A thin layer low rolling resistance pavement and preparation method thereof
By setting up a thin-layer pavement structure with small-diameter aggregates without compaction on existing roads, the problem of balancing low rolling resistance and high skid resistance on existing roads has been solved, achieving the effects of rapid construction and high friction performance.
Patent Information
- Application Number
- CN202211047652.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-30
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-08-30
AI Technical Summary
Existing technologies cannot quickly achieve a balance between low rolling resistance and high skid resistance on existing roads, and the investment in new low rolling resistance asphalt concrete pavement projects is large, which is not conducive to rapid promotion.
A first epoxy asphalt seal, a second epoxy asphalt seal, and a sealing layer are applied to the original road surface using a synchronous spreading process. Anti-skid aggregates and binders of specific particle sizes are used to form a thin-layer road structure with small-particle aggregates that are not compacted.
It achieves a reduction of over 10% in rolling resistance of existing roads, a saving of over 3% in energy consumption, and an increase of over 50% in road surface friction, enabling rapid construction and high friction performance.
Smart Images

Figure CN115354546B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of road maintenance engineering, and in particular relates to a thin-layer low-rolling resistance pavement and a preparation method thereof. Background Art
[0002] The rolling resistance of the tire is a kind of energy loss when the tire moves on the road. Too high rolling resistance not only causes traction loss but also produces more pollutants. When the rolling resistance is low, the pollutants (such as CO2 and NO X ) will be reduced. Studies have shown that rolling resistance is closely related to vehicle fuel consumption. When rolling resistance is reduced by 10% to 20%, fuel consumption can be reduced by up to 2.5% to 3.6%, and the fuel consumption reduction effect of heavy vehicles is more obvious. Reducing the rolling resistance during vehicle operation has become a necessary technical research in the automotive industry, and has also achieved relatively obvious results. The tire industry is committed to reducing the rolling resistance of tires during operation from the tire manufacturing field, while ignoring the impact of the road on the tire.
[0003] Studies have shown that tire-road rolling resistance is directly related to the road surface structure, smoothness, and road surface strength. The better the road surface smoothness, the smaller the tire-road rolling resistance. Danish researchers first noticed this detail and began to study low rolling resistance roads and achieved certain results. The "Roads Saving Energy" project promoted by the Danish Road Administration has designed a durable asphalt concrete pavement that can reduce rolling resistance by 5%, namely "low rolling resistance asphalt concrete pavement." According to calculations by relevant Danish departments: The application of low rolling resistance asphalt concrete pavement can reduce the fuel consumption of transportation equipment in Denmark by about 3.3%, saving 48 million liters of fuel and 45,000 tons of greenhouse gases each year.
[0004] Low rolling resistance asphalt concrete pavement achieves the purpose of reducing tire-road rolling resistance by improving the overall performance of asphalt concrete pavement and reducing the surface structural depth. However, the reduction of pavement structural depth will have a certain negative impact on anti-skid performance, so there are certain limitations to the research on low rolling resistance pavement based on asphalt concrete. At the same time, the investment in new low rolling resistance asphalt concrete pavement projects is large. If existing roads are to be renovated, milling is required, which is not conducive to rapid promotion.
[0005] As of 2019, the total mileage of China's highways has reached 4.8465 million kilometers. Compared with the construction of new low-rolling resistance asphalt concrete pavement, it is more practical and economically beneficial to transform the existing pavement into a low-rolling resistance pavement to achieve the function of "low-rolling resistance pavement". Assumption: The fuel consumption of civilian vehicles is 8 liters, and each vehicle travels 10,000 kilometers per year. Reducing the tire-road rolling resistance by 5% is equivalent to saving 1.5% of energy consumption, saving 0.12 liters of fuel per 100 kilometers, and saving 12 liters of fuel per vehicle per year. Based on the 3.727 million vehicles in Shenzhen in 2021, if the low rolling resistance transformation can be applied on a large scale in Shenzhen's road network, it can be shown that Shenzhen can reduce fuel consumption by 44.72 million liters per year, which has very large economic and environmental benefits.
[0006] Road surface texture is the most important characteristic index that determines the interaction between tires and roads, such as friction, noise, hydroplaning, tire wear, rolling resistance, etc. The World Road Association divides road surface characteristics into four scales from large to small: roughness, macrotexture, macrotexture and microtexture, based on the wavelength, amplitude, power spectrum characteristics of the road surface structure and its possible impact on road users.
