Hydroxyl modified ethylene propylene diene monomer rubber and preparation method thereof
Through the olefin cross-metalysis reaction and ruthenium carbene-type catalyst, the unsaturation and grafting rate of ethylene propylene ternary rubber are improved, and the problems of low grafting rate and complex process during its modification process are solved, which is improved with polar rubber The blending properties and vulcanization speed simplify the process and reduce costs.
Patent Information
- Application Number
- CN202110570978.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-05-25
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-05-25
AI Technical Summary
The existing ethylene propylene ternary rubber has low grafting rate and unsaturation during the modification process, and the process conditions are harsh, which can easily lead to crosslinking, serious environmental pollution, high equipment costs, and difficult to blend well with polar polymers.
Using the olefin cross-metalysis reaction method, ethylene propylene ternary rubber is grafted with compounds derived from specific structures in the presence of ruthenium carbene catalyst to improve its unsaturation and grafting rate, and by increasing side chain double bonds The content increases the vulcanization rate.
The hydroxy-modified ethylene propylene ternary rubber with high unsaturation and grafting rate is achieved, which improves the blending performance and vulcanization speed with polar rubber, simplifies the process flow, and reduces environmental pollution and equipment costs.
Smart Images

Figure CN115386022B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of rubber, and in particular to a hydroxyl-modified ethylene propylene diene monomer rubber and a preparation method thereof. Background Art
[0002] EPDM (ethylene propylene diene monomer) rubber has excellent physical and chemical properties such as high elasticity, viscoelasticity, and electrical insulation, and is particularly well-known for its toughening of engineering plastics and its resistance to ozone aging. However, since EPDM is a non-polar rubber, it has poor oil resistance, chemical resistance, self-adhesion, and mutual adhesion. By combining it with diene rubbers (such as natural rubber, butadiene rubber, nitrile rubber, chloroprene rubber, etc.), it is expected to obtain a rubber with relatively good comprehensive performance. However, EPDM rubber is very different from most diene rubbers in terms of polarity and saturation, and is difficult to blend with polar polymers, so its application range is subject to certain restrictions.
[0003] The chemical modification of EPDM rubber is to introduce other atoms or groups into the molecular chain through the chemical reaction of rubber to make the molecular chain polar or change the flexibility, so as to improve the compatibility of EPDM rubber and diene rubber blends. That is, polar groups such as esters and acrylonitrile are connected to the main chain of EPDM rubber, and the modified EPDM rubber is used as a combined compatibilizer to expand the application field of EPDM rubber.
[0004] The grafting reaction is mainly based on thermomechanical chemical modification methods and solution modification. The rubber refining equipment commonly used in rubber processing can be used for this modification treatment. However, it is difficult to remove residual monomers and initiators after the modification is completed. The resulting product has a strong odor, the process conditions are demanding, the side reactions are not easy to control, it is easy to cause cross-linking of the rubber, and the equipment cost is relatively high.
[0005] Solution modification mainly involves chemical modification of EPDM rubber in chemical solvents or aqueous emulsions by the initiation of benzoyl peroxide, etc. However, the existing solution modification method requires the use of a wide variety of catalysts and additives in the production process, which makes post-reaction treatment difficult and causes serious environmental pollution. In addition, the reaction process is still a free radical reaction, with a long initiation and reaction time, and the reaction process is difficult to control, and is prone to side reactions such as cross-linking.
[0006] Therefore, it is particularly important to modify EPDM rubber to enhance its compatibility with polar polymers. Summary of the invention
[0007] The purpose of the present invention is to overcome the problems of low grafting rate and unsaturation degree of modified EPDM rubber in the prior art, and to provide a hydroxyl modified EPDM rubber and a preparation method thereof, wherein the modified EPDM rubber has high unsaturation degree and grafting rate and high vulcanization speed.
[0008] In order to achieve the above object, the first aspect of the present invention provides a hydroxyl-modified EPDM rubber, wherein the hydroxyl-modified EPDM rubber contains a first structural unit provided by ethylene, a second structural unit provided by propylene and a third structural unit provided by a non-conjugated diene monomer, and at least part of the third structural unit contains a grafted group derived from a compound having a structure represented by formula (1);
[0009]
[0010] In formula (1), n1 is an integer of 1-20, and m1 is an integer of 2-40.
