A method for preparing nano silicon dioxide with core-shell structure

Core-shell structured nano-silica was prepared by sol-gel method and hyperbranching modification, which solved the problems of uneven particle size, inconsistent shape and agglomeration in the existing technology, and achieved good dispersion and compatibility of nano-silica in polymer, thus improving the uniformity of resin.

CN115368578BActive Publication Date: 2024-11-08INNER MONGOLIA TIANYI CHENGXIN ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202110547905.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-05-19
Publication Date
2024-11-08
Estimated Expiration
2041-05-19

AI Technical Summary

Technical Problem

Existing silica production processes are unstable, resulting in uneven particle size and shape. Nano-silica is prone to agglomeration, leading to poor compatibility with polymers and uneven dispersion when used as a filler, thus causing resin defects.

Method used

Core-shell structured nano-silica with hyperbranched polyurethane as the shell and nano-silica as the core was prepared by sol-gel method and hyperbranching modification. By controlling the reaction conditions and using specific catalysts, uniform particle size and regular shape were ensured.

Benefits of technology

The prepared nano-silica has uniform size and regular shape, good compatibility with polymers, can be uniformly dispersed in organic phase, does not easily settle, and improves the appearance uniformity of resin.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115368578B_ABST
    Figure CN115368578B_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing silicon dioxide with a core-shell structure, wherein the nano silicon dioxide prepared by the method is a spherical structure with a hyperbranched polyurethane as a shell and nano silicon dioxide as a core. The silicon dioxide is not only regular in shape and uniform in size, with a diameter within the range of 80-120 nm, but also has good dispersibility in an organic phase.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing modified nano silicon dioxide, in particular to a method for preparing nano silicon dioxide with hyperbranched polyurethane as a shell and nano silicon dioxide as a core. Background Art

[0002] Silica, also known as white carbon black, has good thermal stability, corrosion resistance, friction resistance, and can absorb ultraviolet rays, so it is widely used in rubber, shoemaking, paint, papermaking, synthetic resins, grease and other industrial sectors. However, the current production of silica is still extensive, the preparation process is unstable, the silica obtained has different shapes and uneven particle sizes, and the obtained nano-silica is easy to agglomerate. When added to organic resins as fillers, it has poor compatibility with polymers, weak interfacial forces, uneven dispersion, and easy sedimentation or agglomeration, which can easily lead to defects in the resin and uneven appearance. Summary of the invention

[0003] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a nano-silicon dioxide with uniform size, regular shape and good dispersion in a polymer and having a core-shell structure.

[0004] To achieve the above object, the technical solution adopted by the present invention is: a nano-silicon dioxide with a core-shell structure, comprising the following steps:

[0005] S1. Add tetraethyl orthosilicate and hydrochloric acid to the ethanol solution and stir for 1-3 hours at a temperature of 22-28°C;

[0006] S2. Add the amino-containing silane coupling agent and hydrochloric acid to the ethanol solution and stir for 1 to 3 hours at a temperature of 38 to 42°C;

[0007] S3. The solution obtained by S1 and S2 was stirred and mixed uniformly at a temperature of 23 to 28 ° C. The reaction mixture was filtered, washed with ethanol, and dried to obtain amino-modified nano-silica;

[0008] S4. Add the aminated nano-silica obtained in step S3 to diisocyanate, stir at 58-62° C. for 1-3 h, filter, wash with ethyl acetate, add the filter cake to vegetable oil-based polyol, add an organic tin catalyst, stir at 78-82° C. for 1-3 h, filter, wash with ethyl acetate, and then dry in a protective gas atmosphere;

[0009] S5. Repeat step S4 three times to obtain the silicon dioxide.

[0010] Preferably, in step S1, the weight ratio of tetraethyl orthosilicate to hydrochloric acid is 9-11:1; in step S2, the weight ratio of the silane coupling agent with amino group to hydrochloric acid is 9-11:1; the weight ratio of the silane coupling agent with amino group to tetraethyl orthosilicate is 0.5-2:1.

