A powder metallurgy pressing die processing technology and powder metallurgy pressing die

By first performing internal drilling and heat treatment in powder metallurgical pressing molds, the problems of uneven internal tissue and cracking in the mold in the prior art are solved, and split structures and alternative materials are used to achieve double improvements in mold cost and performance.

CN115365767BActive Publication Date: 2024-11-22SHANDONG TECHGONG GEOTECHN ENG EQUIP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211033450.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-26
Publication Date
2024-11-22
Estimated Expiration
2042-08-26

AI Technical Summary

Technical Problem

When the existing powder metallurgical pressing mold is pressed with large alloys, four to five tempering is required to eliminate the internal stress of the Cr12MoV mold material due to its large shape and volume, resulting in uneven internal tissue and local cracking may occur, which increases production cost and processing time. .

Method used

Drill the inside of the mold first, then heat treatment and 2-3 tempering. After changing the process, only 2-3 tempering is required to eliminate the internal stress of the material. The upsurge of the split structure is used, and 45# steel or 42CrMo material replaces part of Cr12MoV material, reducing the specific mold accumulation and processing time.

Benefits of technology

It achieves the uniformity of the internal tissue of the mold and the perfect heat treatment effect, reduces the use of Cr12MoV materials, reduces the price and processing time of the mold, and improves market competitiveness and product performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115365767B_ABST
    Figure CN115365767B_ABST
Patent Text Reader

Abstract

The present invention proposes a powder metallurgy pressing die processing technology and a powder metallurgy pressing die, step 1: punching holes inside the integral blank die; step 2: heat treating the integral blank die after step 1; step 3: tempering the integral blank die after step 2; step 4: wire-cutting the integral blank die after step 3. The die body is first drilled inside the material, and then heat-treated. After the internal holes are punched, the die body volume is reduced, and the internal structure conversion is more uniform during heat treatment. After changing the process, only 2-3 temperings are needed to eliminate the internal stress of the material, avoiding the phenomenon of local cracking of the material during processing on the online cutting wire.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field related to powder metallurgy, and in particular relates to a powder metallurgy pressing die processing technology and a powder metallurgy pressing die. Background Art

[0002] The statements in this section merely provide background information related to the present invention and do not necessarily constitute prior art.

[0003] The pressing and molding of products in the field of powder metallurgy requires molds. When large pieces of alloy are pressed (cross-sectional area greater than 100 square centimeters), the cost of designing and making the materials and manufacturing process of the mold will greatly increase the production cost of the product.

[0004] The existing powder metallurgy pressing mold is heat treated as a whole blank during processing. Due to its large shape and volume, it needs four to five tempering to eliminate the internal stress of the Cr12MoV mold material and make the internal structure uniform. If the internal structure is uneven, the slow-feeding wire cutting equipment will have local cracking when processing the mold forming cavity, which will cause the mold to be scrapped.

[0005] In addition, the existing powder metallurgy pressing mold is an integral Cr12MoV upper punch, which increases the processing time of the wire cutting equipment, and the overall use of Cr12MoV material causes the overall price of the powder pressing mold to increase. Summary of the invention

[0006] In order to overcome the shortcomings of the above-mentioned prior art, the present invention provides a powder metallurgy pressing mold processing process and a powder metallurgy pressing mold. The mold body is first drilled inside the material and then heat treated. After the internal drilling, the volume of the mold body is reduced, and the internal structure conversion is more uniform during heat treatment. After the process is changed, only 2-3 temperings are needed to eliminate the internal stress of the material, avoiding the phenomenon of local cracking of the material during processing on slow-feeding wire cutting equipment, so that the heat treatment effect of the position that needs to be processed and cut perfectly meets the original process requirements.

[0007] To achieve the above objectives, one or more embodiments of the present invention provide the following technical solutions: A powder metallurgy pressing die processing process, comprising:

[0008] Step 1: Punch holes inside the overall blank mold;

[0009] Step 2: heat treating the integral blank mold processed in step 1;

[0010] Step 3: Tempering the integral blank mold processed in step 2;

[0011] Step 4: Perform wire cutting on the overall blank mold processed in step 3.

[0012] A second aspect of the present invention provides a powder metallurgy pressing die, characterized in that it includes a die body and an upper punch for pressing, and the upper punch is a split structure.

[0013] One or more of the above technical solutions have the following beneficial effects:

[0014] In the present invention, holes are first drilled inside the mold and then heat treated. After the internal holes are drilled, the volume of the mold is reduced, and the internal structure conversion is more uniform during heat treatment. After changing the process, only 2-3 temperings are needed to eliminate the internal stress of the material, avoiding local cracking of the material during processing on slow-feed wire cutting equipment, so that the heat treatment effect of the position that needs to be processed and cut perfectly meets the original process requirements.

[0015] In the present invention, the existing integral upper punch structure is changed into a split structure, the upper part of the upper punch is made of 45# steel or 42CrMo, and the lower part is made of Cr12MoV, which effectively reduces the use of Cr12MoV material, reduces the mold price, and increases the market competitiveness of the product. In addition, when the wire is cut slowly, only the lower part of the upper punch needs to be processed, which reduces the processing time of the wire cutting equipment.

