A kind of styrene-polyolefin functional polymer and preparation method thereof
By using the preparation method of styrene-polyolefin functional polymers in polyolefin and polystyrene materials, the defects in the material in terms of mechanical properties and weather resistance are solved, and high-performance and environmentally friendly material modification is achieved, which is suitable for multiple application fields.
Patent Information
- Application Number
- CN202210992797.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-18
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-08-18
AI Technical Summary
The existing blended materials of polyolefin and polystyrene have shortcomings in terms of mechanical properties and weather resistance, and the existing modification methods have problems with difficulty in control, high cost and environmental protection.
Using the preparation method of styrene-polyolefin functional polymer, the molecular structure is adjusted through suspension polymerization and extrusion reaction technology, and the compatibility and chemical resistance of the polymer are improved as a compatibilizer or additive. Material properties.
The high performance of polyolefin/polystyrene alloys has been achieved, providing a broader application space, especially in the fields of 5G applications, green recycling and electronic appliances, and improving the mechanical properties and aging resistance of the materials.
Smart Images

Figure CN115368687B_ABST
Abstract
Description
Technical Field
[0002] The invention belongs to the field of synthesis and reactive extrusion of polymer materials and relates to a styrene-polyolefin functional polymer and a preparation method thereof. Background Art
[0004] Polyolefin (PO) and polystyrene (PS) are among the top five general-purpose plastics, with large social demand and are also the main types of waste plastics. PS has the advantages of high hardness, low shrinkage, good thermoforming and easy printing, but its weather resistance is poor, it is easy to crack, and its toughness and solvent resistance are not ideal. The main categories of PO are polypropylene (PP) and polyethylene (PE). As a common general-purpose plastic, PP is extremely widely used, and has excellent mechanical properties, good electrical insulation and chemical resistance, but it has the disadvantages of large molding shrinkage, low hardness, easy aging, and poor thermoforming ability; PE is odorless, non-toxic, feels like wax, has excellent low-temperature resistance (the lowest operating temperature can reach -100~-70℃), good chemical stability, and can withstand the corrosion of most acids and alkalis (not resistant to oxidizing acids). PE is widely used and is mainly used to make films, packaging materials, containers, pipes, monofilaments, wires and cables, daily necessities, etc., and can be used as high-frequency insulation materials for televisions, radars, etc. It is insoluble in general solvents at room temperature, has low water absorption, and excellent electrical insulation, but PE has general mechanical properties, low tensile strength, poor creep resistance, and low temperature resistance. In order to overcome the shortcomings of the above two types of materials, PS, PP or PE will be blended and modified to prepare alloy materials. According to research, PS and PP or PE are typical incompatible systems. Simple mixing will lead to aggregation of the dispersed phase, thus showing lower mechanical properties. In order to effectively blend the two, measures need to be taken to reduce the surface tension between the two phases and improve their compatibility.
[0005] At present, most of the in-situ compatibilization technology between PP or PE and PS is used, which has the advantages of being cheap and easy to use. For example, in patent CN101402765, Lewis acid is used as a catalyst to induce Friedel-Crafts alkylation reaction between PE and PS, thereby increasing the compatibilization of PE / PS alloy in situ; US Patent US172384 also mentions the use of anhydrous aluminum chloride as a reaction catalyst for increasing the compatibilization of polyolefins and PS, but this method has certain problems in controllability during the reaction process, and Lewis acids such as anhydrous aluminum chloride are highly corrosive and sensitive to water, which will cause the degradation of PS, and the color of the prepared alloy material is easy to turn yellow, and the aging resistance is reduced, resulting in limited application of the material.
[0006] In addition, patent CN101580614 discloses another method for preparing PP-g-PS copolymers. The polymer is prepared by coordination-anionic polymerization. This method has complex production steps, uses a variety of organic solvents and catalysts, and the reaction process requires precise control. Not only is the manufacturing cost high, but the method can only produce copolymers with specific PP main chains and PS side chains. The product structure is relatively single. What is more serious is that under the current background of carbon peak and increasing environmental pressure, the multiple organic solvents and other additives used in this method are also not conducive to environmental protection, significantly increasing the recycling cost and the risk of environmental pollution.
[0007] There are also some patents such as CN102757596 and CN101402766 that mention the use of SBS, SEP or SEBS to modify the PP / PS alloy system, which does produce some beneficial effects in improving the interfacial bonding strength, but it acts more as a toughening agent, and adding too much will affect the strength and rigidity of the material.
[0008] In addition, there are studies that use PP-g-MAH, POE-g-MAH, etc. as compatibilizers to modify polyolefin / PS alloys. For example, CN103589060 mentions the use of grafted polypropylene as a compatibilizer. However, the functional groups such as anhydride used in this method fail to provide a suitable reaction pathway in the alloy to improve the two-phase interface, and no detailed explanation is given in terms of mechanism. It may not be possible to achieve a good compatibilization effect in large-scale industrialization. Summary of the invention
[0010] The present invention utilizes the deficiencies of the prior art and provides a styrene-polyolefin functional polymer and a preparation method thereof based on the prior art. The polymer combines the characteristics of the synthetic reaction technology and the reactive extrusion technology to realize the functionalization of the polymer. A major advantage of the product is that the molecular structure is adjustable, and polystyrene can be made into the main chain of the molecule and polyolefin can be designed as a branch chain, or polyolefin can be made into the main chain of the molecule and polystyrene can be designed as a branch chain structure. Moreover, according to different applications, the main chain or branch chain molecular weight can be adjusted within a certain range, so that the polymer of this structure type can not only provide compatibility in the polystyrene / polyolefin alloy, but also improve the chemical resistance of polystyrene and reduce the dielectric properties; it can also improve the friction properties of engineering plastics such as PA and POM, etc., so it can provide a wider application space.
