defects of the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] Specifically, as one aspect of the technical solution of the present invention, a wide temperature range low friction composite coating involved therein comprises: a transition layer and a VAlN / Ag alternating laminate formed on the surface of a substrate in sequence, wherein the VAlN / Ag alternating laminate is a nano multilayer coating formed by alternatingly laminating a VAlN layer as a support layer and an Ag layer as a lubricating layer, and the outermost layer of the VAlN / Ag alternating laminate is an Ag layer;

[0027] The VAlN layer is composed of a VN phase with crystal plane indices (111) and (220) and a w-A1N phase with a crystal plane index (101); the Ag layer is composed of an Ag phase with crystal plane indices (200) and (220).

[0028] Furthermore, the wide temperature range low friction composite coating has tribological properties of low friction coefficient and long wear life in a wide temperature range of 25 to 650°C.

[0029] In some preferred embodiments, the VAlN / Ag alternating stack comprises 1 to 5 alternating stacking periodic layers, wherein each alternating stacking periodic layer comprises a VAlN layer and an Ag layer.

[0030] Furthermore, in each of the alternately stacked periodic layers, the thickness of the VAlN layer is 0.20-0.32 μm, and the thickness of the Ag layer is 0.05-0.15 μm.

[0031] In some preferred embodiments, the structural schematic diagram of the wide temperature range low friction composite coating of the present invention is as follows Figure 7a-Figure 7b shown.

[0032] In some preferred embodiments, the VAlN layer has a dense columnar crystal structure.

[0033] In some preferred embodiments, the Ag layer is a dense and smooth nanolayer structure.

[0034] In some preferred embodiments, the VAlN layer is tightly bonded to the Ag layer.

[0035] In some preferred embodiments, the material of the transition layer includes any one of titanium, tantalum, chromium, and niobium, but is not limited thereto.

[0036] In some preferred embodiments, the thickness of the transition layer is 0.15-0.35 μm.

[0037] In some preferred embodiments, the wide temperature range low friction composite coating has a thickness of 1.1 to 2.1 μm.

[0038] In the present invention, the function of the VAlN layer is to provide support and inhibit the rapid diffusion of the Ag element; the function of the Ag layer is to provide lubricity and is conducive to inducing the formation of a lubricating phase at high temperature. The wide temperature range low friction composite coating of the present invention obtains low friction coefficients of about 0.40, 0.30, and 0.13 at 25°C, 300°C, and 650°C, respectively, and does not fail after high speed (10cm / s) and long distance (180m) friction, thereby making the composite coating have the characteristics of low friction coefficient and long wear life in a wide temperature range.

[0039] After high-temperature friction, the wide-temperature-range low-friction composite coating of the present invention mainly forms AgVO3 phases with crystal plane indices of (-301) and (112) and Ag3VO4 phases with crystal plane indices of (011) and (301), which, as lubricating phases, are beneficial to reducing the high-temperature friction coefficient and making the composite coating have high-temperature self-lubricating properties.

[0040] Another aspect of the embodiments of the present invention further provides a method for preparing the aforementioned wide temperature range low friction composite coating, which comprises:

[0041] providing a substrate;

[0042] A DC reactive magnetron sputtering technique is used to deposit a transition layer on the surface of the substrate;

[0043] Furthermore, a DC reactive magnetron sputtering composite high-power pulsed magnetron sputtering technology is used to deposit VAlN / Ag alternating layers on the surface of the transition layer until the wide temperature range low-friction composite coating is formed.

[0044] In some preferred embodiments, the preparation method specifically comprises:

[0045] The substrate is placed in a vacuum chamber of a coating device, with an inert gas as the working atmosphere and a metal target as the target material. A DC reactive magnetron sputtering technique is used to deposit a transition layer on the surface of the substrate, wherein the material of the metal target includes any one of titanium, tantalum, chromium, and niobium, and the sputtering power of the metal target is 70 to 100 W.

[0046] Furthermore, the substrate is placed in a vacuum chamber of a coating device, and the vacuum chamber is evacuated to 5 to 9×10 -4 pa, and then the substrate is subjected to argon plasma etching.

