A corrosion-resistant NdFeB thin sheet and preparation method thereof
Through secondary modification and surface treatment, the corrosion problem of NdFeB magnets in high salt spray and high humidity environments was solved, improving their corrosion resistance and magnetic properties, and enabling stable application in specific environments.
Patent Information
- Application Number
- CN202211012077.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-23
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-08-23
AI Technical Summary
Existing sintered NdFeB magnets are prone to corrosion in high salt spray and high humidity environments, which affects their application. Although the addition of nano-rare earth powder improves corrosion resistance, it reduces magnetic properties.
A two-stage modification process is adopted. First, metal nitrides are used to fill the pores and defects of NdFeB to increase its density. Then, silicon carbide and titanium carbide are used to improve the interfacial phase distribution. Combined with slow and fast cooling and surface coating treatment, a dense oxide film is formed to improve corrosion resistance and magnetic properties.
This improves the corrosion resistance and magnetic properties of NdFeB magnets, while maintaining or enhancing their mechanical properties and extending their service life.
Smart Images

Figure GDA0003852064820000061 
Figure GDA0003852064820000062 
Figure GDA0003852064820000063
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of magnet preparation, and more specifically, to a corrosion-resistant NdFeB sheet and a preparation method thereof. Background Art
[0002] Since the corrosion-resistant NdFeB thin sheets have the advantages of small size and high magnetic properties, their applications are widely used in aerospace, energy, medical and health, computers, communications and automobile industries. However, the corrosion resistance and temperature resistance of sintered NdFeB magnets are insufficient to a certain extent. On the one hand, sintered NdFeB magnets are composed of the main phase NdFeB phase and the intergranular Nd-rich phase. Due to the potential difference between the two phases, it is very easy to cause intergranular corrosion, which affects the use of NdFeB magnets in high salt fog and high humidity environments, so they are often limited to many applications. Therefore, it is particularly important to improve these properties.
[0003] Research has found that the corrosion resistance of NdFeB magnets is largely determined by the grain boundary conditions of the magnets. Therefore, the performance of magnets is improved by adding nano-rare earth and its alloys to the grain boundaries, so as to achieve the purpose of optimizing the corrosion resistance of materials in the laboratory. Nano-rare earth powder has strong activity and reacts with materials at the grain boundaries to form a stable grain boundary structure, so that the magnets maintain relatively ideal magnetic properties and make the distribution of neodymium-rich phases more ideal. During sintering, the potential difference between the main phase and the grain boundary can be reduced, thereby reducing the degree of corrosion.
[0004] However, the inventors found that during the industrial production of NdFeB magnets, due to the addition of nano rare earth powder, the interface structure was changed, the coercivity of the magnet was improved, but the remanence and maximum magnetic energy product were reduced. Although the corrosion resistance was improved, the ideal magnetic properties could not be maintained. Summary of the invention
[0005] In order to improve the corrosion resistance of NdFeB magnet sheets in industry and maintain or improve the magnetic properties, the present application provides a corrosion-resistant NdFeB sheet.
[0006] In the first aspect, the present application provides a corrosion-resistant NdFeB thin sheet using the following technical solution:
[0007] It is mainly made of NdFeB main alloy which is treated with the first modifier and the second modifier in sequence.
[0008] By weight, for every 100 parts of the NdFeB main alloy, the first modifier including the following components is added: 0.005-2 parts of AlN, 0.005-2 parts of ZrN, and 0.005-2 parts of VN;
[0009] The NdFeB main alloy is treated with the first modifier in sequence to obtain a first modified NdFeB alloy. By weight, for every 100 parts of the first modified NdFeB alloy, the second modifier comprising the following components is added: 0.005-1 part of SiC and 0.005-1 part of TiC.
[0010] By adopting the above technical solution, the crystal phase structure of NdFeB can be directionally changed.
[0011] Due to the doping of nano-level rare earth elements in the existing process, the order of the doping will lead to irregular crystal phase structure of NdFeB. Among them, metal nitride fills the pores and defects of NdFeB, which will increase the density and continuity of the magnet; adding a certain amount of silicon carbide and titanium carbide makes the distribution of the boundary phase more uniform and increases the contact area between the main phase grains. At the same time, titanium generally produces a specific new phase in the grain boundary area, thereby reducing the potential difference and increasing the corrosion resistance.