[0007] In his paper "Research on Decision-making of Asphalt Pavement Anti-skid Restoration Technology Based on Road Surface Texture Characteristics", Jiang Yongmao from Southeast University pointed out that conventional asphalt concrete pavement needs to be rolled during construction, so the texture structure of the pavement after forming is "negative texture". Under this negative texture characteristic, the larger the macro texture, the better the pavement's anti-skid performance, but the greater the pavement's rolling resistance.
[0008] The opposite of negative texture is the "positive texture" structure with more outstanding anti-slip performance, such as Figure 1 As shown, the positive texture pavement structure is used to minimize the texture structure of the pavement while ensuring the skid resistance, which can achieve an effective balance between the pavement's skid resistance and the pavement's rolling resistance.
[0009] like Figure 2 As shown, the grayscale processing of the scanned photos of different pavement structures is used to intuitively reflect the differences between different pavement texture structures. The present invention can form a more uniform, fine and dense positive texture pavement structure by combining anti-skid aggregate of specific particle size with a certain amount of binder compared to asphalt concrete pavement, micro-surfacing, crushed stone seal, etc. Summary of the invention
[0010] In order to enable an existing road surface to achieve the road surface function of reducing tire-road rolling resistance through simple modification, the present invention provides a thin-layer low rolling resistance road surface and a preparation method thereof.
[0011] The technical solution adopted by the present invention is: a thin layer of low rolling resistance pavement and a preparation method thereof, wherein a first epoxy asphalt seal layer, a second epoxy asphalt seal layer and a sealing layer are arranged from bottom to top on the original pavement by a synchronous spreading process; the original pavement, the first epoxy asphalt seal layer, the second epoxy asphalt seal layer and the sealing layer are arranged in sequence from bottom to top.
[0012] Furthermore, the original road surface is one of an asphalt concrete road surface and an asphalt concrete road surface with a seal layer or a functional overlay.
[0013] Furthermore, a thin-layer low rolling resistance pavement and a preparation method thereof comprises the following steps:
[0014] Step 1: A first epoxy asphalt seal layer is arranged on the original pavement; the first epoxy asphalt seal layer is prepared by a simultaneous spreading process of a binder and an anti-skid aggregate, and the anti-skid aggregate uses an anti-skid aggregate with a particle size of 1 to 2 mm or an anti-skid aggregate with a particle size of 1 to 1.5 mm; the binder uses one of 0.6 to 1.4 kg / m2 of water-based epoxy asphalt or 0.3 to 0.7 kg / m2 of oil-based epoxy asphalt; the anti-skid aggregate is selected from one of corundum, basalt particles, and ceramic particles, and the amount used is 1.5 to 2.8 kg / m2.
[0015] Step 2: After the first layer of epoxy asphalt seal is dried and cured, the construction of the second layer of epoxy asphalt seal is started; the second epoxy asphalt seal adhesive and anti-skid aggregate are prepared by a synchronous sprinkling (scattering) process, and the anti-skid aggregate has a particle size of 1 to 1.5 mm or a particle size of 0.5 to 1 mm; the adhesive uses 0.6 to 1.2 kg / ㎡ of water-based epoxy asphalt or 0.3 to 0.6 kg / ㎡ of oil-based epoxy asphalt; the anti-skid aggregate can be selected from one of corundum, basalt particles, and ceramic particles, with a dosage of 1.4 to 2.0 kg / ㎡.
[0016] Step 3: After the second layer of epoxy asphalt seal is dried and cured, the construction of the sealing layer begins; the sealing layer is prepared by spreading 0.5-0.8 kg / ㎡ of water-based epoxy asphalt or 0.2-0.4 kg / ㎡ of oil-based epoxy asphalt.
[0017] Different construction techniques and aggregate particle sizes have different effects on the anti-skid performance and reduction of tire-road rolling resistance of the formed thin-layer pavement structure.
[0018] The anti-skid performance and tire-road rolling resistance of different thin-layer pavement structures were studied by using anti-skid aggregates with different particle sizes and different forming processes (rolling and non-rolling).