[0011] Preferably, in step S4, the weight ratio of the amino-modified nano-silica to the diisocyanate is 1:3-5; the weight ratio of the amino-modified nano-silica to the vegetable oil-based polyol is 1:3-5.

[0012] Preferably, in step S1 and step S2, the stirring speed is 800-1500 rpm.

[0013] Preferably, in step S1, the weight ratio of tetraethyl orthosilicate to ethanol is 1:15-25; in step S2, the weight ratio of the silane coupling agent with amino group to ethanol is 1:15-25.

[0014] Preferably, the silane coupling agent with amino group is at least one of KH-550, KH-602 and KH-792.

[0015] Preferably, the diisocyanate is at least one of toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate and dicyclohexylmethane-4,4'-diisocyanate.

[0016] Preferably, the vegetable oil-based polyol is at least one of castor oil-based polyol and leprosy resin oil-based polyol.

[0017] Preferably, the organotin catalyst is at least one of dibutyltin dilaurate, dibutyltin oxide and stannous octoate.

[0018] Preferably, the weight ratio of the organotin catalyst to the amino-modified nano-silicon dioxide is 1:20-30.

[0019] The invention has the beneficial effects that: the invention adopts the sol-gel method and hyperbranching modification to prepare nano silicon dioxide with hyperbranched polyurethane as the shell and nano silicon dioxide as the core, and the silicon dioxide has a regular shape and uniform size. At the same time, the silicon dioxide has inorganic nanoparticles as the core and hyperbranched polyurethane as the shell, and has the advantages of thermal stability, corrosion resistance, ultraviolet absorption, friction resistance, etc. of silicon dioxide, and also has the advantages of good compatibility with polymers and strong action force, and can be evenly dispersed in an organic phase or a polymer solution without sedimentation. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1It is the nano silicon dioxide with core-shell structure as described in Example 1. DETAILED DESCRIPTION

[0021] Example 1

[0022] The method for preparing silicon dioxide described in this embodiment comprises the following steps:

[0023] S1 Add 5 parts by weight of tetraethyl orthosilicate and 0.5 parts by weight of hydrochloric acid to 100 parts by weight of ethanol solution, stir at 1000 rpm for 2 h at a temperature of 25°C;

[0024] S2: Add 5 parts by weight of silane coupling agent KH550 with amino group and 0.5 parts by weight of hydrochloric acid to 100 parts by weight of ethanol solution, stir at 1000 rpm for 2 h at 40°C;

[0025] S3: Mix the solutions obtained in S1 and S2, stir at 25°C, filter the reaction mixture, wash with ethanol, and dry to obtain amino-modified nano-silica;

[0026] S4: adding 5 parts by weight of the aminated nano-silica obtained in step S3 to 20 parts by weight of hexamethylene diisocyanate, stirring at 60° C. for 2 hours, filtering, washing with ethyl acetate, adding the filter cake to 20 parts by weight of leprosy resin oil-based polyol, adding 0.2 parts by weight of dibutyltin dilaurate catalyst, stirring at 80° C. for 2 hours, filtering, washing with ethyl acetate, and then drying in a protective gas atmosphere;

[0027] S5: Repeat step S4 three times to obtain nano-silica with hyperbranched polyurethane as the shell and nano-silica as the core. The obtained core-shell structured silica is nano-scale with a diameter in the range of 80-150 nm.