[0012] However, when metal nitrides and carbides are added at the same time in industrial production, a situation will occur where silicon carbide and titanium carbide will make the newly formed phase of the interface dense enough, and the metal nitride cannot fill the pores and defects of NdFeB. In the subsequent sintering process, the rare earth metal elements will be blocked, and finally the crystal structure will be irregular, and the ideal magnetic properties cannot be achieved.
[0013] In summary, through the secondary modification method, firstly, metal nitrides are used to fill the pores and defects of NdFeB to increase the density and continuity of the magnet. Secondly, the atomic magnetic moment of rare earth metal elements is large, and the existence of orbital magnetic moment makes the coupling between spin magnetic moment and orbital magnetic moment very strong, thereby improving the mechanical properties and magnetic properties of NdFeB magnets. Then, through silicon carbide and titanium carbide, the distribution of the boundary phase is more uniform, and new phases are generated between crystals, which improves the corrosion resistance of NdFeB. While silicon carbide and titanium carbide are doped, silicon and carbon have the effect of absorbing oxygen, and to a certain extent, they can also reduce the corrosion of NdFeB by oxygen. Silicon and carbon have the ability to combine with oxygen. Under the subsequent high-temperature process, combined with oxygen brought by the outside world, silicon dioxide increases the hardness of NdFeB crystals, and carbon dioxide takes away the oxygen content of NdFeB crystals, further improving the performance of the magnet.
[0014] Preferably, by weight, for every 100 parts of the NdFeB main alloy, the first modifier comprising the following components is added: 0.05-1.5 parts of AlN, 0.5-1.5 parts of ZrN, and 0.5-1.5 parts of VN.
[0015] By adopting the above technical solution, metal nitrides fill the pores and defects of NdFeB, which will increase the density and continuity of the magnet and improve the mechanical and magnetic properties of NdFeB magnets. However, a large amount of metal nitride doping forms a regular structure at the crystal surface, and there is an overlap of electron clouds between adjacent atoms, causing the valence electrons in this area to be localized, increasing the corrosion caused by the potential difference. Controlling the doping components of metal nitrides can improve the corrosion resistance of NdFeB.
[0016] Preferably, in parts by weight, for every 100 parts of the first modified NdFeB alloy, the second modifier comprising the following components is added: 0.05-0.2 parts of SiC and 0.1-0.35 parts of TiC.
[0017] By adopting the above technical solution, due to silicon carbide and titanium carbide, the distribution of the boundary phase is more uniform, and the contact area between the main phase grains is increased. However, a large increase in silicon carbide and titanium carbide will make the bonding ability between the grain boundaries worse, and the brittleness of NdFeB will increase. Controlling the doping components of silicon carbide and titanium carbide can increase corrosion resistance while avoiding the increase of brittleness as much as possible.
[0018] Preferably, in the first modifier, the average particle size of the AlN is 100-120 nm; the average particle size of the ZrN is 100-160 nm; and the average particle size of the VN is 100-160 nm.
[0019] By adopting the above technical solution, the average particle size range of nitrides can be differentiated, which can effectively fill the pores and defects in the NdFeB magnets and increase the mechanical and magnetic properties of NdFeB.
[0020] Preferably, the average particle size of the SiC in the first modifier is 60-100 nm; the average particle size of the TiC is 60-100 nm.
[0021] By adopting the above technical solution, the particle size of silicon carbide and titanium carbide particles is controlled within a certain range, which can not only make the distribution of the boundary phase more uniform and increase the contact area between the main phase grains, but also combine with the oxygen brought in by the outside world to further improve the magnetic properties of NdFeB.
[0022] On the other hand, the present application provides a method for preparing a corrosion-resistant NdFeB thin sheet, using the following technical solution:
[0023] Primary modification: weighing a set weight portion of the NdFeB main alloy and the first modifier, smelting to obtain a molten liquid, and then pouring it on a cooling roller for casting to obtain a primary modified NdFeB alloy;
[0024] Secondary modification: weighing a set weight portion of the second modifier and adding it to the primary modified NdFeB alloy for remelting, pouring the obtained molten liquid on a cooling roller for casting, and obtaining a secondary modified NdFeB alloy;
[0025] Hydrogen crushing and grinding: the secondary modified NdFeB alloy is subjected to hydrogen crushing treatment, and the obtained magnet powder is subjected to air flow milling treatment to obtain magnetic powder;
[0026] Pressing into sheets: placing the magnetic powder into a forming mold under an argon atmosphere to press into a blank sheet;
[0027] Diffusion sintering: The blank sheet is sintered in a nitrogen atmosphere to obtain a sintered NdFeB sheet.