[0011] The second aspect of the present invention provides a method for preparing a hydroxyl-modified EPDM rubber, wherein the preparation method comprises: contacting the EPDM rubber with a compound derived from a structure represented by formula (2) in an organic solvent under the conditions of an olefin cross-metathesis reaction in the presence of a ruthenium carbene catalyst, wherein the EPDM rubber contains a first structural unit provided by ethylene, a second structural unit provided by propylene, and a third structural unit provided by a non-conjugated diene monomer;
[0012]
[0013] In formula (2), n2 is an integer of 1-20, and m2 is an integer of 2-40.
[0014] The third aspect of the present invention provides a hydroxyl-modified EPDM rubber prepared by the aforementioned preparation method.
[0015] Through the above technical solution, the technical solution provided by the present invention has the following beneficial effects:
[0016] The present invention adopts a ruthenium carbene catalyst with a structure shown in formula (3) to catalyze the olefin cross-metathesis reaction of ethylene propylene diene rubber and a compound derived from the structure shown in formula (1), so that the unsaturation degree of the prepared modified ethylene propylene diene rubber is 0.56-1 mol / kg.
[0017] Furthermore, the hydroxyl-modified EPDM rubber provided by the present invention also has a high grafting rate. Specifically, based on the weight of the modified EPDM rubber, the grafting rate of the modified EPDM rubber provided by the present invention is 1.1-13.5% by weight.
[0018] Furthermore, compared with the unmodified EPDM rubber, the vulcanization rate of the hydroxyl-modified EPDM rubber provided by the present invention is improved to a certain extent. The possible reason is that after the present invention subjects the compound derived from the structure shown in formula (1) to the EPDM rubber through an olefin ring-opening cross-decomposition reaction, the double bond content of the side chain of the EPDM rubber can be increased, which is beneficial to the vulcanization process, thereby improving the vulcanization rate of the modified EPDM rubber.
[0019] Furthermore, the hydroxyl-modified EPDM rubber provided by the present invention has a good compatibilizing effect when the EPDM rubber and the polar rubber are used together.
[0020] Furthermore, the preparation method of the hydroxyl-modified EPDM rubber provided by the present invention has the characteristics of rapid reaction and simple and easy implementation.
[0021] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION
[0022] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0023] According to a first aspect of the present invention, the present invention provides a hydroxyl-modified EPDM rubber, wherein the hydroxyl-modified EPDM rubber contains a first structural unit provided by ethylene, a second structural unit provided by propylene, and a third structural unit provided by a non-conjugated diene monomer, and at least part of the third structural unit contains a grafted group derived from a compound having a structure represented by formula (1);
[0024]
[0025] In formula (1), n1 is an integer of 1-20, and m1 is an integer of 2-40.
[0026] According to the present invention, the improvement of the present invention mainly lies in that compared with the unmodified EPDM rubber, the modified EPDM rubber provided by the present invention introduces hydroxyl groups into the side chains, the polarity of the EPDM rubber is improved, and the double bond content in the side chains of the modified EPDM rubber is increased, the vulcanization speed is improved, and the modified EPDM rubber has a good volume expansion effect when the EPDM rubber is used in combination with the polar rubber. In addition, in the preparation method provided by the present invention, the role of the organic solvent is to dissolve the EPDM rubber, the catalyst, and the modified monomer into a homogeneous solution, increase the contact probability of the catalyst, the monomer and the EPDM rubber, and improve the grafting efficiency; the advantage of the ruthenium carbene catalyst is that the initiation activity is high and the reaction conditions are relatively mild.
[0027] According to the present invention, in formula (1), n1 is an integer of 3-10, and m1 is an integer of 6-20; more preferably, the compound of the structure shown in formula (1) is selected from one or more of 4-pentenyl-1-ol, 9-decenyl-1-ol, 2-propenyl-1-ol, 5-hexenyl-1-ol and 7-octenyl-1-ol; further preferably, the compound of the structure shown in formula (1) is one or more of 4-pentenyl-1-ol, 9-decenyl-1-ol and 2-propenyl-1-ol.