[0011] The purpose of the present invention can be achieved by the following technical solutions:
[0012] On the one hand, the present invention relates to a styrene-polyolefin functional polymer, which comprises the following components and weight parts: 30-70 parts of polymer I, 30-70 parts of polymer II, 0.01-1 parts of catalyst, 0.1-1 parts of antioxidant, 0.1-1 parts of lubricant, and 0.2-5 parts of devolatilizer;
[0013] Wherein, polymer I is prepared by suspension polymerization in an aqueous medium from styrene, reactive monomer I, oil-soluble initiator, dispersant, dispersant aid, and molecular weight regulator in a weight ratio of (80-99):(1-20):(0.1-1.0):(0.1-2.0):(0.01-0.1):(0.1-1.0);
[0014] The polymer II is prepared from polyolefin, peroxide initiator, reactive monomer II, diluent and processing aid in a weight ratio of 100:(0.01~2):(0.5~6):(0.1~5):(0.2~1.0).
[0015] As an embodiment, the reactive monomer I is selected from one of methyl methacrylate, ethyl methacrylate, butyl methacrylate, and glycidyl methacrylate. A further preferred reactive monomer I is glycidyl methacrylate;
[0016] As an embodiment, the oil-soluble initiator is an azo initiator. The azo initiator is selected from at least one of azobisisobutyronitrile, azobisisoheptanenitrile or dimethyl azobisisobutyrate. A further preferred initiator is azobisisobutyronitrile.
[0017] As an embodiment, the dispersant is at least one of polyvinyl alcohol, active calcium phosphate and hydroxyethyl cellulose.
[0018] As an embodiment, the dispersant is sodium dodecylbenzene sulfonate or sodium dodecyl sulfate.
[0019] As an embodiment, the molecular weight regulator is dodecyl mercaptan.
[0020] As an embodiment, the preparation method of the polymer I comprises: A1, mixing the styrene monomer, reactive monomer, oil-soluble initiator, dispersant, dispersant aid, molecular weight regulator and water, reacting at 65-80° C. for 3-6 hours, heating to 85-90° C. for aging for 0.5-2 hours; the mass ratio of the total weight of the monomer to water is (1-3):1;
[0021] A2. After the reaction is completed, filter and wash, dry at 75-85°C to constant weight, and then sieve to obtain polymer I.
[0022] In some embodiments, the styrene monomer, reactive monomer, oil-soluble initiator, dispersant, dispersant aid and molecular weight regulator are mixed with deionized water in a weight ratio of (1-3):1 to the total weight of the monomers in a reactor, heated to 65-80°C under stirring, and reacted for 3-6 hours, heated to 85-90°C and matured for 0.5-2 hours; after completion, the mixture is placed in a storage tank, the obtained material is filtered, washed with deionized water 2-5 times, dried at 75-85°C to constant weight, and sieved to obtain polymer I.
[0023] As an embodiment, the polyolefin is selected from one or a combination of polybutene, polypropylene, polyethylene, ethylene-propylene copolymer, ethylene-butene copolymer, and ethylene-octene copolymer.
[0024] As an embodiment, the peroxide initiator is selected from dicumyl peroxide, benzoyl peroxide, p-chlorobenzoyl peroxide, di-tert-butyl peroxide isopropylbenzene, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexyne, 2,5-dimethyl-2,5-bis(benzoyl peroxide)hexane, 1,1-bis(tert-butyl peroxide)-3,3,5-trimethylcyclohexane, tert-butyl peroxide, or a combination thereof. A further preferred peroxide initiator is 1,1-bis(tert-butyl peroxide)-3,3,5-trimethylcyclohexane.
[0025] As an embodiment, the reactive monomer II is selected from one or a combination of acrylic acid, methacrylic acid, acrylamide, methacrylic acid amide, maleic anhydride, fumaric acid, dibutyl maleate, citric acid, itaconic acid. A further preferred reactive monomer is acrylic acid or maleic anhydride.
[0026] As an embodiment, the diluent is at least one of acetone, methyl ethyl ketone, methyl acetate, ethanol, and mineral oil.
[0027] As an embodiment, the processing aid is a composition of a lubricant (silicone, low molecular wax, fatty acid amide, metal soap salt) and an antioxidant (hindered phenol, phosphite). The weight ratio of the lubricant to the antioxidant is 1: (0.5-2).