[0028] Preferably, in the first modification step, a slow cooling method is adopted, and the rotation speed of the water-cooled roller is 10-30 m / s.
[0029] Preferably, in the secondary modification step, a rapid cooling method is adopted, and the rotation speed of the water-cooled roller is 30-50 m / s.
[0030] By adopting the above technical solution, the method of slow cooling in the first modification process can increase the density and continuity of the magnet. In the second modification process, the method of rapid cooling can inhibit the formation of α-Fe dendrites, and the dispersion of the grain boundary phase is good during the casting process. In addition, the corrosion resistance of NdFeB is improved.
[0031] Preferably, the method for preparing corrosion-resistant NdFeB further comprises the following steps:
[0032] Surface coating: a protective agent is coated on the surface of the sintered NdFeB thin slice, and after being irradiated by a high-current pulse electron beam, a NdFeB magnet thin slice is obtained;
[0033] By weight, every 100 parts of sintered NdFeB thin sheets are coated with the protective agent comprising the following components in weight: 0.005-0.05 parts of nano-grade aluminum powder and 0.005-0.03 parts of nano-grade chromium powder.
[0034] By adopting the above technical solution, the high-current pulsed electron beam irradiation treatment increases the density of grain boundaries. A large number of grain boundaries provide channels for metal atoms to diffuse to the metal surface, that is, more active Cr atoms and Al atoms participate in the diffusion of 0 2- The reaction promoted Cr 2 O 3 Oxide film and Al 2 O 3 The oxide film is formed, which greatly reduces the corrosion rate of NdFeB.
[0035] Preferably, in the step of surface coating, the high-current pulse electron beam acceleration voltage is 10-15 kV, the pulse current is 150-200 A, the pulse duration is 10-20 μs, the pulse frequency is 0.5-5 Hz, and the number of pulses is 10-20 times.
[0036] By adopting the above technical solution, the high-current pulsed electron beam treatment performs multiple pulse irradiations in a short period of time, so that the surface layer of the NdFeB material undergoes ultra-high-speed cooling and solidification, and the grains in the surface layer are refined to form ultra-fine grains. Grain refinement can increase the grain boundary density and promote the surface Cr 2 O 3 Passivation film and Al 2 O 3 The formation and adhesion of the passivation film reduces the composition difference between the grain boundaries and the bulk grains.
[0037] In summary, this application has the following beneficial effects:
[0038] 1. This application adopts secondary modification. First, metal nitrides are used to fill the pores and defects of NdFeB to increase the density and continuity of the magnet. Secondly, silicon carbide and titanium carbide are used to make the distribution of the boundary phase more uniform, and new phases are generated between crystals, so that the corrosion resistance of NdFeB is improved.
[0039] 2. In the present application, aluminum nitride, zirconium nitride and vanadium nitride are preferably used as the first modifier; silicon carbide and titanium carbide are used as the second modifier, because zirconium nitride and vanadium nitride as rare earth metal nitrides can fill the pores and defects of NdFeB, and the rare earth metals improve the magnetic properties of NdFeB; aluminum nitride can fill the pores and defects of NdFeB, and the aluminum element can improve the crystal structure; silicon carbide and titanium carbide can combine with oxygen to reduce the corrosion of NdFeB and improve the magnetic properties of NdFeB while making the distribution of the interface phase more uniform.
[0040] 3. The method of the present application increases the density and continuity of the magnet by adopting a slow cooling method in the first modification step and a fast cooling method in the second modification step, while improving the dispersion of the grain boundary phase, thereby improving the corrosion resistance of NdFeB.
[0041] 4. The method of the present application forms a dense Cr on the surface of a sintered NdFeB alloy coated with a protective agent by irradiating the sintered NdFeB alloy with a high current pulse electron beam. 2 O 3 Passivation film and Al 2 O 3 The passivation film greatly reduces the corrosion rate of NdFeB. DETAILED DESCRIPTION
[0042] The present application is further described in detail below with reference to the embodiments.
[0043] In order to improve the corrosion resistance of NdFeB magnets in industry and maintain or improve the magnetic properties, the present invention is obtained on this basis.
[0044] The present application is further described in detail below with reference to the embodiments.
[0045] The raw materials used in the examples are all commercially available.