[0019] The test results show that in terms of pavement anti-skid performance, the thin-layer pavement structure with sand (0-0.5mm) has poor anti-skid performance and is rarely used in actual engineering projects; the anti-skid performance of the thin-layer pavement structure compacted with small-size aggregates (0.5-2mm) and large-size aggregates (2-8mm) is significantly lower than that of the thin-layer pavement structure with the same particle size that has not been compacted. This is consistent with the research results of Jiang Yongmao in "Research on Decision-making of Asphalt Pavement Anti-skid Recovery Technology Based on Road Surface Texture Characteristics".
[0020] In terms of tire-road rolling resistance, the tire-road rolling resistance of the thin-layer pavement structure with large-size aggregate (2-8mm) is significantly reduced after rolling. However, the effect of rolling on the tire-road rolling resistance of the thin-layer pavement structure with small-size aggregate (0.5-2mm) is not obvious; the tire-road rolling resistance of the thin-layer pavement structure with small-size aggregate but not rolled (0.5-2mm) is significantly lower than that of the thin-layer pavement structure with large-size aggregate rolled (2-8mm).
[0021] According to the research results, in order to achieve a balance between low rolling resistance and skid resistance of the pavement, it is necessary to use small-particle aggregate (0.5-2mm) and non-rolling molding technology. The small-particle epoxy asphalt seal layer just meets the above conditions.
[0022] Therefore, the present invention has the following advantages.
[0023] 1. Reduce the road-tire rolling resistance
[0024] Reshaping the road surface texture can reduce tire-road rolling resistance by more than 10%, saving more than 3% of energy consumption.
[0025] 2. Improve the anti-skid performance of the road surface
[0026] The road friction is increased by more than 50%, the swing value is stably maintained at more than 70BPN, and the lateral force coefficient (SFC) is stably maintained at more than 70.
[0027] 3. Balance between rolling resistance and anti-skid performance
[0028] It not only reduces the rolling resistance of the asphalt pavement, but also improves the anti-skid performance of the asphalt pavement.
[0029] 4. Rapid construction
[0030] Through sealing construction, it is used to quickly complete the maintenance (renovation) of the existing road surface and achieve low rolling resistance and high friction application performance of the road surface. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 Schematic diagram of negative texture pavement structure and positive texture pavement structure
[0032] Figure 2Grayscale images of pavement textures formed by different pavement structures (same scale)
[0033] From left to right: asphalt concrete pavement, the present invention, micro-surfacing, and chip seal
[0034] Figure 3 Schematic diagram of a thin-layer low rolling resistance road surface
[0035] Among them: 1—original road surface, 2—first epoxy asphalt seal layer, 3—second epoxy asphalt seal layer, 4—sealing layer. DETAILED DESCRIPTION
[0036] Example 1
[0037] like Figure 3 As shown, a thin layer of low rolling resistance pavement and a preparation method thereof are provided on the original pavement by a synchronous spreading (sprinkling) process from bottom to top to arrange a first epoxy asphalt seal layer, a second epoxy asphalt seal layer and a sealing layer; the original pavement, the first epoxy asphalt seal layer, the second epoxy asphalt seal layer and the sealing layer are arranged in sequence from bottom to top.
[0038] A thin-layer low rolling resistance pavement and a preparation method thereof comprises the following steps:
[0039] Step 1: Set the first epoxy asphalt seal layer on the asphalt concrete pavement; the first epoxy asphalt seal layer is prepared by a simultaneous spreading process of a binder and an anti-skid aggregate. The binder uses 0.6kg / ㎡ of water-based epoxy asphalt, and the anti-skid aggregate is corundum with a particle size of 1-2mm and a dosage of 1.5kg / ㎡.
[0040] Step 2: After the first layer of epoxy asphalt seal is dried and cured, start the construction of the second layer of epoxy asphalt seal; the second epoxy asphalt seal adhesive and anti-skid aggregate are prepared by a synchronous sprinkling (scattering) process, and the adhesive uses 0.6kg / ㎡ water-based epoxy asphalt; the anti-skid aggregate is selected from corundum, with a particle size of 1 to 1.5mm and a dosage of 1.4kg / ㎡.
[0041] Step 3: After the second layer of epoxy asphalt seal is dry and solidified, start the construction of the sealing layer; the sealing layer is prepared by spreading 0.5kg / ㎡ of water-based epoxy asphalt.