[0047] In some preferred embodiments, the preparation method specifically comprises:

[0048] After the transition layer is deposited, a VAlN layer is formed on the surface of the transition layer by using nitrogen as the working atmosphere and a VA1 composite target as the target material, using a DC reactive magnetron sputtering composite high-power pulsed magnetron sputtering technology, wherein the sputtering power supply of the VAl composite target is a DC power supply, the sputtering power is 90 to 150 W, the sputtering time is 25 to 40 min, and the flow rate of nitrogen is 5 to 15 sccm;

[0049] Using an inert gas as the working atmosphere and an Ag target as the target material, a DC reactive magnetron sputtering composite high-power pulsed magnetron sputtering technology is used to deposit an Ag layer on the surface of the VAlN layer, wherein the sputtering power supply of the Ag target is a high-power pulsed power supply, the sputtering power is 10 to 40 W, the sputtering time is 10 to 40 minutes, and the duty cycle of the high-power pulsed power supply is 4% to 10%;

[0050] And, the VAlN layer and the Ag layer are alternately stacked until the VAlN / Ag alternate stack is formed.

[0051] Furthermore, the atomic percentage ratio of V to Al in the VAl composite target is 50:50.

[0052] Furthermore, the sputtering yield of soft metal targets (taking Ag targets as an example) is high, and the high-power pulse power supply has the advantages of high plasma density, good winding properties, and high ionization rate. It can prepare high-density, relatively smooth, and large-particle-free coatings, which can meet the preparation requirements of stable and content-controllable low-friction coatings in a wide temperature range.

[0053] In some preferred embodiments, the rotation speed of the base frame on which the substrate is placed is 20 to 50 r / min.

[0054] In some preferred embodiments, the material of the substrate includes Ni-based high-temperature alloy, but is not limited thereto.

[0055] Furthermore, the Ni content in the Ni-based high-temperature alloy is 55-72wt%.

[0056] Another aspect of the embodiments of the present invention further provides the use of the aforementioned wide temperature range low friction composite coating in the field of solid lubrication protection.

[0057] For example, in the field of protection of critical moving parts in aerospace engines or industrial machinery.

[0058] Furthermore, the use is in the preparation of a solid lubricating coating with a wide temperature range of 25 to 650°C.

[0059] The technical solution of the present invention is further described in detail below in conjunction with several preferred embodiments and drawings. This embodiment is implemented on the premise of the technical solution of the invention, and a detailed implementation method and specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments.

[0060] Unless otherwise specified, the experimental materials used in the following examples can be purchased from conventional biochemical reagent companies.

[0061] Example 1

[0062] Preparation of wide temperature range low friction composite coating: polish the high temperature alloy substrate to a roughness of Ra ≤ 0.1 μm, ultrasonically clean it with ethanol and acetone three times respectively, and then stick it on the base frame, and set the base frame rotation speed to 20 r / min. Turn on the mechanical pump and molecular pump in turn, and evacuate the equipment to 9×10 -4 Pa, heat the coating chamber. Then introduce Ar to raise the chamber pressure to 2MPa, turn on the pulse power supply, and etch the substrate for 30 minutes. Turn on the DC power supply to sputter the titanium target with a sputtering power of 70W, and deposit a transition layer with a thickness of about 0.15 microns. Introduce N2, turn on the VA1 target DC power supply, sputter for 25 minutes, and deposit a VAlN layer with a thickness of about 0.20 microns; then turn off the VAl target DC power supply and the N2 valve, turn on the high-power pulse power supply, sputter the Ag target, set the duty cycle to 10%, the sputtering power to 10W, sputter for 10 minutes, and deposit an Ag layer with a thickness of about 0.05 microns; repeat the deposition 4 times alternately to form a VAlN / Ag alternating stack.

[0063] After the coating is completed, wait for the temperature of the vacuum chamber to drop to room temperature, take out the prepared wide temperature range low-friction composite coating sample, and test its tribological properties with a ball-disc friction machine. The friction coefficient at 25°C is 0.51, the friction coefficient at 300°C is 0.36, and the average friction coefficient at 650°C is 0.22. The composite coating has good toughness and wear resistance, and it still does not fail after long-distance and high-speed friction, showing excellent tribological properties in a wide temperature range. Figure 1 : is the XRD diagram of the wide temperature range low friction composite coating at different temperatures in this embodiment; Figure 2a-2b They are respectively the surface and cross-sectional SEM images of the wide temperature range low friction composite coating in this embodiment; Figure 3 is a tribological performance diagram of the wide temperature range low friction composite coating at different temperatures in this embodiment; Figure 4 This is a long friction distance life diagram of the wide temperature range low friction composite coating at high temperature in this embodiment.

