A carboxyl-containing compound with triazine as skeleton and its preparation method and application
By using a carboxyl-containing compound with triazine as the skeleton as an adhesion accelerator in the Mini LED encapsulant, the problem of insufficient bonding performance of the encapsulant is solved, and the adhesive force and temperature resistance of the base material are significantly improved, meeting the requirements Mini LED packaging needs.
Patent Information
- Application Number
- CN202211198387.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-29
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2042-09-29
AI Technical Summary
The bonding performance of existing Mini LED encapsulation adhesives is insufficient and difficult to meet the requirements of Mini LED encapsulation. In particular, the adhesion to the substrate and temperature resistance are defective, resulting in reduced production yield and yellowing problems.
A carboxyl-containing compound with a triazine skeleton is used as an adhesion promoter, prepared through the reaction of succinic anhydride, hydrogen-containing siloxane and isocyanurate, and added to the encapsulant to improve adhesion and temperature resistance. performance.
Significantly improves the adhesion between the encapsulant and the substrate, improves the bonding strength to a variety of metal and glass substrates, prolongs high temperature stability, reduces yellowing, and maintains the light transmittance of the encapsulant and molding effects.
Smart Images

Figure CN115368397B
Abstract
Description
Technical Field
[0001] The invention belongs to the field of organic silicon adhesion promoters, and specifically relates to a carboxyl-containing compound with triazine as a skeleton, and a preparation method and application thereof. Background Art
[0002] In recent years, as one of the countries with the most potential in the global electronics industry, China has been increasingly using Mini LED packaging technology in terminal fields such as televisions, monitors, wearable devices, and in-vehicle displays. The main reason is that traditional display technologies such as LCD and OLED are gradually unable to meet the rapid development of the market. Technically, the advantages of Mini LED backlight display are high-definition display, long service life, and lower cost than OLED; in terms of process, Mini LED backlight process is relatively simple, with low production difficulty, and can be quickly put into production, filling the gap in high-definition display screens in the current market.
[0003] Mini LED encapsulation glue is one of the core materials in the packaging process, so it is required to have good light transmittance, thermal stability, yellowing resistance and air tightness. The two most commonly used types of Mini LED encapsulation glue on the market are epoxy resin and silicone resin. Among them, epoxy resin has high curing hardness and good air tightness, but its defects are also obvious. Epoxy resin has slightly poor temperature resistance, is prone to yellowing after long-term use, and has large curing stress, which can easily lead to a decrease in production yield. Silicone resin overcomes the shortcomings of epoxy resin and has obvious advantages in temperature resistance, yellowing resistance, and curing stress, but silicone resin itself has poor adhesion and is difficult to meet the requirements of the packaging process.
[0004] At present, in order to improve the bonding performance of silicone encapsulation glue, an appropriate amount of adhesion promoter is usually added to it. However, on the substrate of Mini LED, the existing adhesion promoter does not have a significant adhesion promoting effect during use and cannot meet normal packaging requirements. Therefore, the bonding performance of silicone resin encapsulation glue has become a bottleneck restricting its application in Mini LED packaging. Summary of the invention
[0005] In order to solve the shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide a method for preparing a carboxyl-containing compound with triazine as a skeleton.
[0006] Another object of the present invention is to provide a carboxyl-containing compound with triazine as the skeleton obtained by the above preparation method.
[0007] Another object of the present invention is to provide the application of the above-mentioned carboxyl-containing compound with triazine as the skeleton in Mini LED silicone encapsulation adhesive. The adhesion promoter is applied to Mini LED silicone encapsulation adhesive to improve the adhesion between the encapsulation adhesive and the substrate, and after the encapsulation adhesive is cured, it can still maintain a good bonding effect.
[0008] The purpose of the present invention is achieved through the following technical solutions:
[0009] A method for preparing a carboxyl-containing compound with triazine as a skeleton comprises the following steps:
[0010] (1) Succinic anhydride, hydrogen-containing siloxane and an organic solvent are mixed, the temperature is raised to 50-90° C., a catalyst is added, the reaction is carried out for 2-8 hours, and low-boiling substances are removed to obtain an intermediate;
[0011] (2) The intermediate, isocyanurate and organic solvent are mixed, the temperature is raised to 50-80° C., a catalyst is added to react for 2-8 hours, and low-boiling substances are removed to obtain a carboxyl-containing compound with triazine as the skeleton.