[0028] According to the present invention, in order to further improve the vulcanization speed of the modified EPDM rubber, the unsaturation of the hydroxyl modified EPDM rubber is 0.56-1 mol / kg, preferably 0.56-0.87 mol / kg; more preferably 0.73-0.87 mol / kg, and further preferably 0.8-0.87 mol / kg. In addition, in the present invention, it should be noted that the unsaturation of the modified EPDM rubber can be, for example, 0.56 mol / kg, 0.58 mol / kg, 0.73 mol / kg, 0.77 mol / kg, 0.8 mol / kg, 0.82 mol / kg, 0.84 mol / kg, 0.85 mol / kg, 0.87 mol / kg and 1 mol / kg, and any value in the range formed by any two of these point values.
[0029] The unsaturation degree of the hydroxyl-modified EPDM rubber in the present invention is determined by iodine titration.
[0030] In the present invention, the third structural unit may be entirely derived from the structural compound shown in formula (2), or part of the third structural unit may be derived from the structural compound shown in formula (2). In order to further improve the vulcanization rate of the modified EPDM rubber, preferably, based on the weight of the hydroxyl-modified EPDM rubber, the grafting rate of the modified EPDM rubber is 1.1-13.5% by weight, preferably 2.5-13.5% by weight, more preferably 3.3-13.5% by weight, more preferably 4.3-13.5% by weight, further preferably 7.5-13.5% by weight, and most preferably 10-13.5% by weight. In addition, in the present invention, it should be noted that the grafting rate of the hydroxyl-modified EPDM rubber can be, for example, 1.1 wt%, 2.5 wt%, 3.3 wt%, 3.9 wt%, 4.3 wt%, 4.5 wt%, 4.9 wt%, 5.1 wt%, 5.2 wt%, 7.5 wt%, 10 wt% and 13.5 wt%, and any value in the range formed by any two of these point values.
[0031] In the present invention, the grafting rate is the mass content of the compound derived from the structure represented by formula (1) in the modified EPDM rubber.
[0032] According to the present invention, the third monomer may be a non-conjugated diene commonly used in the art, so as to enable the ethylene propylene diene rubber to undergo an olefin cross-decomposition reaction with the compound of the structure represented by formula (2), for example, it may be one or more of 1,4-hexadiene, dicyclopentadiene (DCPD) and 5-ethylidene-2-norbornene. In order to obtain a higher grafting rate to increase the vulcanization speed of the modified ethylene propylene diene rubber, dicyclopentadiene is preferably used.
[0033] Preferably, when the third monomer is dicyclopentadiene (DCPD), at least part of the third structural unit containing the grafted group has a structure shown in formula (I),
[0034]
[0035] In formula (I), n1 is an integer of 1-20, and m1 is an integer of 2-40.
[0036] When the third monomer is dicyclopentadiene (DCPD), in order to further improve the vulcanization speed of the modified EPDM rubber, at least part of the third structural unit also contains a structural unit represented by formula (II),
[0037]
[0038] In the present invention, it should be noted that the structural units in the EPDM rubber are mainly ethylene structural units of the structure shown in formula (III) and propylene structural units of the structure shown in formula (IV), and the structural units derived from the third monomer are called third structural units.
[0039]
[0040] According to the modified EPDM rubber of the present invention, preferably, the modified EPDM rubber is obtained by contacting the EPDM rubber with a compound derived from the structure represented by formula (1) under olefin cross-metathesis reaction conditions.
[0041] According to the modified EPDM rubber of the present invention, the EPDM rubber is capable of undergoing olefin cross-metathesis reaction with the compound derived from the structure represented by formula (1), and based on the weight of the modified EPDM rubber, the content of the first structural unit provided by ethylene is 50-70wt%, and the content of the third structural unit provided by the non-conjugated diene monomer is 4-8wt%; preferably, based on the total weight of the modified EPDM rubber, the content of the first structural unit provided by ethylene is 55-65wt%, and the content of the third structural unit provided by the non-conjugated diene monomer is 5-7wt%.
[0042] According to the present invention, the weight average molecular weight of the modified EPDM rubber is 100,000-400,000, preferably 120,000-300,000, and preferably 120,000-200,000.
[0043] The weight average molecular weight of the modified EPDM rubber in the present invention is measured by gel permeation chromatography (GPC) method.
[0044] The modified EPDM rubber is prepared by the method described below.
[0045] The second aspect of the present invention provides a method for preparing a hydroxyl-modified EPDM rubber, wherein the preparation method comprises: contacting the EPDM rubber with a compound derived from a structure represented by formula (2) in an organic solvent under the conditions of an olefin cross-metathesis reaction in the presence of a ruthenium carbene catalyst, wherein the EPDM rubber contains a first structural unit provided by ethylene, a second structural unit provided by propylene, and a third structural unit provided by a non-conjugated diene monomer;
[0046]
[0047] In formula (2), n2 is an integer of 1-20, and m2 is an integer of 2-40.