[0042] Example 2
[0043] like Figure 3 As shown, a thin layer of low rolling resistance pavement and a preparation method thereof are provided on the original pavement by a synchronous spreading (sprinkling) process from bottom to top to arrange a first epoxy asphalt seal layer, a second epoxy asphalt seal layer and a sealing layer; the original pavement, the first epoxy asphalt seal layer, the second epoxy asphalt seal layer and the sealing layer are arranged in sequence from bottom to top.
[0044] A thin-layer low rolling resistance pavement and a preparation method thereof comprises the following steps:
[0045] Step 1: Set the first epoxy asphalt seal layer on the asphalt concrete pavement; the first epoxy asphalt seal layer is prepared by a simultaneous spreading process of a binder and an anti-skid aggregate, and the binder uses 1.4kg / ㎡ of water-based epoxy asphalt; the anti-skid aggregate is selected as corundum, with a particle size of 1-2mm and a dosage of 2.8kg / ㎡.
[0046] Step 2: After the first layer of epoxy asphalt seal is dried and cured, start the construction of the second layer of epoxy asphalt seal; the second epoxy asphalt seal adhesive and anti-skid aggregate are prepared by a synchronous sprinkling (scattering) process, and the adhesive uses 1.2kg / ㎡ of water-based epoxy asphalt; the anti-skid aggregate is selected from corundum, with a particle size of 1 to 1.5mm and a dosage of 2.0kg / ㎡.
[0047] Step 3: After the second layer of epoxy asphalt seal is dry and solidified, the construction of the sealing layer begins; the sealing layer is prepared by spreading 0.8kg / ㎡ of water-based epoxy asphalt.
[0048] Example 3
[0049] like Figure 3 As shown, a thin layer of low rolling resistance pavement and a preparation method thereof are provided on the original pavement by a synchronous spreading (sprinkling) process from bottom to top to arrange a first epoxy asphalt seal layer, a second epoxy asphalt seal layer and a sealing layer; the original pavement, the first epoxy asphalt seal layer, the second epoxy asphalt seal layer and the sealing layer are arranged in sequence from bottom to top.
[0050] A thin-layer low rolling resistance pavement and a preparation method thereof comprises the following steps:
[0051] Step 1: Set the first epoxy asphalt seal layer on the asphalt concrete pavement with functional overlay; the first epoxy asphalt seal layer is prepared by a simultaneous spreading process of binder and anti-skid aggregate, and the binder uses 1.0kg / ㎡ of water-based epoxy asphalt; the anti-skid aggregate is basalt particles with a particle size of 1-2mm and a dosage of 2.2kg / ㎡.
[0052] Step 2: After the first layer of epoxy asphalt seal is dried and cured, the second layer of epoxy asphalt seal is constructed; the second epoxy asphalt seal adhesive and anti-skid aggregate are prepared by a synchronous spreading process, and the adhesive uses 1.0kg / ㎡ of water-based epoxy asphalt; the anti-skid aggregate is basalt particles with a particle size of 1 to 1.5mm and a dosage of 1.7kg / ㎡.
[0053] Step 3: After the second layer of epoxy asphalt seal is dry and solidified, the construction of the sealing layer begins; the sealing layer is prepared by spreading 0.7kg / ㎡ of water-based epoxy asphalt.
[0054] Example 4
[0055] like Figure 3As shown, a thin layer of low rolling resistance pavement and a preparation method thereof are provided on the original pavement by a synchronous spreading (sprinkling) process from bottom to top to arrange a first epoxy asphalt seal layer, a second epoxy asphalt seal layer and a sealing layer; the original pavement, the first epoxy asphalt seal layer, the second epoxy asphalt seal layer and the sealing layer are arranged in sequence from bottom to top.
[0056] A thin-layer low rolling resistance pavement and a preparation method thereof comprises the following steps:
[0057] Step 1: Set the first epoxy asphalt seal layer on the asphalt concrete pavement with functional overlay; the first epoxy asphalt seal layer is prepared by a simultaneous spreading process of binder and anti-skid aggregate, and the binder uses 0.5kg / ㎡ of oily epoxy asphalt; the anti-skid aggregate is basalt particles with a particle size of 1-2mm and a dosage of 2.2kg / ㎡.