[0028] As an embodiment, the preparation method of polymer II comprises: uniformly mixing the polyolefin, peroxide initiator, reactive monomer II, diluent and processing aid, and then putting them into a reaction extruder, and then granulating and drying after melt mixing, extrusion reaction and devolatilization to obtain polymer II. Preferably, the reaction extruder is a twin-screw extruder with an aspect ratio of (44-60): 1, an extrusion temperature of 160-240°C, and a screw speed of 200-400rpm.
[0029] As an embodiment, the catalyst is selected from at least one of quaternary ammonium salts, quaternary phosphonium salts, tertiary amines, tertiary phosphorus, and imidazole compounds. A further preferred catalyst is an imidazole compound or a tertiary amine.
[0030] As an embodiment, the antioxidant is selected from at least one of hindered phenols and phosphites. Preferably, the antioxidant is a combination of hindered phenols and phosphites; more preferably, the weight ratio of hindered phenols to phosphites is 1:(0.3-3).
[0031] As an embodiment, the lubricant is at least one of fatty acid amides, silicones, and pentaerythritol stearate.
[0032] As an embodiment, the devolatilizer is selected from at least one of anhydrous ethanol, acetone, supercritical CO2, deionized water, N2, etc.
[0033] A second aspect of the present invention is to provide a method for preparing a styrene-polyolefin functional polymer, the method comprising the following steps:
[0034] S1, the polymer I, polymer II, catalyst, antioxidant, and lubricant are mixed evenly, and fed into a twin-screw extruder with a length-to-diameter ratio of (44-60):1 through a main feed port, with a processing temperature of 180-240°C and a rotation speed of 180-600rpm;
[0035] S2, adding the devolatilizer through the injection port at the rear end of the twin-screw extruder, and discharging the residual small molecular substances and the devolatilizer in the reaction process through the devolatilization port;
[0036] S3, after being extruded through a die head, water-cooled, and pelletized by a pelletizer, the styrene-polyolefin functional polymer is obtained.
[0037] In a third aspect, the present invention relates to the use of the styrene-polyolefin functional polymer, wherein the polymer is used as a compatibilizer for polyolefin / polystyrene alloys, or as an additive for improving the chemical resistance of polystyrene, or as an additive for reducing the dielectric properties of polystyrene, or as an additive for improving the friction properties of engineering plastics. The engineering plastics include PA, POM, etc.
[0038] Compared with the prior art, the present invention has the following beneficial effects: The preparation method of the present invention has advanced technology. A polymer intermediate is first prepared by a relatively environmentally friendly suspension polymerization process, and then another polyolefin intermediate with a reactive functional group is prepared by an extrusion reaction process. The two are then further subjected to an extrusion reaction process to prepare a final styrene-polyolefin functional polymer in a twin-screw extruder. The product prepared by the method of the present invention can be widely used in plastic modification, especially as a compatibilizer for polyolefin / polystyrene alloys, and has broad application value in 5G applications, green recycling, electronic appliances and other fields, and is a core technology for realizing high performance, functionalization and high added value of plastic alloy materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:
[0040] Figure 1 The optical microscope photos are the microscopic surface morphology of samples 9 and 10 in Application Example 5 and the solvent-corroded surfaces of samples 16 and 17 in Application Example 8; among them, (a) is sample 9, (b) is sample 10, (c) is sample 16, and (d) is sample 17. DETAILED DESCRIPTION
[0042] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0043] Example 1
[0044] This embodiment 1 provides a styrene-polyolefin functional polymer, which includes the following components in parts by weight: 30 parts of polymer I, 70 parts of polymer II, 0.05 parts of catalyst, 0.3 parts of antioxidant, 0.2 parts of lubricant, and 1 part of devolatilizer; wherein the polymer I is prepared from 95 parts of styrene, 5 parts of reactive monomers, 0.2 parts of oil-soluble initiator, 1 part of dispersant, 0.05 parts of dispersant, and 0.5 parts of molecular weight regulator; the polymer II is prepared from 100 parts of polyolefin, 0.05 parts of peroxide initiator, 2 parts of reactive monomers, 2 parts of diluent, 0.3 parts of lubricant and 0.2 parts of antioxidant.
[0045] The reactive monomer in the polymer I is glycidyl methacrylate, the oil-soluble initiator is azobisisobutyronitrile, the dispersant is hydroxyethyl cellulose, the auxiliary dispersant is sodium dodecyl sulfate, and the molecular weight regulator is dodecyl mercaptan.
[0046] The polypropylene in the polymer II is a random copolymer polypropylene with a melt index of 7 (230°C, 2.16kg), a brand of Yungsox 5060, provided by Formosa Plastics Corporation; the peroxide initiator is 1,1-bis(tert-butyl peroxide)-3,3,5-trimethylcyclohexane, the reactive monomer is acrylic acid, the diluent is acetone, the lubricant is PE wax, and the antioxidant is 168 and 1010 mixed in a ratio of 1:1.
[0047] The catalyst is 2-methylimidazole, the antioxidant is a 1:1 composite of 168 and 1076, the lubricant is EBS, and the devolatilizer is anhydrous ethanol.