[0048] According to the present invention, preferably, n2 is an integer of 3-10, and m2 is an integer of 6-20; more preferably, the compound of the structure shown in formula (1) is selected from one or more of 4-pentene-1-ol, 9-decene-1-ol, 2-propylene-1-ol, 5-hexene-1-ol and 7-octen-1-ol; further preferably, the compound of the structure shown in formula (1) is one or more of 4-pentene-1-ol, 9-decene-1-ol and 2-propylene-1-ol. In addition, in the present invention, it should be noted that 2-propylene-1-ol, also known as allyl alcohol, has a CAS number of 107-18-6.
[0049] According to the present invention, the catalyst has a structure shown in formula (3);
[0050]
[0051] According to the present invention, in formula (3), R1 is hydrogen, C2-C 20 Substituted or unsubstituted alkenyl, C2-C 20 Substituted or unsubstituted alkynyl, C1-C 20 Substituted or unsubstituted alkyl, C6-C 20 Substituted or unsubstituted aryl, C2-C 20 Substituted or unsubstituted carboxylate group, C1-C 20 Substituted or unsubstituted alkoxy, C2-C 20 Substituted or unsubstituted alkenyloxy, C2-C 20 Substituted or unsubstituted alkynyloxy, C6-C 20 Substituted or unsubstituted aryloxy, C1-C 20 Substituted or unsubstituted alkylthio, C1-C 20 Substituted or unsubstituted alkylsulfonyl or C1-C 20 a substituted or unsubstituted alkylsulfinyl group;
[0052] According to the present invention, in formula (3), X1 and X2 can be various common anionic ligands, for example, X1 and X2 are each independently anionic ligands.
[0053] According to the present invention, in formula (3), L1 and L2 are each independently a neutral ligand, and optionally L1 and L2 can be connected to each other to form a bidentate neutral ligand.
[0054] According to the present invention, preferably, R1 is C6-C 20 The substituted or unsubstituted aryl group is preferably a phenyl group.
[0055] According to the present invention, preferably, X1 and X2 are each independently a halogen ion, preferably a chloride ion.
[0056] According to the present invention, preferably, L1 and L2 are each independently a phosphine, an amine, a thioether, a carbene, or a substituted or unsubstituted imidazolidine. Preferably, L1 and L2 are each independently a phosphine, a carbene, or a substituted or unsubstituted imidazolidine.
[0057] According to the present invention, more preferably, R1 is phenyl, L1 is substituted or unsubstituted imidazolidine, L2 is phosphine, and X1 and X2 are chloride ions.
[0058] According to the present invention, the phosphine can be a compound in which the hydrogen in various phosphine molecules is partially or completely replaced by organic groups, preferably a trialkylphosphine, wherein the organic groups are the same or different and each can be selected from chain alkyl (such as C1-C 10 Alkyl) or substituted or unsubstituted cycloalkyl (such as C6-C 12 substituted or unsubstituted cycloalkyl), preferably each selected from substituted or unsubstituted cycloalkyl, more preferably cyclohexyl. Specifically, examples of the phosphine may include, but are not limited to, one or more of trimethylphosphine, triethylphosphine, tri-n-butylphosphine, tri-sec-butylphosphine, tripropylphosphine, tripentylphosphine, trihexylphosphine, trioctylphosphine and tricyclohexylphosphine.
[0059] According to the present invention, L1 is a substituted or unsubstituted imidazolidine, and L1 is an imidazolidine of the structure shown in formula (4),
[0060]
[0061] In formula (4), R2 and R3 are the same or different and are each independently C6-C 20 a substituted or unsubstituted aryl group;
[0062] Preferably, R2 and R3 are the same or different and are each independently R4, R5, R6, R7 and R8 are each independently selected from hydrogen or C1-C5 substituted or unsubstituted alkyl;
[0063] Preferably, in formula (3), R2 and R3 are
[0064] More preferably, R2 and R3 are each
[0065] In the present invention, specific examples of the C1-C5 alkyl group may include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl and n-pentyl.
[0066] In a preferred embodiment of the present invention, in formula (3), R1 is a phenyl group, L1 is a substituted or unsubstituted imidazolidine, L2 is a phosphine, and X1 and X2 are chloride ions.