[0046] Commercially available NdFeB main alloy: CAS number is 918106-59-9, purity ≥ 99% (including 33% neodymium, 64% iron, and 2% boron);
[0047] Aluminum nitride: CAS No. 24304-00-5, purity ≥ 99.5%, its particle size can be adjusted as needed, and this embodiment takes 110±10nm as an example for explanation;
[0048] Zirconium nitride: CAS number is 1306-38-3, purity ≥ 99.5%, and this embodiment is described by taking 130±30nm as an example;
[0049] Vanadium nitride: CAS number is 24646-85-3, purity is ≥99%, and this embodiment is described by taking 130±30nm as an example;
[0050] Silicon carbide: CAS number is 409-21-2, purity ≥ 99%, this embodiment is described by taking 80±20nm as an example;
[0051] Titanium carbide: CAS number is 12070-08-5, purity ≥ 99%, and this embodiment is described by taking 80±20nm as an example;
[0052] Nano-grade chromium powder: CAS number is 440-47-3, purity is ≥99%, and this embodiment is described by taking 50±10nm as an example;
[0053] Nano-grade aluminum powder: CAS number is 7429-90-5, purity is ≥99%, and this embodiment is described by taking 50±10 nm as an example.
[0054] Example
[0055] Example 1
[0056] A method for preparing a corrosion-resistant NdFeB thin sheet disclosed in Example 1 comprises the following steps:
[0057] Primary modification: Weigh 100kg of NdFeB main alloy, add 0.005kg of AlN, 0.005kg of ZrN, and 0.005kg of VN into a furnace for smelting, and obtain a molten liquid. Slowly cool the casting in a water-cooled roller, the water-cooled roller speed is 10m / s, and the casting thickness is 300μm, to obtain a primary modified NdFeB alloy;
[0058] Secondary modification: 100 kg of the primary modified NdFeB alloy was weighed, mixed with 0.005 kg of SiC and 0.005 kg of TiC, and put into a melting furnace for smelting. The obtained molten liquid was rapidly cooled in a water-cooled roller to form a casting sheet. The water-cooled roller speed was 30 m / s, and the casting sheet thickness was 300 μm, to obtain a secondary modified NdFeB alloy;
[0059] Hydrogen crushing and grinding: the obtained secondary modified NdFeB alloy is put into a hydrogen crushing furnace for hydrogen crushing treatment, evacuated to a vacuum degree of ≤1.5Pa, then hydrogen is introduced to a vacuum value of 0.3Mpa, hydrogen crushing treatment is performed for 3h, and cooled to room temperature to obtain magnet powder;
[0060] Airflow milling: The magnetic powder is passed through an airflow mill, and compressed air is filled into a nitrogen tank to obtain magnetic powder with a particle size of 3.0-4.5μm;
[0061] Pressing into tablets: The prepared magnetic powder is placed in a forming mold and pressed in a 3.0T pulse magnetic field under an argon atmosphere to obtain a density of 4.2g / cm 3 The NdFeB green body was then placed in an isostatic tablet press and pressed under 2800Mpa oil pressure to obtain a density of 4.5g / cm 3 The blank sheet;
[0062] Diffusion sintering: The blank thin slice is sintered in a nitrogen atmosphere using a spark plasma sintering furnace. The temperature is raised to 800°C at a heating rate of 80°C / min and the pressure is 60Mpa with a holding time of 60 minutes. After sintering, wait for the temperature of the vacuum sintering furnace to drop to room temperature to obtain corrosion-resistant NdFeB thin slices.
[0063] Surface coating: The sintered NdFeB thin slices are coated with a protective agent, the content of the protective agent is 0.005kg of nano-grade chromium powder; 0.005kg of nano-grade aluminum powder. The sintered NdFeB thin slices are irradiated with a strong pulse electron beam, with an acceleration voltage of 10kV, a pulse current of 150A, a pulse duration of 10μs, a pulse frequency of 0.5Hz, and a pulse number of 10 times. Corrosion-resistant NdFeB magnet thin slices are obtained.
[0064] Embodiment 26
[0065] Example 26 is based on the preparation method of Example 1, and the content of each component of the first modifier and the second modifier is adjusted.
[0066] The specific component adjustments of the above Example 16 are shown in Table 1 below, in units of kg.
[0067] Table 1. Raw material composition for the preparation of corrosion-resistant NdFeB thin sheets
[0068]
[0069] Embodiment 7-9
[0070] The difference between Examples 7-9 and Example 3 is that in the surface coating step, the components of the protective agent are different.