[0048] The preparation method of the styrene-polyolefin functional polymer comprises the following steps:
[0049] (1) Preparation of polymer I: Styrene monomer, reactive monomer, oil-soluble initiator, dispersant, dispersant aid and molecular weight regulator in a weight ratio of 2:1 with deionized water are mixed in a reaction kettle, heated to 75°C with stirring, and reacted for 5 hours, then heated to 85°C and aged for 2 hours; after the reaction, the mixture is placed in a storage tank, the obtained material is filtered, washed with deionized water 3 times, dried at 80°C to constant weight, and sieved to obtain polymer I.
[0050] (2) Preparation of polymer II: The polyolefin, initiator, reactive monomer, diluent and processing aid in a weight ratio are weighed and mixed uniformly, and then fed into a twin-screw extruder. After melt mixing, extrusion reaction and devolatilization, granulation and drying are performed to obtain polymer II; the length-to-diameter ratio of the twin-screw extruder is 50:1, the extrusion temperature is 160~240℃, and the screw speed is 300rpm.
[0051] (3) Polymer I, polymer II, catalyst, antioxidant and lubricant are mixed uniformly in proportion, and fed into a twin-screw extruder with a length-to-diameter ratio of 52:1 through the main feed port, with a processing temperature of 180-240°C and a rotation speed of 400 rpm; at the rear end of the twin-screw extruder, a devolatilizing agent is added through the injection port, and the target polymer is obtained after devolatilization and extrusion granulation.
[0052] Example 2
[0053] This embodiment 2 provides a styrene-polyolefin functional polymer, which includes the following components in parts by weight: 70 parts of polymer I, 30 parts of polymer II, 1 part of catalyst, 0.6 parts of antioxidant, 0.1 parts of lubricant, and 5 parts of devolatilizer; wherein the polymer I is prepared from 80 parts of styrene, 20 parts of reactive monomers, 1 part of oil-soluble initiator, 2 parts of dispersant, 0.01 parts of dispersant, and 1 part of molecular weight regulator; the polymer II is prepared from 100 parts of polyolefin, 0.2 parts of peroxide initiator, 6 parts of reactive monomers, 3 parts of diluent, 0.5 parts of lubricant and 0.5 parts of antioxidant.
[0054] The reactive monomer in the polymer I is glycidyl methacrylate, the oil-soluble initiator is azobisisobutyronitrile, the dispersant is active calcium phosphate, the auxiliary dispersant is sodium dodecylbenzene sulfonate, and the molecular weight regulator is dodecyl mercaptan.
[0055] The polyolefin in the polymer II is linear low-density polyethylene with a melt index of 20 (190°C, 2.16kg), a brand of LL6101XR, provided by ExxonMobil Corporation of the United States; the peroxide initiator is 1,1-bis(tert-butyl peroxide)-3,3,5-trimethylcyclohexane, the reactive monomer is acrylic acid, the diluent is white oil, the lubricant is zinc stearate, and the antioxidant is 168 and 1076 mixed in a ratio of 1:3.
[0056] The catalyst is 2-phenylimidazole, the antioxidant is a composite of 168 and 1010 in a ratio of 1:1, the lubricant is silicone, and the devolatilization aid is supercritical CO2.
[0057] The preparation method of the styrene-polyolefin functional polymer is the same as that of Example 1.
[0058] Example 3
[0059] This embodiment 3 provides a styrene-polyolefin functional polymer, which includes the following components in parts by weight: 50 parts of polymer I, 50 parts of polymer II, 0.1 parts of catalyst, 0.3 parts of antioxidant, 0.3 parts of lubricant, and 0.2 parts of devolatilizer; wherein the polymer I is prepared from 99 parts of styrene, 1 part of reactive monomer, 0.1 parts of oil-soluble initiator, 0.1 parts of dispersant, 0.1 parts of dispersant, and 0.5 parts of molecular weight regulator; the polymer II is prepared from 100 parts of polyolefin, 2 parts of peroxide initiator, 0.5 parts of reactive monomer, 1 part of diluent, 0.3 parts of lubricant and 0.2 parts of antioxidant.
[0060] The reactive monomer in the polymer I is glycidyl methacrylate, the oil-soluble initiator is azobisisoheptanenitrile, the dispersant is active calcium phosphate, the auxiliary dispersant is sodium dodecyl sulfate, and the molecular weight regulator is dodecyl mercaptan.
[0061] The polyolefin in the polymer II is an ethylene-octene copolymer with a melt index of 1 (190°C, 2.16kg), a brand of Engage 8842, provided by Dow Chemical Company of the United States; the peroxide initiator is 1,1-bis(tert-butyl peroxide)-3,3,5-trimethylcyclohexane, the reactive monomer is maleic anhydride, the diluent is methyl acetate, the lubricant is calcium stearate, and the antioxidant is 168 and 1010 in a 1:1 mixture.
[0062] The catalyst is triethylamine, the antioxidant is a composite of 168 and 1010 in a ratio of 1:1, the lubricant is stearic acid amide, and the devolatilization aid is deionized water.
[0063] The preparation method of the styrene-polyolefin functional polymer is the same as that of Example 1.