[0067] In a more preferred embodiment of the present invention, in formula (3), R1 is phenyl, L1 is L2 is a trialkylphosphine, and X1 and X2 are chloride ions.
[0068] According to the present invention, in order to make the catalyst have a better catalytic effect, it is further preferred that the catalyst with the structure shown in formula (3) has the structure shown in formula (5):
[0069]
[0070] In the above formula (5), PCy3 represents tricyclohexylphosphine, and Ph represents a phenyl group.
[0071] The catalyst represented by the above formula (5) is commercially available.
[0072] According to the present invention, the substituted or unsubstituted C2-C 20 The alkenyl group may be straight chain or branched, and specific examples may include, but are not limited to, ethenyl, propenyl, butenyl, pentenyl, hexenyl, heptenyl, octenyl, nonenyl, decenyl, undecenyl, and dodecenyl.
[0073] According to the present invention, the substituted or unsubstituted C2-C 20 The alkynyl group may be linear or branched, and specific examples may include, but are not limited to, ethynyl, propynyl, butynyl, pentynyl, hexynyl, heptynyl, octynyl, nonynyl and decynyl.
[0074] According to the present invention, substituted or unsubstituted C1-C 20 The alkyl group may be linear or branched, and specific examples may include, but are not limited to, methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, and octadecyl.
[0075] According to the present invention, substituted or unsubstituted C6-C 20 Specific examples of the aryl group may include, but are not limited to, phenyl, methylphenyl, and naphthyl.
[0076] According to the present invention, the substituted or unsubstituted C2-C 20 The carboxylate group refers to the carboxylate group in the molecular chain Specific examples may include, but are not limited to, methyl propionate, ethyl acetate, and propyl formate.
[0077] According to the present invention, substituted or unsubstituted C1-C 20Specific examples of the alkoxy group may include, but are not limited to, methoxy, ethoxy, propoxy, isopropoxy, butoxy, sec-butoxy, tert-butoxy, pentyloxy, hexyloxy, heptyloxy, octyloxy, nonyloxy, decyloxy, and octadecyloxy.
[0078] According to the present invention, the substituted or unsubstituted C2-C 20 Specific examples of the alkenyloxy group may include, but are not limited to, 1-allyloxy, 2-allylbutoxy, and 1-allylpentoxy.
[0079] According to the present invention, the substituted or unsubstituted C2-C 20 Specific examples of the alkynyloxy group may include, but are not limited to, 1-propargyloxy, 2-ynylbutoxy, 1-ynylpentoxy.
[0080] According to the present invention, substituted or unsubstituted C6-C 20 Specific examples of the aryloxy group may include, but are not limited to, phenoxy and naphthyloxy.
[0081] According to the present invention, substituted or unsubstituted C1-C 20 The alkylthio group is a straight or branched C1-C 20 Specific examples of alkyl include, but are not limited to, methylthio (CH3-S-), ethylthio, propylthio, butylthio, pentylthio, 1-methylpropylthio, 2-methylpropylthio and 1,1-dimethylethylthio.
[0082] According to the present invention, substituted or unsubstituted C1-C 20 Specific examples of the alkylsulfonyl group may include, but are not limited to, methylsulfonyl, ethylsulfonyl, propylsulfonyl, butylsulfonyl, and nonylsulfonyl.
[0083] According to the present invention, substituted or unsubstituted C1-C 20 Specific examples of the alkylsulfinyl group may include, but are not limited to, methylsulfinyl and ethylsulfinyl.
[0084] According to the present invention, the third monomer may be a non-conjugated diene commonly used in the art, so as to enable the ethylene propylene diene rubber to undergo an olefin cross-decomposition reaction with the compound of the structure represented by formula (2), for example, it may be one or more of 1,4-hexadiene, dicyclopentadiene (DCPD) and 5-ethylidene-2-norbornene. In order to obtain a higher grafting rate to improve the vulcanization speed and compatibilization of the modified ethylene propylene diene rubber, dicyclopentadiene (DCPD) is preferred.