[0028] Example 2

[0029] The method for preparing silicon dioxide described in this embodiment comprises the following steps:

[0030] S1 Add 5 parts by weight of tetraethyl orthosilicate and 0.5 parts by weight of hydrochloric acid to 100 parts by weight of ethanol solution, stir at 1000 rpm for 2 h at a temperature of 25°C;

[0031] S2: Add 5 parts by weight of amino-containing silane coupling agent KH-602 and 0.5 parts by weight of hydrochloric acid to 100 parts by weight of ethanol solution, stir at 1000 rpm for 2 h at a temperature of 40°C;

[0032] S3: Mix the solutions obtained in S1 and S2, stir at 25°C, filter the reaction mixture, wash with ethanol, and dry to obtain amino-modified nano-silica;

[0033] S4: adding 5 parts by weight of the aminated nano-silica obtained in step S3 to 20 parts by weight of toluene diisocyanate, stirring at 60° C. for 2 hours, filtering, washing with ethyl acetate, adding the filter cake to 20 parts by weight of leprosy resin oil-based polyol, adding 0.2 parts by weight of dibutyltin dilaurate catalyst, stirring at 80° C. for 2 hours, filtering, washing with ethyl acetate, and then drying in a protective gas atmosphere;

[0034] S5: Repeat step S4 three times to obtain nano-silica with hyperbranched polyurethane as the shell and nano-silica as the core. The obtained core-shell structured silica is nano-scale with a diameter in the range of 80-150 nm.

[0035] Example 3

[0036] The method for preparing silicon dioxide described in this embodiment comprises the following steps:

[0037] S1 Add 5 parts by weight of tetraethyl orthosilicate and 0.5 parts by weight of hydrochloric acid to 100 parts by weight of ethanol solution, stir at 1000 rpm for 2 h at a temperature of 25°C;

[0038] S2: Add 5 parts by weight of amino-containing silane coupling agent KH-602 and 0.5 parts by weight of hydrochloric acid to 100 parts by weight of ethanol solution, stir at 1000 rpm for 2 h at a temperature of 40°C;

[0039] S3: Mix the solutions obtained in S1 and S2, stir for 2 hours at room temperature, filter the reaction mixture, wash with ethanol, and dry to obtain amino-modified nano-silica;

[0040] S4: adding 5 parts by weight of the aminated nano-silica obtained in step S3 to 20 parts by weight of toluene diisocyanate, stirring at 60° C. for 2 hours, filtering, washing with ethyl acetate, adding the filter cake to 20 parts by weight of castor oil-based polyol, adding 0.2 parts by weight of dibutyltin dilaurate catalyst, stirring at 80° C. for 2 hours, filtering, washing with ethyl acetate, and then drying in a protective gas atmosphere;

[0041] S5: Repeat step S4 three times to obtain nano-silica with hyperbranched polyurethane as the shell and nano-silica as the core. The obtained core-shell structured silica is nano-scale with a diameter in the range of 80-150 nm.

[0042] Example 4

[0043] The method for preparing silicon dioxide described in this embodiment comprises the following steps:

[0044] S1 5 parts by weight of tetraethyl orthosilicate and 0.5 parts by weight of hydrochloric acid were added to 100 parts by weight of ethanol solution, and stirred at 1000 rpm for 2 h at a temperature of 25°C.

[0045] S2 5 parts by weight of silane coupling agent KH-602 with amino group and 0.5 parts by weight of hydrochloric acid were added to 100 parts by weight of ethanol solution, and stirred at 1000 rpm for 2 hours at a temperature of 40°C.

[0046] S3: Mix the solutions obtained in S1 and S2, stir, and keep the temperature at room temperature. The reaction mixture is filtered, washed with ethanol, and dried to obtain amino-modified nano-silica.

[0047] S4: adding 5 parts by weight of the aminated nano-silica obtained in step S3 to 20 parts by weight of toluene diisocyanate, stirring at 60° C. for 2 hours, filtering, washing with ethyl acetate, adding the filter cake to 20 parts by weight of castor oil-based polyol, adding 0.2 parts by weight of dibutyltin oxide catalyst, stirring at 80° C. for 2 hours, washing with ethyl acetate, and then drying in a protective gas atmosphere;

[0048] S5: Repeat step S4 three times to obtain nano-silica with hyperbranched polyurethane as the shell and nano-silica as the core. The obtained core-shell structured silica is nano-scale with a diameter in the range of 80-150 nm.