[0058] Step 2: After the first layer of epoxy asphalt seal is dried and cured, start the construction of the second layer of epoxy asphalt seal; the second epoxy asphalt seal adhesive and anti-skid aggregate are prepared by a synchronous sprinkling (scattering) process, and the adhesive uses 0.5kg / ㎡ of oily epoxy asphalt; the anti-skid aggregate is corundum, with a particle size of 0.5-1mm and a dosage of 1.8kg / ㎡.
[0059] Step 3: After the second layer of epoxy asphalt seal is dry and solidified, start the construction of the sealing layer; the sealing layer is prepared by spreading 0.3kg / ㎡ of oily epoxy asphalt.
[0060] Example 5
[0061] like Figure 3 As shown, a thin layer of low rolling resistance pavement and a preparation method thereof are provided on the original pavement by a synchronous spreading (sprinkling) process from bottom to top to arrange a first epoxy asphalt seal layer, a second epoxy asphalt seal layer and a sealing layer; the original pavement, the first epoxy asphalt seal layer, the second epoxy asphalt seal layer and the sealing layer are arranged in sequence from bottom to top.
[0062] A thin-layer low rolling resistance pavement and a preparation method thereof comprises the following steps:
[0063] Step 1: Set the first epoxy asphalt seal layer on the asphalt concrete pavement with a seal layer; the first epoxy asphalt seal layer is prepared by a simultaneous spreading process of a binder and an anti-skid aggregate, and the binder uses 0.7kg / ㎡ of oily epoxy asphalt; the anti-skid aggregate is ceramic particles with a particle size of 1 to 2mm and a dosage of 2.8kg / ㎡.
[0064] Step 2: After the first layer of epoxy asphalt seal is dried and cured, the second layer of epoxy asphalt seal is constructed; the second epoxy asphalt seal adhesive and anti-skid aggregate are prepared by a simultaneous spreading process, with 0.6kg / ㎡ of oily epoxy asphalt used as the adhesive; basalt particles are selected as the anti-skid aggregate, with a particle size of 0.5-1mm and a dosage of 2.0kg / ㎡.
[0065] Step 3: After the second layer of epoxy asphalt seal is dry and solidified, start the construction of the sealing layer; the sealing layer is prepared by spreading 0.4kg / ㎡ of oily epoxy asphalt.
[0066] Example 6
[0067] like Figure 3 As shown, a thin layer of low rolling resistance pavement and a preparation method thereof are provided on the original pavement by a synchronous spreading (sprinkling) process from bottom to top to arrange a first epoxy asphalt seal layer, a second epoxy asphalt seal layer and a sealing layer; the original pavement, the first epoxy asphalt seal layer, the second epoxy asphalt seal layer and the sealing layer are arranged in sequence from bottom to top.
[0068] A thin-layer low rolling resistance pavement and a preparation method thereof comprises the following steps:
[0069] Step 1: Set the first epoxy asphalt seal layer on the asphalt concrete pavement with a seal layer; the first epoxy asphalt seal layer is prepared by a simultaneous spreading process of a binder and an anti-skid aggregate, and the binder uses 0.6kg / ㎡ of oily epoxy asphalt; the anti-skid aggregate is ceramic particles with a particle size of 1 to 2mm and a dosage of 2.5kg / ㎡.
[0070] Step 2: After the first layer of epoxy asphalt seal is dried and cured, start the construction of the second layer of epoxy asphalt seal; the second epoxy asphalt seal adhesive and anti-skid aggregate are prepared by a synchronous sprinkling (scattering) process, and the adhesive uses 1.0kg / ㎡ of water-based epoxy asphalt; the anti-skid aggregate is corundum, with a particle size of 0.5-1mm and a dosage of 1.8kg / ㎡.
[0071] Step 3: After the second layer of epoxy asphalt seal is dry and solidified, start the construction of the sealing layer; the sealing layer is prepared by spreading 0.6kg / ㎡ of water-based epoxy asphalt.
[0072] Example 7
[0073] like Figure 3 As shown, a thin layer of low rolling resistance pavement and a preparation method thereof are provided on the original pavement by a synchronous spreading (sprinkling) process from bottom to top to arrange a first epoxy asphalt seal layer, a second epoxy asphalt seal layer and a sealing layer; the original pavement, the first epoxy asphalt seal layer, the second epoxy asphalt seal layer and the sealing layer are arranged in sequence from bottom to top.