[0071] The specific component adjustments of the above Examples 7-9 are shown in Table 2 below, in kg.
[0072] Table 2. Components of protective agent for corrosion-resistant NdFeB thin sheets
[0073]
[0074] Examples 10-12
[0075] Examples 10-12 are optimized based on the raw material components of Example 8. The cooling speed is controlled by the roller speed in the two modification processes.
[0076] The specific component adjustments of the above Examples 10-12 are shown in Table 3 below.
[0077] Table 3. Optimization table of process modification of corrosion-resistant NdFeB thin sheets
[0078]
[0079]
[0080] Examples 13-15
[0081] Examples 13-15 are optimized on the raw material components of Example 11. In the surface coating step, the irradiation parameters of the high-current pulse electron beam are optimized.
[0082] The specific optimization conditions of the above-mentioned embodiments 13-15 are shown in Table 4 below.
[0083] Table 4. Optimization table of irradiation parameters of high-current pulsed electron beam
[0084]
[0085] Comparative Example
[0086] Comparative Example 1
[0087] The difference between Comparative Example 1 and Example 1 is that the first modifier and the second modifier are added at the same time.
[0088] Comparative Example 2
[0089] The difference between Comparative Example 2 and Example 1 is that the second modifier is added first and then the first modifier is added.
[0090] Comparative Example 3
[0091] The difference between Comparative Example 3 and Example 1 is that the first modifier is not added.
[0092] Comparative Example 4
[0093] The difference between Comparative Example 4 and Example 1 is that no second modifier is added.
[0094] Performance testing
[0095] Performance testing was performed on the NdFeB magnets provided in Examples 1-18 and Comparative Examples 1-4 of the present application.
[0096] 1. Resistance performance.
[0097] The NdFeB magnets were placed in a sealed box with a constant temperature set at 90°C and an oxygen concentration set at 50%, and the time when rust first appeared on the magnet surface was tested. The NdFeB magnets were subjected to a neutral salt spray test (NSS test) for metal covering layers according to the national standard GB / T10125-1997 to test the time when rust first appeared on the magnet surface.
[0098] 2. Magnetic properties
[0099] The magnetic properties of NdFeB magnets were tested according to the GB / T3217 permanent magnet (hard magnetic) material magnetic test method.
[0100] Table 5. Performance test data table
[0101]
[0102] The following describes the present application in detail in conjunction with the test data provided in Table 2.
[0103] In Examples 1-6, a comparison was made on the addition ratio of each component of the first modifier and the second modifier, and it was found that when the content of the first modifier was 0.8 weight part of AlN, 0.8 weight part of ZrN, and 0.8 weight part of VN per 100 weight parts of the NdFeB main alloy; and the content of the second modifier was 0.1 weight part of SiC and 0.2 weight part of TiC per 100 weight parts of the once-modified NdFeB alloy, the obtained NdFeB magnet had higher coercive force, remanence and maximum magnetic energy product while improving the corrosiveness.
[0104] Combined with Comparative Example 1, it is found that when the first modifier and the second modifier are added at the same time, the time when rust spots first appear on the NdFeB magnet at 90°C and the time when rust spots first appear under neutral salt spray are reduced, that is, adding them at the same time will make the NdFeB magnet more susceptible to corrosion; secondly, the coercive force, remanence and maximum magnetic energy product of the NdFeB magnet obtained by double modification will be higher.
[0105] Combining the analysis of Example 1 and Comparative Examples 1-2, when the second modifier is added first and then the first modifier is added, the time when the first rust spot appears on the NdFeB magnet at 90°C and the time when the first rust spot appears under neutral salt spray are reduced, and even lower than Comparative Example 1. This indicates that when silicon carbide and titanium carbide make the newly formed phase of the interface dense enough, the metal nitride cannot fill the pores and defects of the NdFeB.
[0106] Combining the analysis of Example 1 and Comparative Examples 3-4, it can be seen that the addition of the first modifier helps to increase the coercive force, remanence and maximum magnetic energy product of the NdFeB magnet; the addition of the second modifier helps to increase the corrosion resistance of the NdFeB magnet. In summary, Example 3 is better.
[0107] Table 6. Performance test data table
[0108]
[0109] It can be seen from Examples 7-10 and Table 6 that adding nano-sized chromium powder and nano-sized aluminum powder to the surface of the NdFeB magnet improves the corrosion resistance of the NdFeB magnet to a certain extent, and its magnetic properties are also improved. Example 8 is better.