[0049] Morphology test: The core-shell structure of nano-silica was observed using a transmission electron microscope; Figure 1 This is a transmission electron microscope image of the silicon dioxide described in Example 1.

[0050] Dispersibility test: 100 g of the nano-silica in Examples 1 to 4 was dispersed into 1 L of toluene solution by stirring for 10 minutes, and then poured into a 1 L measuring cylinder. The solution was allowed to stand and the time required for the nano-silica to settle 1 cm at the bottom of the measuring cylinder was observed.

[0051] Table 1

[0052] Dispersibility Average particle size / nm Example 1 20 days 92 Example 2 18 days 102 Example 3 20 days 96 Example 4 15 days 114

[0053] from Figure 1 It can be seen from Table 1 that the nano-silicon dioxide in the embodiment has a core-shell structure and is a spherical particle with a regular shape and a uniform particle size between 80-120 nm. The nano-silicon dioxide with the core-shell structure is well dispersed in the organic phase.

[0054] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing silicon dioxide having a core-shell structure, characterized in that: The following steps are involved: S1. Add tetraethyl orthosilicate and hydrochloric acid to the ethanol solution and stir at a speed of 800 to 1500 rpm for 1 to 3 hours at a temperature of 22 to 28°C; S2. Add the amino-containing silane coupling agent and hydrochloric acid to the ethanol solution, stir at a speed of 800 to 1500 rpm for 1 to 3 hours at a temperature of 38 to 42°C; S3. The solution obtained by S1 and S2 was stirred and mixed uniformly at a temperature of 23 to 28 ° C. The reaction mixture was filtered, washed with ethanol, and dried to obtain amino-modified nano-silica; S4. The aminated nano-silica of step S3 is added to the diisocyanate, stirred at 58-62°C for 1-3h, then filtered, washed with ethyl acetate, and then the filter cake is added to the vegetable oil-based polyol, an organic tin catalyst is added, stirred at 78-82°C for 1-3h, filtered, washed with ethyl acetate, and then dried in a protective gas atmosphere; S5. Repeat step S4 three times to obtain a nano-silica having a hyperbranched polyurethane shell and nano-silica as a core, wherein the diameter of the obtained core-shell structure of silica is in the range of 80-150nm; In step S1, the weight ratio of tetraethyl orthosilicate to hydrochloric acid is 9-11:1, and the weight ratio of tetraethyl orthosilicate to ethanol is 1:15-25; in step S2, the weight ratio of the silane coupling agent with amino group to hydrochloric acid is 9-11:1, and the weight ratio of the silane coupling agent with amino group to ethanol is 1:15-25; the weight ratio of the silane coupling agent with amino group to tetraethyl orthosilicate is 0.5-2:1; In step S4, the weight ratio of the aminated nano-silica to the diisocyanate is 1:3-5; the weight ratio of the aminated nano-silica to the vegetable oil-based polyol is 1:3-5; the weight ratio of the organotin catalyst to the aminated nano-silica is 1:20-30; the diisocyanate is at least one of toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate and dicyclohexylmethane-4,4'-diisocyanate; the vegetable oil-based polyol is at least one of castor oil-based polyol and leprosy resin oil-based polyol.

2. The method for preparing silicon dioxide having a core-shell structure according to claim 1, characterized in that: The silane coupling agent with amino group is at least one of KH-550, KH-602 and KH-792.

3. The method for preparing silicon dioxide having a core-shell structure according to claim 1, characterized in that: The organotin catalyst is at least one of dibutyltin dilaurate, dibutyltin oxide and stannous octoate.

Citation Information

Patent Citations

  • Hyperbranched resin-based UV curing ink-jet ink, preparation method and application thereof

    CN107987611A

  • Hyperbranched polymer electrode active material and preparation method thereof

    CN109638252A

  • Surface treating agent and metal surface treating method

    CN111455361A