[0064] Example 4
[0065] This embodiment 4 provides a styrene-polyolefin functional polymer, which includes the following components in parts by weight: 60 parts of polymer I, 40 parts of polymer II, 0.5 parts of catalyst, 0.2 parts of antioxidant, 0.4 parts of lubricant, and 3 parts of devolatilizer; wherein the polymer I is prepared from 97 parts of styrene, 3 parts of reactive monomers, 0.5 parts of oil-soluble initiator, 0.8 parts of dispersant, 0.05 parts of dispersant, and 0.3 parts of molecular weight regulator; the polymer II is prepared from 100 parts of polyolefin, 0.4 parts of peroxide initiator, 1.5 parts of reactive monomers, 2 parts of diluent, 0.3 parts of lubricant and 0.2 parts of antioxidant.
[0066] The reactive monomer in the polymer I is methyl methacrylate, the oil-soluble initiator is dimethyl azobisisobutyrate, the dispersant is polyvinyl alcohol, the auxiliary dispersant is sodium dodecyl sulfate, and the molecular weight regulator is dodecyl mercaptan.
[0067] The polyolefin in the polymer II is an ethylene-propylene copolymer with a melt index of 8 (230°C, 2.16kg), a brand of Vistamaxx 3588, provided by Exxon Mobil Corporation of the United States; the peroxide initiator is 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, the reactive monomer is methyl methacrylic acid amide, the diluent is ethanol, the lubricant is polypropylene wax, and the antioxidant is 168 and 1010 mixed in a ratio of 1:1.
[0068] The catalyst is triphenylphosphine, the antioxidant is a 1:1 composite of 168 and 1010, the lubricant is erucic acid amide, and the devolatilization aid is N2.
[0069] The preparation method of the styrene-polyolefin functional polymer is the same as that of Example 1.
[0070] Example 5
[0071] This embodiment 5 provides a styrene-polyolefin functional polymer, which includes the following components in parts by weight: 40 parts of polymer I, 60 parts of polymer II, 0.2 parts of catalyst, 0.4 parts of antioxidant, 0.2 parts of lubricant, and 1 part of devolatilizer; wherein the polymer I is prepared from 90 parts of styrene, 10 parts of reactive monomers, 0.8 parts of oil-soluble initiator, 1.2 parts of dispersant, 0.03 parts of dispersant, and 0.5 parts of molecular weight regulator; the polymer II is prepared from 100 parts of polyolefin, 0.1 parts of peroxide initiator, 3 parts of reactive monomers, 3 parts of diluent, 0.2 parts of lubricant and 0.3 parts of antioxidant.
[0072] The reactive monomer in the polymer I is glycidyl methacrylate, the oil-soluble initiator is azobisisobutyronitrile, the dispersant is active calcium phosphate, the auxiliary dispersant is sodium dodecylbenzene sulfonate, and the molecular weight regulator is dodecyl mercaptan.
[0073] The polyolefin in the polymer II is homopolypropylene with a melt index of 3 (230°C, 2.16kg), a brand of T30S, and is sourced from Sinopec; the peroxide initiator is 1,1-bis(tert-butyl peroxide)-3,3,5-trimethylcyclohexane, the reactive monomer is itaconic acid, the diluent is methyl ethyl ketone, the lubricant is zinc stearate, and the antioxidant is triphenyl phosphite and 1010 in a 1:1 ratio.
[0074] The catalyst is 2-methylimidazole, the antioxidant is a compound of triphenyl phosphite and 1010 in a ratio of 1:1, the lubricant is a compound of pentaerythritol stearate and silicone in a ratio of 1:1, and the devolatilization aid is acetone.
[0075] The preparation method of the styrene-polyolefin functional polymer is the same as that of Example 1.
[0076] Example 6
[0077] Slightly different from Example 5, the polymer includes the following components by weight: 60 parts of polymer I, 40 parts of polymer II, 0.2 parts of catalyst, 0.4 parts of antioxidant, 0.2 parts of lubricant, and 1 part of devolatilizer. The rest are the same as Example 5.
[0078] Comparative Example 1
[0079] Referring to the method disclosed in U.S. Pat. No. 172384, anhydrous aluminum chloride was used as a catalyst to initiate an in-situ compatibilization reaction between PP and PS to prepare a PP-g-PS copolymer sample; wherein the weight ratio of PP to PS was 7:3, PP was a random copolymer polypropylene with a melt index of 7 (230°C, 2.16 kg), the brand was Yungsox 5060, provided by Formosa Plastics Corporation, and the melt index of PS was 2 (190°C, 2.16 kg).
[0080] Comparative Example 2
[0081] Referring to the method disclosed in U.S. Pat. No. 172384, anhydrous aluminum chloride was used as a catalyst to initiate an in-situ compatibilization reaction between LLDPE and PS to prepare a PS-g-LLDPE copolymer sample; wherein the weight ratio of LLDPE to PS was 3:7, the melt index of LLDPE was 20 (190°C, 2.16kg), the brand was LL6101XR, provided by ExxonMobil Corporation of the United States, and the melt index of PS was 2 (190°C, 2.16kg).