[0074] A thin-layer low rolling resistance pavement and a preparation method thereof comprises the following steps:
[0075] Step 1: Set the first epoxy asphalt seal layer on the asphalt concrete pavement; the first epoxy asphalt seal layer is prepared by a simultaneous spreading process of a binder and an anti-skid aggregate, and the binder uses 0.3kg / ㎡ of oily epoxy asphalt; the anti-skid aggregate is ceramic particles with a particle size of 1 to 1.5mm and a dosage of 1.5kg / ㎡.
[0076] Step 2: After the first layer of epoxy asphalt seal is dried and cured, start the construction of the second layer of epoxy asphalt seal; the second epoxy asphalt seal adhesive and anti-skid aggregate are prepared by a synchronous sprinkling (scattering) process, and the adhesive uses 0.6kg / ㎡ water-based epoxy asphalt; the anti-skid aggregate is selected from corundum, with a particle size of 1 to 1.5mm and a dosage of 1.4kg / ㎡.
[0077] Step 3: After the second layer of epoxy asphalt seal is dry and solidified, start the construction of the sealing layer; the sealing layer is prepared by spreading 0.5kg / ㎡ of water-based epoxy asphalt.
[0078] Example 8
[0079] like Figure 3 As shown, a thin layer of low rolling resistance pavement and a preparation method thereof are provided on the original pavement by a synchronous spreading (sprinkling) process from bottom to top to arrange a first epoxy asphalt seal layer, a second epoxy asphalt seal layer and a sealing layer; the original pavement, the first epoxy asphalt seal layer, the second epoxy asphalt seal layer and the sealing layer are arranged in sequence from bottom to top.
[0080] A thin-layer low rolling resistance pavement and a preparation method thereof comprises the following steps:
[0081] Step 1: Set the first epoxy asphalt seal layer on the asphalt concrete pavement with a seal layer; the first epoxy asphalt seal layer is prepared by a simultaneous spreading process of a binder and an anti-skid aggregate, and the binder uses 1.0kg / ㎡ of water-based epoxy asphalt; the anti-skid aggregate is ceramic particles with a particle size of 1 to 1.5mm and a dosage of 2.0kg / ㎡.
[0082] Step 2: After the first layer of epoxy asphalt seal is dried and cured, start the construction of the second layer of epoxy asphalt seal; the second epoxy asphalt seal adhesive and anti-skid aggregate are prepared by a synchronous sprinkling (scattering) process, and the adhesive uses 1.2kg / ㎡ of water-based epoxy asphalt; the anti-skid aggregate is selected from corundum, with a particle size of 1 to 1.5mm and a dosage of 1.6kg / ㎡.
[0083] Step 3: After the second layer of epoxy asphalt seal is dry and solidified, start the construction of the sealing layer; the sealing layer is prepared by spreading 0.3kg / ㎡ of oily epoxy asphalt.
[0084] Example 9
[0085] like Figure 3As shown, a thin layer of low rolling resistance pavement and a preparation method thereof are provided on the original pavement by a synchronous spreading (sprinkling) process from bottom to top to arrange a first epoxy asphalt seal layer, a second epoxy asphalt seal layer and a sealing layer; the original pavement, the first epoxy asphalt seal layer, the second epoxy asphalt seal layer and the sealing layer are arranged in sequence from bottom to top.
[0086] A thin-layer low rolling resistance pavement and a preparation method thereof comprises the following steps:
[0087] Step 1: Set the first epoxy asphalt seal layer on the asphalt concrete pavement; the first epoxy asphalt seal layer is prepared by a simultaneous spreading process of a binder and an anti-skid aggregate, and the binder uses 0.7kg / ㎡ of oily epoxy asphalt; the anti-skid aggregate is ceramic particles with a particle size of 1 to 1.5mm and a dosage of 2.5kg / ㎡.
[0088] Step 2: After the first layer of epoxy asphalt seal is dried and cured, start the construction of the second layer of epoxy asphalt seal; the second epoxy asphalt seal adhesive and anti-skid aggregate are prepared by a synchronous sprinkling (scattering) process, and the adhesive uses 1.2kg / ㎡ of water-based epoxy asphalt; the anti-skid aggregate is corundum, with a particle size of 1 to 1.5mm and a dosage of 1.8kg / ㎡.