[0012] Preferably, the succinic anhydride described in step (1) is at least one of allyl succinic anhydride, butenyl succinic anhydride, pentenyl succinic anhydride, hexenyl succinic anhydride, heptenyl succinic anhydride, octenyl succinic anhydride, nonenyl succinic anhydride, decenyl succinic anhydride, dodecenyl succinic anhydride, pentadecenyl succinic anhydride, octadecenyl succinic anhydride, and the like.
[0013] Preferably, the hydrogen-oxygen siloxane in step (1) is at least one of tetramethyldisiloxane, tetramethylcyclotetrasiloxane, dimethyldiphenyldisiloxane, etc.;
[0014] The isocyanurate in step (2) is at least one of triallyl isocyanurate, diallyl isocyanurate, allyl isocyanurate, etc.;
[0015] The organic solvent in steps (1) and (2) is at least one of toluene, xylene, cyclohexane and methylcyclohexane; and the catalyst is at least one of platinum, palladium and rhodium and their complexes.
[0016] Preferably, the catalyst in steps (1) and (2) is at least one of chloroplatinic acid and 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum; the amount of the catalyst in step (1) is 30-100 ppm of the mass of the reactants in step (1); and the amount of the catalyst in step (2) is 20-80 ppm of the mass of the reactants in step (2).
[0017] Preferably, the molar ratio of succinic anhydride to hydrogen-containing siloxane in step (1) is 1:(1-1.2), more preferably 1:(1-1.1);
[0018] The molar ratio of the intermediate to isocyanurate in step (2) is 1:(1-1.2), more preferably 1.1.
[0019] Preferably, the structural formula of the intermediate is as follows:
[0020]
[0021] Preferably, the reaction time of steps (1) and (2) is 4 to 5 hours.
[0022] The reaction temperature in step (1) is 80-90°C, and the reaction temperature in step (2) is 70-80°C;
[0023] The conditions for removing low boiling points in steps (1) and (2) are: adding activated carbon for adsorption filtration, the vacuum degree is -0.06-0.09 MPa, and the temperature is 120-130°C.
[0024] Preferably, the catalyst is added dropwise in steps (1) and (2).
[0025] A carboxyl-containing compound with triazine as the skeleton is obtained by the above-mentioned preparation method.
[0026] A carboxyl-containing compound with triazine as the skeleton, the structural formula is as follows:
[0027]
[0028] Application of a carboxyl-containing compound with triazine as the skeleton in Mini LED silicone encapsulation adhesive.
[0029] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0030] 1. The present invention provides a carboxyl-containing compound with triazine as the skeleton, wherein the carboxyl group is introduced into the triazine structure as the skeleton, wherein the triazine structure is stable at high temperature and UV-resistant, which effectively improves the temperature resistance of the Mini LED encapsulation adhesive and reduces the yellowing caused by high-temperature aging.
[0031] 2. After adding the adhesion promoter prepared by the present invention, the hardness, transmittance and molding effect of the encapsulation glue remain basically unchanged, the adhesion to the bonding substrate is significantly improved, the shear force on the aluminum substrate is increased by 125-355%, and the shear force on the glass plate is increased by 56-463%. The carboxyl-containing compound with triazine as the skeleton prepared by the present invention includes carbonyl, vinyl / hydrogen, carboxyl and other active groups in the structure. When it is added to the Mini LED encapsulation glue together with the epoxy type adhesion promoter, it can promote the opening of the epoxy group, which can greatly improve the Mini LED encapsulation glue to a variety of metals (aluminum, copper, stainless steel) and electronic plastic substrates, polyimide (PI), printed circuit boards (PCB)) and glass substrates. It has a wider range of applications than existing adhesives and can meet the use of most Mini LED substrates and electronic devices.
[0032] 3. The carboxyl-containing compound with triazine as the skeleton prepared by the present invention has good compatibility with the system and will not affect its light transmittance because it contains a siloxane structure similar to the packaging glue.