[0064] Example 2

[0065] Preparation of wide temperature range low friction composite coating: polish the high temperature alloy substrate to a roughness Ra ≤ 0.1 μm, ultrasonically clean it with ethanol and acetone three times respectively, and then stick it on the base frame, and set the base frame rotation speed to 30 r / min. Turn on the mechanical pump and molecular pump in turn, and evacuate the equipment to 9×10 -4 Pa, heat the coating chamber. Then introduce Ar to raise the chamber pressure to 2MPa, turn on the pulse power supply, and etch the substrate for 30 minutes. Turn on the DC power supply to sputter the tantalum target with a sputtering power of 80W, and deposit a transition layer with a thickness of about 0.2 microns. Introduce N2, turn on the VA1 target DC power supply, sputter for 30 minutes, and deposit a VAlN layer with a thickness of about 0.25 microns; then turn off the VAl target DC power supply and the N2 valve, turn on the high-power pulse power supply, sputter the Ag target, set the duty cycle to 8%, the sputtering power to 20W, sputter for 20 minutes, and deposit an Ag layer with a thickness of about 0.07 microns; repeat the deposition 4 times alternately to form a VAlN / Ag alternating stack.

[0066] After the coating is completed, wait for the temperature of the vacuum chamber to drop to room temperature, take out the prepared wide temperature range low-friction composite coating sample, and test its tribological properties with a ball-disc friction machine. The friction coefficient at 25°C is 0.47, the friction coefficient at 300°C is 0.34, and the average friction coefficient at 650°C is 0.19. The coating has good toughness and wear resistance, and it still does not fail after long-distance and high-speed friction, showing excellent tribological properties in a wide temperature range.

[0067] Example 3

[0068] Preparation of wide temperature range low friction composite coating: polish the high temperature alloy substrate to a roughness of Ra ≤ 0.1 μm, ultrasonically clean it with ethanol and acetone three times respectively, and then stick it on the base frame, and set the base frame rotation speed to 40 r / min. Turn on the mechanical pump and molecular pump in turn, and evacuate the equipment to 9×10 -4Pa, heat the coating chamber. Then introduce Ar to raise the chamber pressure to 2MPa, turn on the pulse power supply, and etch the substrate for 30 minutes. Turn on the DC power supply to sputter the chromium target with a sputtering power of 90W, and deposit a transition layer with a thickness of about 0.3 microns. Introduce N2, turn on the VAl target DC power supply, sputter for 35 minutes, and deposit a VAlN layer with a thickness of about 0.28 microns; then turn off the VAl target DC power supply and the N2 valve, turn on the high-power pulse power supply, sputter the Ag target, set the duty cycle to 6%, the sputtering power to 30W, and sputter for 30 minutes, and deposit an Ag layer with a thickness of about 0.09 microns; repeat the deposition 4 times alternately to form a VAlN / Ag alternating stack.

[0069] After the coating is completed, wait for the temperature of the vacuum chamber to drop to room temperature, take out the prepared wide temperature range low-friction composite coating sample, and test its tribological properties with a ball-disc friction machine. The friction coefficient at 25°C is 0.43, the friction coefficient at 300°C is 0.33, and the average friction coefficient at 650°C is 0.15. The coating has good toughness and wear resistance, and it still does not fail after long-distance and high-speed friction, showing excellent tribological properties in a wide temperature range.

[0070] Example 4

[0071] Preparation of wide temperature range low friction composite coating: polish the high temperature alloy substrate to a roughness Ra ≤ 0.1 μm, ultrasonically clean it three times with ethanol and acetone respectively, and then stick it on the base frame, and set the base frame rotation speed to 50 r / min. Turn on the mechanical pump and molecular pump in turn, and evacuate the equipment to 9×10 -4 Pa, heat the coating chamber. Then introduce Ar to raise the chamber pressure to 2MPa, turn on the pulse power supply, and etch the substrate for 30 minutes. Turn on the DC power supply to sputter the niobium target, with a sputtering power of 100W, and deposit a transition layer with a thickness of about 0.35 microns. Introduce N2, turn on the VAl target DC power supply, sputter for 40 minutes, and deposit a VAlN layer with a thickness of about 0.32 microns; then turn off the VAl target DC power supply and the N2 valve, turn on the high-power pulse power supply, sputter the Ag target, set the duty cycle to 4%, the sputtering power to 40W, and sputter for 40 minutes, and deposit an Ag layer with a thickness of about 0.11 microns; repeat the deposition 4 times alternately to form a VAlN / Ag alternating stack.