[0089] Step 3: After the second layer of epoxy asphalt seal is dry and solidified, start the construction of the sealing layer; the sealing layer is prepared by spreading 0.4kg / ㎡ of oily epoxy asphalt.
[0090] Example 10
[0091] like Figure 3 As shown, a thin layer of low rolling resistance pavement and a preparation method thereof are provided on the original pavement by a synchronous spreading (sprinkling) process from bottom to top to arrange a first epoxy asphalt seal layer, a second epoxy asphalt seal layer and a sealing layer; the original pavement, the first epoxy asphalt seal layer, the second epoxy asphalt seal layer and the sealing layer are arranged in sequence from bottom to top.
[0092] A thin-layer low rolling resistance pavement and a preparation method thereof comprises the following steps:
[0093] Step 1: Set the first epoxy asphalt seal layer on the asphalt concrete pavement with functional overlay; the first epoxy asphalt seal layer is prepared by a simultaneous spreading process of binder and anti-skid aggregate, and the binder uses 0.5kg / ㎡ of oily epoxy asphalt; the anti-skid aggregate is ceramic particles with a particle size of 1 to 1.5mm and a dosage of 1.8kg / ㎡.
[0094] Step 2: After the first layer of epoxy asphalt seal is dried and cured, start the construction of the second layer of epoxy asphalt seal; the second epoxy asphalt seal adhesive and anti-skid aggregate are prepared by a synchronous spreading process, and the adhesive uses 0.5kg / ㎡ oily epoxy asphalt; the anti-skid aggregate is corundum, with a particle size of 0.5-1mm and a dosage of 1.7kg / ㎡.
[0095] Step 3: After the second layer of epoxy asphalt seal is dry and solidified, start the construction of the sealing layer; the sealing layer is prepared by spreading 0.6kg / ㎡ of water-based epoxy asphalt.
[0096] Embodiment 11
[0097] like Figure 3 As shown, a thin layer of low rolling resistance pavement and a preparation method thereof are provided on the original pavement by a synchronous spreading (sprinkling) process from bottom to top to arrange a first epoxy asphalt seal layer, a second epoxy asphalt seal layer and a sealing layer; the original pavement, the first epoxy asphalt seal layer, the second epoxy asphalt seal layer and the sealing layer are arranged in sequence from bottom to top.
[0098] A thin-layer low rolling resistance pavement and a preparation method thereof comprises the following steps:
[0099] Step 1: Set the first epoxy asphalt seal layer on the asphalt concrete pavement with functional overlay; the first epoxy asphalt seal layer is prepared by a simultaneous spreading process of binder and anti-skid aggregate, and the binder uses 1.0kg / ㎡ of water-based epoxy asphalt; the anti-skid aggregate is ceramic particles with a particle size of 1 to 1.5mm and a dosage of 2.5kg / ㎡.
[0100] Step 2: After the first layer of epoxy asphalt seal is dried and cured, start the construction of the second layer of epoxy asphalt seal; the second epoxy asphalt seal adhesive and anti-skid aggregate are prepared by a synchronous sprinkling (scattering) process, and the adhesive uses 1.1kg / ㎡ of water-based epoxy asphalt; the anti-skid aggregate is corundum, with a particle size of 0.5-1mm and a dosage of 1.8kg / ㎡.
[0101] Step 3: After the second layer of epoxy asphalt seal is dry and solidified, start the construction of the sealing layer; the sealing layer is prepared by spreading 0.3kg / ㎡ of oily epoxy asphalt.
[0102] Example 12
[0103] like Figure 3 As shown, a thin layer of low rolling resistance pavement and a preparation method thereof are provided on the original pavement by a synchronous spreading (sprinkling) process from bottom to top to arrange a first epoxy asphalt seal layer, a second epoxy asphalt seal layer and a sealing layer; the original pavement, the first epoxy asphalt seal layer, the second epoxy asphalt seal layer and the sealing layer are arranged in sequence from bottom to top.
[0104] A thin-layer low rolling resistance pavement and a preparation method thereof comprises the following steps:
[0105] Step 1: Set the first epoxy asphalt seal layer on the asphalt concrete pavement with a seal layer; the first epoxy asphalt seal layer is prepared by a simultaneous spreading process of a binder and an anti-skid aggregate, and the binder uses 0.9kg / ㎡ of water-based epoxy asphalt; the anti-skid aggregate is ceramic particles with a particle size of 1 to 1.5mm and a dosage of 1.8kg / ㎡.