[0082] Comparative Example 3
[0083] Referring to the preparation of PP-g-PS copolymer by coordination polymerization-anionic polymerization method disclosed in Chinese patent CN101580614, propylene and p-allyltoluene are firstly subjected to coordination polymerization to prepare an intermediate, and then the benzyl carbon in the copolymer intermediate is lithiated by lithiation reaction, styrene is added, and anionic graft polymerization is carried out to obtain PP-g-PS copolymer.
[0084] Application Example 1
[0085] 10 parts of the samples in Example 1 and Comparative Example 1 were taken respectively, and blended and extruded with 70 parts of PP (Shanghai Secco Petrochemical, K8003), 30 parts of HIPS (Shanghai Secco Petrochemical, 622P), 10 parts of SEBS (Yueyang Petrochemical, YH503) and 0.5 parts of processing aid in a twin-screw extruder to obtain PP / PS alloy samples 1 and 2, respectively. The relevant test results are shown in Table 1.
[0086] Application Example 2
[0087] 5 parts of the samples in Example 2 and Comparative Example 2 were taken respectively, and blended and extruded with 30 parts of LLDPE (Sinopec, 7042), 70 parts of HIPS (Shanghai Secco Petrochemical, 622P), 5 parts of SEBS (Kraton, G1652) and 0.5 parts of processing aid in a twin-screw extruder to obtain PS / PE alloy samples 3 and 4, respectively. The relevant test results are shown in Table 1.
[0088] Application Example 3
[0089] 10 parts of the sample in Example 3 and SEBS (Kraton, G1652) were taken respectively, and blended with 50 parts of PP (Sabic, 575P), 50 parts of HIPS (Shanghai Secco Petrochemical, 622P) and 0.5 parts of processing aid in a twin-screw extruder for extrusion to obtain PP / PS alloy samples 5 and 6, respectively. The relevant test results are shown in Table 2.
[0090] Application Example 4
[0091] 10 parts of the sample in Example 4 and SBS (Kraton, D1102K) were taken respectively, and blended with 60 parts of PP (Sabic, 575P), 40 parts of HIPS (Shanghai Secco Petrochemical, 622P) and 0.5 parts of processing aid in a twin-screw extruder for extrusion to obtain PP / PS alloy samples 7 and 8, respectively. The relevant test results are shown in Table 2.
[0092] Application Example 5
[0093] Ten parts of the sample in Example 5 were blended and extruded with 60 parts of PP (Sabic, 575P), 40 parts of HIPS (Shanghai Secco Petrochemical, 622P) and 0.5 parts of processing aid in a twin-screw extruder to prepare PP / PS alloy sample 9; the other part was blended and extruded with only 60 parts of PP (Sabic, 575P), 40 parts of HIPS (Shanghai Secco Petrochemical, 622P) and 0.5 parts of processing aid in a twin-screw extruder without adding any compatibilizer or toughening agent to obtain PP / PS sample 10. The relevant test results are shown in Tables 2 and Figure 1 a, b.
[0094] Application Example 6
[0095] 5 parts of the samples in Example 5 and Example 6 and PP-g-MAH product (CMG5701, Jiayirong Polymer (Shanghai) Co., Ltd.) were taken respectively, and blended with 60 parts of PP (Sabic, 575P), 40 parts of HIPS (Shanghai Secco Petrochemical, 622P) and 0.5 parts of processing aid in a twin-screw extruder for extrusion to obtain PP / PS alloy samples 11, 12 and 13, respectively. The relevant test results are shown in Table 3.
[0096] Application Example 7
[0097] 5 parts of the samples in Example 1 and Comparative Example 3 were taken respectively, and blended and extruded with 70 parts of PP (Shanghai Secco Petrochemical, K8003), 30 parts of HIPS (Shanghai Secco Petrochemical, 622P), 10 parts of SEBS (Yueyang Petrochemical, YH503) and 0.5 parts of processing aid in a twin-screw extruder to obtain PP / PS alloy samples 14 and 15, respectively. The relevant test results are shown in Table 4.
[0098] Application Example 8
[0099] HIPS (Zhenjiang Chimei, PH-88) was taken as sample 16, and 10 parts of the POE-g-PP sample in Example 3 were compounded with 90 parts of HIPS (same brand) and 0.5 parts of processing aids and then blended and extruded in a twin-screw extruder to obtain a modified PS sample 17. Samples 16 and 17 were injection molded into ISO specimens and then immersed in a mixed solvent of ethyl acetate and ethanol in a mass ratio of 1:1. After 10 seconds, the specimens were taken out and the surface corrosion of the specimens was observed under a microscope. The relevant test results are shown in Figure 1 c, d.
[0100] The processing aids in the above formula are: 0.1 parts each of antioxidants 1010 and 168, and 0.3 parts of lubricant calcium stearate. Twin-screw extruder parameters: aspect ratio 40:1, screw diameter 35mm, temperature set to 200~230℃.
[0101] Performance Testing
[0102] Tensile strength: tested according to ISO 527 standard, test speed is 50mm / min;
[0103] Bending strength: tested according to ISO 178 standard, the test speed is 2mm / min;
[0104] Charpy notched impact strength: tested according to ISO 179-1 standard, impact energy is 4J;
[0105] Aging test: The injection molded specimens were placed in a thermal oxygen aging chamber at 150°C for 200 hours. After aging, the yellowness index of the specimens was tested according to ASTM E313 standard.