[0016] Advantages of additional aspects of the present invention will be given in part in the following description, and in part will become obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0018] Figure 1 This is a schematic diagram of drilling holes before heat treatment of the mold in Example 1 of the present invention;

[0019] Figure 2 is an overall schematic diagram of the mold drilling in the first embodiment of the present invention;

[0020] Figure 3 The cross section of the die body and the upper punch in the second embodiment of the present invention is a schematic diagram;

[0021] Figure 4 It is an overall schematic diagram of the mold body and the upper punch in the second embodiment of the present invention.

[0022] Description of the drawings: 1. Hole position; 2. Cutting outer ring; 3. Upper part of the upper punch; 4. Lower part of the upper punch; 5. Die body; 6. Bolts DETAILED DESCRIPTION

[0023] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0024] It should be noted that the terms used herein are for describing specific embodiments only and are not intended to be limiting of exemplary embodiments according to the present invention.

[0025] In the absence of conflict, the embodiments of the present invention and the features of the embodiments may be combined with each other.

[0026] Embodiment 1

[0027] like Figure 1-Figure 2 As shown, this embodiment discloses a powder metallurgy pressing die processing process, comprising:

[0028] Step 1: Punch holes inside the overall blank mold;

[0029] Step 2: heat treating the integral blank mold processed in step 1;

[0030] Step 3: Tempering the integral blank mold processed in step 2;

[0031] Step 4: Perform wire cutting on the overall blank mold processed in step 3.

[0032] In this embodiment, the holes inside the whole blank are cut off before heat treatment, and then heat treatment is performed. After the holes are punched inside the whole blank, the volume of the mold body is reduced, and the internal structure conversion is more uniform during heat treatment, which can eliminate the internal stress of the material and avoid the phenomenon of local cracking of the material during processing by slow-feeding wire cutting equipment.

[0033] In step 1 of this embodiment, multiple holes 1 are set inside the integral blank according to the size of the die cavity of the pressing die, and the cutting outer ring 2 formed by the multiple holes is adapted to the size of the die cavity of the pressing die. By pre-drilling the interior of the integral blank, the volume of the integral blank is reduced.

[0034] In step 2 of this embodiment, the integral blank after the treatment in step 1 is subjected to heat treatment, and the heat treatment conditions are:

[0035] The mold blank undergoes double refinement preparatory heat treatment to improve defects such as metal segregation, eutectic carbide corner rounding, and uniformly refine the round material grains. The specific steps are as follows

[0036] ① High temperature quenching: First, preheating is carried out before heating to the temperature, that is, two-stage preheating at 600℃ for 135 minutes and 830℃ for 90 minutes; then 1130℃ for 100 minutes, then oil cooling (oil temperature 50℃) for 15 minutes, and finally high temperature tempering at 720℃ for 4 hours and air cooling.

[0037] ② Low temperature quenching: first preheat to the temperature before heating, that is, two-stage preheating at 600℃ for 135 minutes and 830℃ for 90 minutes; then keep at 960℃ for 90 minutes, then oil cool (temperature 50℃) for 15 minutes, and finally high temperature tempering at 720℃ for 4 hours and air cool.

[0038] Then the mold is subjected to conventional quenching and cryogenic treatment, and then 2-3 tempering treatments in step 3 are added to improve the mold strength, toughness, wear resistance, eliminate stress, and stabilize the structural properties. The specific steps are as follows:

[0039] ① Quenching process: preheating before heating to the temperature, that is, two-stage preheating at 600℃ for 140 minutes and 830℃ for 90 minutes, then 1040℃ for 75 minutes, oil cooling (oil temperature 60℃) for 10 minutes, and then slowly cooling to room temperature after taking out of the furnace.

[0040] ② Cryogenic treatment: Place the quenched and slowly cooled mold into a cryogenic device, reduce the temperature to -130°C at a rate of 2°C / min, keep warm for 60 minutes, then open the box and air cool to room temperature.

[0041] In step 3 of this embodiment, the whole blank after the treatment in step 2 is tempered 2-3 times, and the tempering conditions are:

[0042] ①Put the deep-cold treated mold into a tempering furnace (the temperature inside the furnace is at room temperature), heat it to 500°C at a rate of 5°C / min, keep it warm for 180 minutes, then take it out of the furnace and air-cool it to room temperature, and then repeat the tempering according to the above process.

[0043] ② Keep the mold after two tempering at 400℃ for 6 hours and then take it out of the furnace and cool it slowly.

[0044] After the above heat treatment process, the hardness of Cr12MoV mold is HRC59-62, and the metallographic structure is: fine needle tempered martensite + rounded eutectic carbide + evenly distributed granular secondary carbide + a small amount of residual austenite, grain size 10-11, and uniform structure. Such a state of organization will further curb the cracking of materials in the subsequent slow wire cutting process.