[0072] After the coating is completed, wait for the temperature of the vacuum chamber to drop to room temperature, take out the prepared wide temperature range low-friction composite coating sample, and test its tribological properties with a ball-disc friction machine. The friction coefficient at 25°C is 0.4, the friction coefficient at 300°C is 0.31, and the average friction coefficient at 650°C is 0.13. The coating has good toughness and wear resistance, and it still does not fail after long-distance and high-speed friction, showing excellent tribological properties in a wide temperature range.

[0073] Comparative Example 1

[0074] Different from Example 1-4, the base frame rotation speed is set to 18r / min, the DC power supply is turned on to sputter the titanium target, the sputtering power is 60W, and the transition layer with a thickness of about 0.10 microns is deposited. The VAl target is sputtered for 20min, and the VAlN layer with a thickness of about 0.16 microns is deposited; when sputtering the Ag target, the duty cycle is set to 15%, the sputtering power is 9W, and the sputtering is performed for 7min, and the Ag layer with a thickness of about 0.03 microns is deposited; this is alternately deposited twice to form a multilayer structure of VAlN and Ag.

[0075] After the coating is completed, the temperature of the vacuum chamber is cooled to room temperature, and the prepared VAlN / Ag coating sample is taken out and its tribological properties are tested by a ball-disc friction machine, and the friction coefficient at 25°C is 0.65, the friction coefficient at 300°C is 0.45, and the average friction coefficient at 650°C is 0.35. Compared with the above-mentioned Examples 1-4, the coating prepared in Comparative Example 1 is thinner, contains less Ag, has insufficient lubricity, cannot form sufficient lubricating phase at high temperature, exhibits a relatively high friction coefficient in a wide temperature range, has a short friction life, and has poor tribological properties.

[0076] Comparative Example 2

[0077] The method is the same as in Example 1, except that a DC reactive magnetron sputtering technique is used to deposit alternating VAlN / Ag layers on the surface of the transition layer. The base frame rotation speed is set to 20 r / min, and the DC power supply is turned on to sputter the titanium target with a sputtering power of 80 W, and a transition layer with a thickness of about 0.24 microns is deposited. The VAl target is sputtered for 25 minutes to deposit a VAlN layer with a thickness of about 0.21 microns; when sputtering the Ag target, the duty cycle is set to 6%, the sputtering power is 11 W, and the sputtering is performed for 8 minutes to deposit an Ag layer with a thickness of about 0.05 microns; this is repeated 4 times to form a multilayer structure coating of VAlN and Ag with a thickness of 2.38 microns.

[0078] After the coating is completed, wait for the temperature of the vacuum chamber to drop to room temperature, take out the prepared VAlN / Ag coating sample, and test its tribological properties with a ball-disc friction machine. The friction coefficient at 25°C is 0.8, the friction coefficient at 300°C is 0.5, and the average friction coefficient at 650°C is 0.4. Compared with the above-mentioned embodiments 1-4, the sputtering mode of the coating prepared in comparative example 2 is different. The Ag layer is thicker, the Ag content is not easy to control, the columnar crystals are coarse, the thickness of the Ag layer is uneven, and there are undulations between the layers. It is uneven and encounters greater resistance during friction. It shows a relatively high friction coefficient in a wide temperature range, the friction life is short, and the tribological performance is poor. The cross-sectional SEM image of the wide temperature range low-friction composite coating in this comparative example is shown in the figure. Figure 5 shown.

[0079] Comparative Example 3

[0080] The method is the same as in Example 1, except that the Ag layer is missing, and a VAlN layer is deposited on the surface of the transition layer by using a DC reactive magnetron sputtering technique. The base frame rotation speed is set to 22 r / min, and a DC power supply is turned on to sputter the titanium target with a sputtering power of 100 W, and a transition layer with a thickness of about 0.27 microns is deposited. The VA1 target is sputtered for 160 minutes, and a VAlN layer with a thickness of about 0.88 microns is deposited; Ag is not sputtered; a VAlN single-layer structure coating is formed with a thickness of 1.15 microns.

[0081] After the coating is completed, wait for the temperature of the vacuum chamber to drop to room temperature, take out the prepared VAlN coating sample, and test its tribological properties with a ball-disc friction machine. The friction coefficient at 25°C is 0.76, the friction coefficient at 300°C is 0.9, and the average friction coefficient at 650°C is 0.44. Compared with the above-mentioned Examples 1-4, the sputtering mode of the coating prepared in Comparative Example 3 is different. There is no Ag layer, and the columnar crystals are finer. The friction coefficient is very high in medium and low temperature environments. In high temperature environments, it mainly generates V2O5 lubricating phase, which has insufficient lubrication performance, resulting in a high high-temperature friction coefficient. The VAlN single-layer structure coating shows a relatively high friction coefficient in a wide temperature range, a short friction life, and poor tribological performance. The cross-sectional SEM image of the wide temperature range low-friction composite coating in this comparative example is shown in the figure. Figure 6 shown.