[0106] Step 2: After the first layer of epoxy asphalt seal is dried and cured, start the construction of the second layer of epoxy asphalt seal; the second epoxy asphalt seal adhesive and anti-skid aggregate are prepared by a synchronous sprinkling (scattering) process, and the adhesive uses 0.5kg / ㎡ of oily epoxy asphalt; the anti-skid aggregate is corundum, with a particle size of 0.5-1mm and a dosage of 1.8kg / ㎡.
[0107] Step 3: After the second layer of epoxy asphalt seal is dry and solidified, start the construction of the sealing layer; the sealing layer is prepared by spreading 0.6kg / ㎡ of water-based epoxy asphalt.
[0108] Through application analysis and tracking detection of the above embodiments, the results show that the application life of a thin layer of low rolling resistance pavement of the present invention can be maintained for 3 to 5 years. During the entire life span, it can reduce tire-road rolling resistance by more than 10%, save energy consumption by more than 3%, and increase road friction by more than 50%.
Claims
1. A thin layer of low rolling resistance pavement, Its characteristics are: The invention comprises an original road surface (1), a first epoxy asphalt seal layer (2), a second epoxy asphalt seal layer (3) and a sealing layer (4); the original road surface (1), the first epoxy asphalt seal layer (2), the second epoxy asphalt seal layer (3) and the sealing layer (4) are laid in sequence from bottom to top, wherein the original road surface (1), the first epoxy asphalt seal layer (2) and the second epoxy asphalt seal layer (3) are laid by a synchronous sprinkling / spreading process; and the sealing layer (4) is laid by a sprinkling process; A method for preparing a thin layer of low rolling resistance pavement comprises the following steps: Step 1: Laying a first epoxy asphalt seal layer (2) on the original road surface (1) by using a synchronous sprinkling / spreading process; Step 2: After the first layer of epoxy asphalt seal (2) is dried and cured, a second layer of epoxy asphalt seal (3) is laid using a synchronous sprinkling / scattering process; Step 3: After the second layer of epoxy asphalt seal (3) is dried and cured, the sealing layer (4) is laid using a spreading process to complete the process; The first epoxy asphalt seal layer (2) is composed of a binder and an anti-skid aggregate, wherein the anti-skid aggregate is one of an anti-skid aggregate with a particle size of 1-2 mm or a particle size of 1-1.5 mm; the binder is 0.6-1.4 kg / m 2 Water-based epoxy asphalt or 0.3kg / m 2 The anti-skid aggregate is selected from one of the oily epoxy asphalts; the anti-skid aggregate is selected from one of the corundum, basalt particles, and ceramic particles, with a dosage of 1.5~2.8kg / m 2 ; The second epoxy asphalt seal layer (3) is composed of a binder and an anti-skid aggregate; wherein the anti-skid aggregate is one of an anti-skid aggregate with a particle size of 1 to 1.5 mm or a particle size of 0.5 to 1 mm; and the binder is 0.6 to 1.2 kg / m 2 Water-based epoxy asphalt or 0.3~0.6kg / m 2 The anti-skid aggregate is selected from one of the oily epoxy asphalts; the anti-skid aggregate is selected from one of the corundum, basalt particles, and ceramic particles, with a dosage of 1.4~2.0kg / m 2 ; Adopt non-rolling forming process; The sealing layer (4) is made of 0.5-0.8 kg / m 2 Water-based epoxy asphalt or 0.2~0.4kg / m 2 One of the oily epoxy asphalt.
2. A thin layer low rolling resistance pavement according to claim 1, Its characteristics are: The original road surface (1) is an asphalt concrete road surface or an asphalt concrete road surface with a seal layer or a functional overlay.
Citation Information
Patent Citations
Vibration molding-based method for design of mix proportion of graded broken stones
CN102021872A
Fine surface treatment method for double-layer spread type bituminous pavement
CN105421185A
Municipal road structure and construction method
CN109137668A
Epoxy modified cement pavement antiskid wearing layer and construction method thereof
CN113322743A
Rubber particle pavement seal coat with vibration reduction and noise reduction functions