[0033] 4. The carboxyl-containing compound with triazine as the skeleton prepared by the present invention has a simple and easy-to-control synthesis process, a yield of up to 98%, and is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is the H NMR spectrum of the compound obtained in Example 1. DETAILED DESCRIPTION
[0035] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto. For process parameters not particularly specified, conventional techniques can be used. The raw materials involved in the present invention are all common commercially available products unless otherwise stated.
[0036] Example 1
[0037] (1) In a three-necked flask, 140 g (1 mol) of allyl succinic anhydride, 147.4 g (1.1 mol) of tetramethyldisiloxane and 205.5 g of toluene were added, the temperature was raised to 80° C., 82.2 g of a toluene solution of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum (the platinum content in the toluene solution was 100 ppm) was added dropwise, the reaction was maintained for 4 hours, activated carbon was added to remove the platinum catalyst by adsorption, and then filtered, and low boiling substances were removed at a vacuum degree of -0.06-0.09 MPa and a temperature of 120-130° C. to obtain 268 g of intermediate 1, with a yield of 97.81%;
[0038] In a three-necked flask, 274 g (1 mol) of intermediate 1, 249 g (1 mol) of triallyl isocyanurate and 418.4 g of toluene were added, the temperature was raised to 70°C, 104.6 g of a toluene solution of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum (the platinum content in the toluene solution was 100 ppm) was added dropwise, the reaction was maintained for 4 hours, activated carbon was added to remove the platinum catalyst by adsorption, and then filtered, and low boiling materials were removed at a vacuum degree of -0.06-0.09 MPa and a temperature of 120-130°C to obtain 518 g of a carboxyl-containing compound 1 with a triazine skeleton, with a yield of 99.04%.
[0039] (2) Preparation of silicone encapsulation samples for Mini LED
[0040] 65 parts by mass of a vinylphenyl silicone resin with a viscosity of 80000 mPa·s and a vinyl content of 4.5 wt%, 25 parts by mass of a vinylphenyl silicone oil with a viscosity of 4000 mPa·s and a vinyl content of 0.32 wt%, 10 parts by mass of a hydrogen-containing phenyl silicone oil with an active hydrogen content of 0.57 wt%, 2 parts by mass of compound 1 and 0.01 parts by mass of 1-ethynyl-1-cyclohexanol were mixed uniformly in a high-speed centrifuge (1200 rpm), and then 0.08 parts by mass of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum (platinum content 5000 ppm) catalyst and 3.5 parts by mass of fumed silica were added, mixed uniformly, vacuum degassed, cured at 90°C for 1 hour and at 150°C for 3-4 hours. The sample properties are shown in Table 2.
[0041] Example 2
[0042] (1) In a three-necked flask, 140 g (1 mol) of allyl succinic anhydride, 264 g (1.1 mol) of tetramethylcyclotetrasiloxane and 990 g of toluene were added, the temperature was raised to 80° C., 114 g of a toluene solution of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum (the platinum content in the toluene solution was 100 ppm) was added dropwise, the reaction was maintained for 4 hours, activated carbon was added to remove the platinum catalyst by adsorption, and then filtered, and low boiling substances were removed at a vacuum degree of -0.06--0.09 MPa and a temperature of 120-130° C. to obtain 373 g of intermediate 2, with a yield of 98.16%;
[0043] In a three-necked flask, 380 g (1 mol) of intermediate 2, 249 g (1 mol) of triallyl isocyanurate and 503.2 g of toluene were added. The temperature was raised to 70°C, and 125.8 g of a toluene solution of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum (the platinum content in the toluene solution was 100 ppm) was added dropwise. The reaction was maintained for 4 hours, and activated carbon was added for adsorption and filtration. Low boiling materials were removed at a vacuum degree of -0.06--0.09 MPa and a temperature of 120-130°C to obtain 621 g of a carboxyl-containing compound 2 with a triazine skeleton, with a yield of 98.73%.
[0044] (2) Preparation of silicone encapsulation samples for Mini LED
[0045] The preparation method of the Mini LED silicone encapsulation adhesive sample in this embodiment is basically the same as that in Example 1, except that Compound 1 in Example 1 is changed to Compound 2. The sample performance is shown in Table 2.