[0082] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.

[0083] It should be understood that the technical solution of the present invention is not limited to the above-mentioned specific implementation cases. Any technical deformation made according to the technical solution of the present invention without departing from the scope of protection of the purpose of the present invention and the claims shall fall within the protection scope of the present invention.

Claims

1. A low-friction composite coating with a wide temperature range, Features include: A transition layer and a VAlN / Ag alternating laminate are sequentially formed on the surface of the substrate, wherein the VAlN / Ag alternating laminate is a nano multilayer coating formed by alternating a VAlN layer as a support layer and an Ag layer as a lubricating layer, and the outermost layer of the VAlN / Ag alternating laminate is an Ag layer; the material of the transition layer is selected from any one of titanium, chromium, and niobium; the thickness of the transition layer is 0.15-0.35 μm; the thickness of the wide temperature range low friction composite coating is 1.1-2.1 μm; The VAlN layer is composed of a VN phase with crystal plane indices of (111) and (220) and a w-AlN phase with a crystal plane index of (101); the Ag layer is composed of an Ag phase with crystal plane indices of (200) and (220); the VAlN layer has a columnar crystal structure; the Ag layer is a smooth nano-layer structure; The method for preparing the wide temperature range low friction composite coating comprises: providing a substrate; The substrate is placed in a vacuum chamber of a coating device, an inert gas is used as a working atmosphere, a metal target is used as a target material, and a DC reactive magnetron sputtering technique is used to deposit a transition layer on the surface of the substrate, wherein the material of the metal target is selected from any one of titanium, chromium, and niobium, and the sputtering power of the metal target is 70-100W; After the transition layer is deposited, a VAlN layer is formed on the surface of the transition layer by using nitrogen as the working atmosphere and a VAl composite target as the target material, and adopting a DC reactive magnetron sputtering composite high-power pulsed magnetron sputtering technology, wherein the sputtering power source of the VAl composite target is a DC power source, the sputtering power is 90-150 W, the sputtering time is 25-40 min, and the flow rate of nitrogen is 5-15 sccm; Using inert gas as working atmosphere and Ag target as target material, a DC reactive magnetron sputtering composite high-power pulsed magnetron sputtering technology is adopted to deposit and form an Ag layer on the surface of the VAlN layer, wherein the sputtering power supply of the Ag target is a high-power pulsed power supply, the sputtering power is 10-40W, the sputtering time is 10-40min, and the duty cycle of the high-power pulsed power supply is 4%-10%; And, the VAlN layer and the Ag layer are alternately stacked until a VAlN / Ag alternating stack is formed, thereby obtaining the wide temperature range low friction composite coating.

2. The wide temperature range low friction composite coating according to claim 1, Features: The VAlN / Ag alternating stack includes 1 to 5 alternating stacking periodic layers, wherein each alternating stacking periodic layer includes a VAlN layer and an Ag layer.

3. The wide temperature range low friction composite coating according to claim 2, Features: The thickness of the VAlN layer in each of the alternately stacked periodic layers is 0.20-0.32 μm, and the thickness of the Ag layer is 0.05-0.15 μm.

4. The wide temperature range low friction composite coating according to claim 1, Features: The substrate is placed in a vacuum chamber of a coating device, and the vacuum chamber is evacuated to 5-9×10 -4 Pa, and then the substrate is subjected to an argon plasma etching treatment.

5. The wide temperature range low friction composite coating according to claim 1, Features: The atomic percentage ratio of V to Al in the VAl composite target is 50:

50.

6. The wide temperature range low friction composite coating according to claim 1, Features: The rotation speed of the base frame on which the substrate is placed is 20-50 r / min.

7. The wide temperature range low friction composite coating according to claim 1, Features: The material of the substrate is selected from Ni-based high-temperature alloy.

8. Use of the wide temperature range low friction composite coating according to any one of claims 1 to 7 in the field of solid lubrication protection.

9. The use according to claim 8, Features: The application is the use of the wide temperature range low friction composite coating in the preparation of a wide temperature range solid lubricating coating of 25-650°C.