[0045] In step 4 of this embodiment, the whole blank processed in step 3 is subjected to wire cutting, and the wire cutting wire cuts the outer ring 2 formed by the plurality of holes. The conditions of the wire cutting equipment are:

[0046] The slow wire cutting method adopts the cutting method of cutting one and repairing two (cutting according to the normal parameters of the machine tool)

[0047] One cutter: Current 15A Wire speed 1.22mm / min

[0048] Second knife: current 11A wire speed 3.72mm / min

[0049] Three knives: current 3A wire speed 1.22mm / min

[0050] Embodiment 2

[0051] like Figure 3-Figure 4 As shown, this embodiment provides a powder metallurgy pressing die, including a die body 5 and an upper punch for pressing, wherein the upper punch is a split structure.

[0052] The existing upper punch is a Cr12MoV overall structure. In this embodiment, the upper punch is divided into two parts, the upper part 3 is made of 45# steel or 42CrMo, and the lower part 4 is made of Cr12MoV. The use of Cr12MoV material is reduced, and only the Cr12MoV part of the lower part of the upper punch needs to be processed, and the outline of the Cr12MoV part of the upper punch bottom is cut out by slow-moving wire cutting. Due to the small height, small wire cutting area, high efficiency, and reduced processing time of slow-moving wire cutting equipment, the mold price is reduced, and the market competitiveness of the product is increased.

[0053] In this embodiment, the upper part is made of 345# steel or 42CrMo material after heat treatment, and the upper part and the lower part are fixed by bolts 6. Specifically, the upper part and the lower part of the upper punch can be fixedly connected by 12.9 grade bolts.

[0054] In this embodiment, the cross-sectional size of the upper punch lower portion 4 is adapted to the size of the pressing cavity of the die body 6, so as to enable the upper punch to be pressed into the pressing cavity of the die body to press the powder metallurgy in the cavity.

[0055] Although the above describes the specific implementation mode of the present invention in conjunction with the accompanying drawings, it is not intended to limit the scope of protection of the present invention. Those skilled in the art should understand that various modifications or variations that can be made by those skilled in the art on the basis of the technical solution of the present invention without creative work are still within the scope of protection of the present invention.

Claims

1. A powder metallurgy pressing die processing process, characterized in that: include: Step 1: Punch holes inside the overall blank mold; Step 2: heat treating the integral blank mold processed in step 1; Step 3: Tempering the integral blank mold processed in step 2; Step 4: Perform wire cutting on the overall blank mold processed in step 3; In the step 1, a plurality of holes are punched inside the integral blank mold, and the outer ring formed by the plurality of holes is a pressing mold cavity of a powder metallurgy pressing mold; the mold material is Cr12MoV; In step 2, the heat treatment conditions are: High temperature quenching: 600℃ holding time for 135 minutes, 830℃ holding time for 90 minutes for two-stage preheating, then 1130℃ holding time for 100 minutes, then oil cooling at 50℃ for 15 minutes, then high temperature tempering at 720℃ for 4 hours, air cooling; Low temperature quenching: 600℃ holding time for 135 minutes, 830℃ holding time for 90 minutes for two-stage preheating, then 960℃ holding time for 90 minutes, oil cooling at 50℃ for 15 minutes, then high temperature tempering at 720℃ for 4 hours, air cooling; After the heat treatment, the mold is also subjected to conventional quenching and cryogenic treatment, specifically: Conventional quenching: first preheat at 600℃ for 140 minutes, then at 830℃ for 90 minutes, then at 1040℃ for 75 minutes, then oil cool at 60℃ for 10 minutes, finally take out of the furnace and slowly cool to room temperature; Cryogenic treatment: put the mold after quenching and slow cooling into a cryogenic device, cool it to -130℃ at a rate of 2℃ / min, keep it warm for 60 minutes, then open the box and air cool it to room temperature; In step 3, 2-3 temperings are performed, and the tempering conditions are: The mold after deep freezing treatment is placed in a tempering furnace, and the temperature is raised to 500℃ at a rate of 5℃ / min. After keeping warm for 180 minutes, it is taken out of the furnace and air-cooled to room temperature. The tempering is repeated according to the above tempering process. After tempering, the mold is kept at 400℃ for 6 hours and then taken out of the furnace and slowly cooled.

2. A powder metallurgy pressing die processing process as claimed in claim 1, characterized in that: In step 4, the wire is slowly threaded along the outer circle formed by the plurality of holes.

3. A powder metallurgy pressing die processing process as claimed in claim 1, characterized in that: In step 4, the wire cutting is performed by cutting one and trimming two.

4. A powder metallurgy pressing die manufactured by the powder metallurgy pressing die manufacturing process according to any one of claims 1 to 3, characterized in that: It comprises a die body and an upper punch for pressing, wherein the upper punch is a split structure.

5. A powder metallurgy pressing die as claimed in claim 4, characterized in that: The upper punch is divided into two parts, the upper part is made of 45# steel or 42CrMo material, and the lower part is made of Cr12MoV material.

6. A powder metallurgy pressing die as claimed in claim 5, characterized in that: The upper part is made of 45# steel or 42CrMo material and is heat treated, and the upper part and the lower part are fixed by bolts.