[0046] Example 3
[0047] (1) 210 g (1 mol) of octenylsuccinic anhydride, 147.4 g (1.1 mol) of tetramethyldisiloxane and 254.2 g of toluene were added to a three-necked flask, the temperature was raised to 80° C., 103.2 g of a toluene solution of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum (the platinum content in the toluene solution was 100 ppm) was added dropwise, the reaction was maintained for 4 hours, activated carbon was added for adsorption and filtration, and low boiling substances were removed at a vacuum degree of -0.06-0.09 MPa and a temperature of 120-130° C. to obtain 334 g of intermediate 3, with a yield of 97.03%;
[0048] In a three-necked flask, 344 g (1 mol) of intermediate 2, 249 g (1 mol) of triallyl isocyanurate and 474.4 g of toluene were added. The temperature was raised to 70°C, and 118.6 g of a toluene solution of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum (the platinum content in the toluene solution was 100 ppm) was added dropwise. The reaction was maintained for 4 hours, and activated carbon was added for adsorption and filtration. Low boiling materials were removed at a vacuum degree of -0.06-0.09 MPa and a temperature of 120-130°C to obtain 580 g of a carboxyl-containing compound 3 with a triazine skeleton, with a yield of 97.8%.
[0049] (2) Preparation of silicone encapsulation samples for Mini LED
[0050] The preparation method of the Mini LED silicone encapsulation adhesive sample in this embodiment is basically the same as that in Example 1, except that Compound 1 in Example 1 is changed to Compound 3. The sample performance is shown in Table 2.
[0051] Example 4
[0052] (1) Add 140 g (1 mol) of allyl succinic anhydride, 147.4 g (1.1 mol) of tetramethyldisiloxane and 205.5 g of toluene into a three-necked flask, raise the temperature to 80° C., dropwise add 82.2 g of a toluene solution of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum (the platinum content in the toluene solution is 100 ppm), maintain the reaction for 4 hours, add activated carbon for adsorption and filtration, remove low boiling substances at a vacuum degree of -0.06-0.09 MPa and a temperature of 120-130° C., and obtain 268 g of intermediate 4 with a yield of 97.81%;
[0053] In a three-necked flask, 274 g (1 mol) of intermediate 4, 209 g (1 mol) of diallyl isocyanurate and 386.4 g of toluene were added, the temperature was raised to 70°C, 96.6 g of a toluene solution of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum (the platinum content in the toluene solution was 100 ppm) was added dropwise, the reaction was maintained for 4 hours, activated carbon was added for adsorption and filtration, low boiling points were removed at a vacuum degree of -0.06-0.09 MPa and a temperature of 120-130°C, and 476 g of a carboxyl-containing compound 4 with a triazine main skeleton was obtained, with a yield of 98.55%.
[0054] (2) Preparation of silicone encapsulation samples for Mini LED
[0055] The preparation method of the Mini LED silicone encapsulation adhesive sample in this embodiment is basically the same as that in Example 1, except that the compound 1 in Example 1 is changed to compound 4. The sample performance is shown in Table 2.
[0056] Example 5
[0057] Preparation of silicone encapsulation samples for Mini LED
[0058] 65 parts by mass of a vinylphenyl silicone resin with a viscosity of 80000 mPa·s and a vinyl content of 4.5 wt%, 25 parts by mass of a vinylphenyl silicone oil with a viscosity of 4000 mPa·s and a vinyl content of 0.32 wt%, 10 parts by mass of a hydrogen-containing phenyl silicone oil with an active hydrogen content of 0.57 wt%, 1 part by mass of compound 1, 1 part by mass of KH-560 and 0.01 parts by mass of 1-ethynyl-1-cyclohexanol were mixed uniformly in a high-speed centrifuge (1200 rpm), and then 0.08 parts by mass of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum (platinum content 5000 ppm) catalyst and 3.5 parts by mass of fumed silica were added, mixed uniformly, vacuum degassed, cured at 90°C for 1 hour and at 150°C for 3-4 hours. The sample properties are shown in Table 2.