[0110] Table 7. Performance test data table
[0111]
[0112] Combining Examples 11-14 and Table 7, it can be seen that in the modification process of the NdFeB magnet, slow cooling is used in the first modification step and rapid cooling is used in the second modification step, and the corrosion resistance of the obtained NdFeB magnet is significantly improved, and its magnetic properties are also improved. Example 12 is better.
[0113] Table 8. Performance test data table
[0114]
[0115]
[0116] It can be seen from Examples 15-18 and Table 8 that surface coating is performed in the final sintering step of the NdFeB magnet. The use of high-current pulsed electron beam irradiation as a coating process can more effectively improve the corrosion resistance and further optimize the performance of the NdFeB magnet than the existing secondary sintering. Example 16 is better.
[0117] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A corrosion-resistant NdFeB sheet, characterized in that: It is mainly made of NdFeB main alloy which is treated with the first modifier and the second modifier in sequence. In parts by weight, for every 100 parts of the NdFeB main alloy, the first modifier including the following components is added: 0.005-2 parts of AlN, 0.005-2 parts of ZrN, and 0.005-2 parts of VN; The NdFeB main alloy is treated with the first modifier in turn to obtain a first modified NdFeB alloy, and the second modifier comprising the following components in parts by weight is added to every 100 parts of the first modified NdFeB alloy: 0.005-1 part of SiC and 0.005-1 part of TiC; In the first modifier, the average particle size of AlN is 100-120 nm; the average particle size of ZrN is 100-160 nm; the average particle size of VN is 100-160 nm; In the second modifier, the average particle size of the SiC is 60-100 nm; the average particle size of the TiC is 60-100 nm; The method for preparing the corrosion-resistant NdFeB thin sheet comprises the following steps: Primary modification: weighing a set weight portion of the NdFeB main alloy and the first modifier, smelting to obtain a molten liquid, and then pouring it on a cooling roller for casting to obtain a primary modified NdFeB alloy; Secondary modification: weighing a set weight portion of the second modifier and adding it to the primary modified NdFeB alloy for remelting, pouring the obtained molten liquid on a cooling roller for casting, and obtaining a secondary modified NdFeB alloy; Hydrogen crushing and grinding: the secondary modified NdFeB alloy is subjected to hydrogen crushing treatment, and the obtained magnet powder is subjected to air flow milling treatment to obtain magnetic powder; Pressing into sheets: placing the magnetic powder into a forming mold under an argon atmosphere to press into a blank sheet; Diffusion sintering: The blank sheet is sintered in a nitrogen atmosphere to obtain a sintered NdFeB sheet.
2. The corrosion-resistant NdFeB sheet according to claim 1, characterized in that: By weight, for every 100 parts of the NdFeB main alloy, the first modifier including the following components is added: 0.05-1.5 parts of AlN, 0.5-1.5 parts of ZrN, and 0.5-1.5 parts of VN.
3. The corrosion-resistant NdFeB sheet according to claim 1, characterized in that: By weight, for every 100 parts of the first modified NdFeB alloy, the second modifier including the following components is added: 0.05-0.2 parts of SiC and 0.1-0.35 parts of TiC.
4. The corrosion-resistant NdFeB sheet according to claim 1, characterized in that: In the first modification step, a slow cooling method is adopted, and the rotation speed of the water-cooled roller is 10-30m / s.
5. The corrosion-resistant NdFeB sheet according to claim 1, characterized in that: In the secondary modification step, a rapid cooling method is adopted, and the rotation speed of the water-cooled roller is 30-50m / s.
6. The corrosion-resistant NdFeB sheet according to claim 1, characterized in that: The following steps are also included: Surface coating: a protective agent is coated on the surface of the sintered NdFeB thin slice, and after being irradiated by a high-current pulse electron beam, a NdFeB magnet thin slice is obtained; By weight, every 100 parts of sintered NdFeB thin sheets are coated with the protective agent comprising the following components in weight: 0.005-0.05 parts of nano-grade aluminum powder and 0.005-0.03 parts of nano-grade chromium powder.
7. The corrosion-resistant NdFeB sheet according to claim 6, characterized in that: In the step of surface coating, a strong pulse electron beam is used for irradiation bombardment with an acceleration voltage of 10-15 kV, a pulse current of 150-200 A, a pulse duration of 10-20 μs, a pulse frequency of 0.5-5 Hz, and a pulse number of 10-20 times.