[0106] Sample microscopic morphology observation: Observe using scanning electron microscope;
[0107] Observation of sample surface corrosion morphology: Observe using an optical microscope.
[0108] The mechanical properties and performance tests after aging of the four samples prepared according to Application Examples 1 and 2 are shown in Table 1:
[0109] Table 1 Performance test data of application examples 1 and 2
[0110]
[0111] Table 2 Performance test data of application examples 3 to 5
[0112]
[0113] Table 3 Performance test data of application example 6
[0114]
[0115] Table 4 Performance test data of application example 7
[0116]
[0117] It can be seen from the data of Application Examples 1 and 2 in Table 1 that equal amounts of styrene-polyolefin functionalized polymers prepared in the embodiment and the comparative example are respectively added as compatibilizers in the same alloy formula system. From the basic mechanical property test data, there is little difference. The compatibilizer prepared by the method of the present invention has a slight advantage in the mechanical properties of the alloy system, especially the impact resistance of the alloy. However, the main difference is that, compared with the method adopted in the embodiment, since anhydrous aluminum chloride is used as a catalyst in the comparative example, it will cause the degradation of polystyrene, thereby deteriorating the anti-aging performance of the material. From the comparison of the yellowness index values of the materials before and after aging, it can be seen that the functional polymer prepared by the method of the present invention has more outstanding aging resistance.
[0118] The test data of Application Examples 3 and 4 in Table 2 illustrate that the styrene-polyolefin functional polymer prepared by the method of the present invention has better overall mechanical properties than conventional SEBS and SBS as compatibilizers / tougheners. Different from the relatively fixed styrene segments and olefin segments of SEBS or SBS, the molecular structure of the styrene-polyolefin functional polymer prepared by the present invention has a greater degree of freedom in adjustment, and can make polystyrene the main chain of the molecule and polyolefin designed as a side chain, or make polyolefin the main chain of the molecule and polystyrene designed as a side chain structure, so that more functionality can be achieved according to different specific applications.
[0119] From Table 2 and Figure 1 In the results of Application Example 5, it can be seen that the mechanical properties of the functional polymer prepared by the present invention are significantly improved compared with the comparative example without using the functional polymer, especially the impact performance is significantly improved. Figure 1 It can be seen that the PP / PS alloy without adding functional polymer (sample 10, Figure 1 (b) The microscopic phase state shows that the interface between the two phases is clear. The PS is distributed in the continuous phase in large blocks with a small amount of fine particles. Due to the poor adhesion between the two phases, the shear-dispersed PS particles are easy to aggregate, resulting in poor compatibility of the alloy system. The PP / PS alloy with the functional polymer of the present invention (sample 9, Figure 1 (a)), the dispersed phase size is significantly reduced, the pores are clear, the phase interface is fuzzy, and the phases are tightly bound, indicating that the polystyrene-polyolefin functional polymer has a good compatibilizing effect.
[0120] It can be seen from the test data of Application Example 6 in Table 3 that there will be certain differences in the presentation of the final results when selecting functional polymers with different molecular structures as the main chain. The functional polymers in Examples 5 and 6 used in this application case have opposite main chain and side chain structures. From the comprehensive mechanical properties of the product, it can be seen that the sample using Example 5 is better than the sample using Example 6. Therefore, a styrene-polyolefin functional polymer with a suitable structure can be selected according to the needs of the application scenario; in addition, a comparison is made between PP-g-MAH as a compatibilizer for PP / PS alloy and the functional polymer prepared by the method of the present invention. From the final test results, the mechanical properties of the product using PP-g-MAH are significantly lower than those of the functional polymer used by the method of the present invention. Therefore, it can be inferred that PP-g-MAH is not suitable for use as a compatibilizer for PP / PS alloy.
[0121] From the mechanical property comparison data of Application Example 7 in Table 4, it can be seen that the sample of Example 1 of the present invention and the sample of Comparative Example 3 are used as compatibilizers for PP / PS alloys for comparison. Although both can improve the compatibility of PP / PS alloys, the functional polymer prepared by the method of the present invention has more advantages in comprehensive performance in the alloy, and the preparation process of the compatibilizer itself is safer, simpler and more environmentally friendly.
[0122] from Figure 1 It can be seen from the optical microscope photo of Application Example 8 that HIPS itself has poor solvent resistance. After being kept in a mixed solvent of ethyl acetate and ethanol for only 10 seconds, obvious pits appeared on the surface of the product ( Figure 1 (c)); When 10 parts of POE-g-PS (the sample of Example 3) were added to HIPS and kept in the same solvent for the same time, the surface of the product was almost not corroded (( Figure 1 (d)), therefore, the styrene-polyolefin functional polymer of the present invention can significantly improve the chemical resistance of PS, and due to the similarity of the molecular chain structures of PS and PO-g-PS, the compatibility of the two after blending can also be well guaranteed.
[0123] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.