[0059] Example 6
[0060] Preparation of silicone encapsulation samples for Mini LED
[0061] 65 parts by mass of vinyl phenyl silicone resin with a viscosity of 80000 mPa·s and a vinyl content of 4.5 wt%, 25 parts by mass of vinyl phenyl silicone oil with a viscosity of 4000 mPa·s and a vinyl content of 0.32 wt%, 10 parts by mass of hydrogen-containing phenyl silicone oil with an active hydrogen content of 0.57 wt%, 1 part by mass of compound 1, 1 part by mass of epoxy tackifier HM-165 developed by our company and 0.01 parts by mass of 1-ethynyl-1-cyclohexanol were mixed uniformly under the action of a high-speed centrifuge (1200 rpm), and then 0.08 parts by mass of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum (platinum content 5000 ppm) catalyst and 3.5 parts by mass of fumed silica were added, mixed uniformly, vacuum degassed, cured at 90°C for 1 hour and at 150°C for 3-4 hours. The sample properties are shown in Table 2.
[0062] Comparative Example 1
[0063] Preparation of silicone encapsulation samples for Mini LED
[0064] 65 parts by mass of a vinylphenyl silicone resin with a viscosity of 80000 mPa·s and a vinyl content of 4.5 wt%, 25 parts by mass of a vinylphenyl silicone oil with a viscosity of 4000 mPa·s and a vinyl content of 0.32 wt%, 10 parts by mass of a hydrogen-containing phenyl silicone oil with an active hydrogen content of 0.57 wt%, 2 parts by mass of KH-560 and 0.01 parts by mass of 1-ethynyl-1-cyclohexanol were mixed uniformly in a high-speed centrifuge (1200 rpm), and then 0.08 parts by mass of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum (platinum content 5000 ppm) catalyst and 3.5 parts by mass of fumed silica were added, mixed uniformly, vacuum degassed, cured at 90°C for 1 hour and at 150°C for 3-4 hours. The sample properties are shown in Table 2.
[0065] Comparative Example 2
[0066] Preparation of silicone encapsulation samples for Mini LED
[0067] 65 parts by mass of vinyl phenyl silicone resin with a viscosity of 80000 mPa·s and a vinyl content of 4.5 wt%, 25 parts by mass of vinyl phenyl silicone oil with a viscosity of 4000 mPa·s and a vinyl content of 0.32 wt%, 10 parts by mass of hydrogen-containing phenyl silicone oil with an active hydrogen content of 0.57 wt%, 2 parts by mass of the company's self-developed epoxy tackifier HM-165 and 0.01 parts by mass of 1-ethynyl-1-cyclohexanol were mixed uniformly in a high-speed centrifuge (1200 rpm), and then 0.08 parts by mass of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum (platinum content 5000 ppm) catalyst and 3.5 parts by mass of fumed silica were added, mixed uniformly, vacuum degassed, cured at 90°C for 1 hour and at 150°C for 3-4 hours. The sample properties are shown in Table 2.
[0068]
[0069]
[0070] The performance test method of Mini LED silicone encapsulation adhesive in Table 2 is as follows:
[0071] Hardness: The hardness of Mini LED silicone encapsulation adhesive is measured in accordance with GB / T531.1-2008.
[0072] Light transmittance: at 25℃, test the light transmittance in the visible light wavelength range of 200-800nm using a UV-visible photometer in accordance with GB / T2410-2008.
[0073] Molding effect: According to the enterprise standard Q / ZQHM 51-2021, the molding effect before and after curing is tested with an optical image tester.
[0074] Bonding tensile shear strength: The bonding tensile shear strength between Mini LED silicone encapsulation adhesive and substrate is measured in accordance with GB / T13936-2014.
[0075] It can be seen from Table 2 Comparative Examples 1 and 2 that after adding the adhesion promoter prepared by the present invention, the hardness, light transmittance and molding effect of the encapsulant remain basically unchanged, the adhesion to the bonding substrate is significantly improved, and the shear force on the aluminum substrate is increased by 125-355%, and the shear force on the glass plate is increased by 56-463%. This may be because the structure contains a unique carboxylic acid functional group, which can produce a strong chemical bond with the hydroxyl group on the metal surface. At the same time, the vinyl group in the structure can also be added to the main resin structure, and has very good chemical compatibility. From Example 5 and Example 6, it can be seen that the bonding strength of the adhesion promoters with epoxy groups and carboxylic acid groups added at the same time will be higher than that of the adhesion promoter with carboxylic acid groups added alone, which may be because the carboxyl group can promote the ring-opening reaction of the epoxy group and act on the bonding substrate at the same time, thereby improving the bonding effect. It can be seen from each embodiment and comparative example that under the same test conditions, the bonding strength of the aluminum substrate is higher than that of the glass substrate. The reason is that the surface of the glass substrate is smooth and the bonding points are relatively few. This is also one of the reasons why aluminum substrates are currently the preferred substrates for Mini LED packaging.
[0076] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing a carboxyl-containing compound with triazine as a skeleton, characterized in that: The steps include: (1) Succinic anhydride, hydrogen-containing siloxane and an organic solvent are mixed, the temperature is raised to 50-90°C, a catalyst is added to react for 2-8 hours, and low-boiling substances are removed to obtain an intermediate; (2) Mixing the intermediate, isocyanurate and organic solvent, raising the temperature to 50-80°C, adding a catalyst and reacting for 2-8 hours, removing low-boiling substances, and obtaining a carboxyl-containing compound with triazine as the skeleton; The succinic anhydride in step (1) is at least one of allyl succinic anhydride, butenyl succinic anhydride, pentenyl succinic anhydride, hexenyl succinic anhydride, heptenyl succinic anhydride, octenyl succinic anhydride, nonenyl succinic anhydride, decenyl succinic anhydride, dodecenyl succinic anhydride, pentadecenyl succinic anhydride and octadecenyl succinic anhydride; The hydrogen-containing siloxane in step (1) is at least one of tetramethyldisiloxane, tetramethylcyclotetrasiloxane and dimethyldiphenyldisiloxane; The isocyanurate in step (2) is at least one of triallyl isocyanurate, diallyl isocyanurate and allyl isocyanurate.
2. The method for preparing a carboxyl-containing compound with triazine as a skeleton according to claim 1, characterized in that: The organic solvent in steps (1) and (2) is at least one of toluene, xylene, cyclohexane and methylcyclohexane; and the catalyst is at least one of platinum, palladium and rhodium and their complexes.
3. The method for preparing a carboxyl-containing compound with triazine as a skeleton according to claim 2, characterized in that: The catalyst in steps (1) and (2) is at least one of chloroplatinic acid and 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum; the amount of the catalyst in step (1) is 30-100 ppm of the mass of the reactants in step (1); the amount of the catalyst in step (2) is 20-80 ppm of the mass of the reactants in step (2).
4. The method for preparing a carboxyl-containing compound with triazine as a skeleton according to claim 1, characterized in that: The molar ratio of succinic anhydride to hydrogen-containing siloxane in step (1) is 1:1 to 1.2; The molar ratio of the intermediate to isocyanurate in step (2) is 1:1 to 1.
2.
5. The method for preparing a carboxyl-containing compound with triazine as a skeleton according to claim 1, characterized in that: The structural formula of the intermediate is as follows: 。 6. The method for preparing a carboxyl-containing compound with triazine as a skeleton according to claim 1, characterized in that: The reaction time of steps (1) and (2) is 4 to 5 hours. The reaction temperature of step (1) is 80-90°C, and the reaction temperature of step (2) is 70-80°C; The conditions for removing low boiling points in steps (1) and (2) are as follows: adding activated carbon for adsorption filtration, the vacuum degree is -0.06-0.09 MPa, and the temperature is 120-130°C.
7. A carboxyl-containing compound with triazine as the skeleton, characterized in that: The method is obtained by the preparation method according to any one of claims 1 to 6.
8. The carboxyl-containing compound with triazine as the skeleton according to claim 7, characterized in that: The structural formula of the carboxyl-containing compound with triazine as the skeleton is as follows: 。 9. Application of a carboxyl-containing compound with triazine as a skeleton as claimed in claim 8 in Mini LED silicone encapsulation adhesive.