Claims
1. A styrene-polyolefin functional polymer, characterized in that: The polymer comprises the following components and weight parts: 30-70 parts of polymer I, 30-70 parts of polymer II, 0.01-1 parts of catalyst, 0.1-1 parts of antioxidant, 0.1-1 parts of lubricant, and 0.2-5 parts of devolatilizer; Wherein, polymer I is prepared by suspension polymerization in an aqueous medium from styrene, reactive monomer I, an oil-soluble initiator, a dispersant, a dispersant aid, and a molecular weight regulator in a weight ratio of (80-99): (1-20): (0.1-1.0): (0.1-2.0): (0.01-0.1): (0.1-1.0); the reactive monomer I is selected from one of methyl methacrylate, ethyl methacrylate, butyl methacrylate, and glycidyl methacrylate; The polymer II is prepared from polyolefin, peroxide initiator, reactive monomer II, diluent and processing aid in a weight ratio of 100: (0.01-2): (0.5-6): (0.1-5): (0.2-1.0); the reactive monomer II is selected from one or a combination of acrylic acid, methacrylic acid, acrylamide, methacrylic acid amide, maleic anhydride, fumaric acid, dibutyl maleate, citric acid and itaconic acid.
2. The styrene-polyolefin functional polymer according to claim 1, characterized in that: The oil-soluble initiator is an azo initiator, including at least one of azobisisobutyronitrile, azobisisoheptanenitrile or dimethyl azobisisobutyrate; the dispersant is at least one of polyvinyl alcohol, active calcium phosphate and hydroxyethyl cellulose; the co-dispersant is sodium dodecylbenzene sulfonate or sodium dodecyl sulfate; and the molecular weight regulator is dodecyl mercaptan.
3. The styrene-polyolefin functional polymer according to claim 1 or 2, characterized in that: The preparation of polymer I comprises: A1, mixing the styrene monomer, reactive monomer I, oil-soluble initiator, dispersant, dispersant aid, molecular weight regulator and water, reacting at 65-80° C. for 3-6 hours, heating to 85-90° C. for aging for 0.5-2 hours; the mass ratio of the total weight of monomers to water is (1-3):1; A2. After the reaction is completed, filter and wash, dry at 75-85°C to constant weight, and then sieve to obtain polymer I.
4. The styrene-polyolefin functional polymer according to claim 1, characterized in that: The polyolefin is selected from one or more of polybutene, polypropylene, polyethylene, ethylene-propylene copolymer, ethylene-butene copolymer, and ethylene-octene copolymer; the peroxide initiator is selected from dicumyl peroxide, benzoyl peroxide, p-chlorobenzoyl peroxide, di-tert-butyl peroxide isopropylbenzene, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexyne, 2,5-dimethyl-2,5-bis(peroxybenzene) The invention relates to a method for preparing the present invention which is characterized in that the present invention comprises one or more of the following: the first, the second, the third, the fourth, the fifth, the fifth, the sixth, the sixth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the ninth, the 5. The styrene-polyolefin functional polymer according to claim 1 or 4, characterized in that: The preparation of polymer II includes: uniformly mixing the polyolefin, peroxide initiator, reactive monomer II, diluent and processing aid, and then feeding into a reaction extruder, and after melt mixing, extrusion reaction and devolatilization, granulation and drying are performed to obtain polymer II.
6. The styrene-polyolefin functional polymer according to claim 1, characterized in that: The catalyst is selected from at least one of quaternary ammonium salts, quaternary phosphonium salts, tertiary amines, tertiary phosphorus and imidazole compounds.
7. The styrene-polyolefin functional polymer according to claim 1, characterized in that: The antioxidant is a combination of hindered phenol and phosphite antioxidants; the lubricant is at least one of fatty acid amides, silicones, and pentaerythritol stearate.
8. The styrene-polyolefin functional polymer according to claim 1, characterized in that: The devolatilizer is selected from at least one of anhydrous ethanol, acetone, supercritical CO2, deionized water, and N2.
9. A method for preparing a styrene-polyolefin functional polymer according to claim 1, characterized in that: The method comprises the following steps: S1, the polymer I, polymer II, catalyst, antioxidant, and lubricant are mixed evenly, and fed into a twin-screw extruder with a length-to-diameter ratio of (44-60):1 through a main feed port, with a processing temperature of 180-240°C and a rotation speed of 180-600rpm; S2, adding the devolatilizer through the injection port at the rear end of the twin-screw extruder, and discharging the residual small molecular substances and the devolatilizer in the reaction process through the devolatilization port; S3, after being extruded through a die head, water-cooled, and pelletized by a pelletizer, the styrene-polyolefin functional polymer is obtained.
10. Use of the styrene-polyolefin functional polymer according to claim 1, characterized in that: The polymer is used as a compatibilizer for polyolefin / polystyrene alloys, or as an auxiliary agent for improving the chemical resistance of polystyrene.
Citation Information
Patent Citations
Method for producing polythene / polystyrene alloy with capacity increasing of reaction in-situ
CN101402765A
Production of solutions of vinyl polymers in reactive monomers
CN101868481A
In-situ compatibilization polyolefin / polystyrene alloy and preparation method and application thereof
CN102643484A
Compatilizer and applications thereof
CN103421139A
Delustering agent for ABS and PC / ABS alloy and preparation method thereof
CN111303438A