[0085] According to the present invention, the amount of the EPDM rubber, the compound of the structure shown in formula (2) and the catalyst can vary within a wide range, as long as the purpose of rapid reaction and obtaining a modified EPDM rubber with a target saturation and a high grafting rate can be achieved. Relative to 100 parts by weight of the EPDM rubber, the amount of the compound derived from the structure shown in formula (2) is 0.05-40 parts by weight, preferably 1-25 parts by weight, and more preferably 9-18 parts by weight; the amount of the catalyst is 0.05-10 parts by weight, preferably 0.2-5 parts by weight, and more preferably 0.5-5 parts by weight.
[0086] According to the present invention, the EPDM rubber is based on the ability to undergo olefin cross-metathesis reaction with the compound of the structure represented by formula (2), the content of ethylene structural units in the EPDM rubber is 50-70 weight%, and the content of structural units derived from the third monomer is 4-8 weight%. Preferably, based on the total weight of the EPDM rubber, the content of the first structural unit provided by ethylene in the EPDM rubber is 55-65 weight%, and the content of the third structural unit provided by the non-conjugated diene monomer is 5-7 weight%.
[0087] In the present invention, based on the weight of the modified EPDM rubber, the total content of the first structural unit provided by ethylene, the second structural unit provided by propylene and the third structural unit provided by the non-conjugated diene monomer in the modified EPDM rubber is 100wt%.
[0088] Preferably, the weight average molecular weight of the EPDM rubber is 100,000-400,000, preferably 120,000-300,000, and more preferably 120,000-200,000.
[0089] According to the present invention, the cross-metathesis reaction of olefins is preferably carried out under an inert atmosphere. The inert atmosphere refers to a gas that does not participate in the reaction, such as nitrogen and one or more gases of the zeroth group of the periodic table, such as argon.
[0090] According to the present invention, the conditions for the cross-metathesis reaction of olefins include: a reaction temperature of 0-150° C., preferably 20-100° C., more preferably 70-100° C. The reaction time can be reasonably selected according to the reaction temperature, for example, the reaction time is 0.1-5h, preferably 0.1-3h.
[0091] In the present invention, the reaction is carried out under the temperature and time conditions, which has the advantage of higher grafting efficiency. If the temperature is too high, the catalyst stability decreases and the grafting efficiency decreases; if the temperature is too low, the catalyst initiation is slow and the grafting efficiency decreases.
[0092] According to the present invention, the addition method of the catalyst is not particularly limited, and the catalyst can be added to the reaction system of EPDM rubber and the compound of the structure shown in formula (2) in a one-time addition method or in multiple addition methods. Considering that the one-time addition of the catalyst easily causes the compound of the structure shown in formula (2) in the reaction system to undergo side reactions, it is preferably added in multiple addition methods. More preferably, the catalyst is added to the reaction system in 2-6 times, and the time interval between two adjacent additions is 3-15min, and the difference between the amount of the catalyst added in any two times accounts for less than 5% by weight of the total amount of the catalyst added. Adding the catalyst in this way is beneficial to improving the grafting rate of the modified EPDM rubber. Further preferably, in order to make the catalyst have a better catalytic effect, the catalyst is added to the reaction system in the form of a solution (preferably the catalyst is dissolved in the organic solvent) in 2-6 times, and the time interval between two adjacent additions is 3-15min, and the difference between the amount of the catalyst added in any two times accounts for less than 5% by weight of the total amount of the catalyst added. Adding the catalyst in this way is beneficial to improving the grafting rate and unsaturation of the modified EPDM rubber.
[0093] According to the present invention, the organic solvent for preparing the modified EPDM rubber is selected from toluene, xylene, chlorobenzene, C6-C 12 Cycloalkanes, C5-C 10 The organic solvent is one or more of straight-chain alkanes, tetrahydrofuran, acetone and 1,4-dioxane. In a further preferred case, the organic solvent is one or more of toluene, xylene, chlorobenzene, cyclohexane, n-hexane, tetrahydrofuran, acetone and 1,4-dioxane; and toluene and / or xylene are most preferred. These solvents can be used alone or in combination.
[0094] According to the present invention, relative to 100 parts by weight of the EPDM rubber, the amount of the organic solvent is 85-3000 mL.
[0095] In addition, in the present invention, the organic solvent defined above is used, which has the effect of promoting the modified grafting reaction. If the organic solvent of the present invention is not used, the grafting efficiency will be reduced.
[0096] According to the present invention, the preparation method of the modified EPDM rubber further comprises a purification step. The purification step may be a conventional purification step in the art, for example, filtering the reaction solution obtained after the reaction with a nickel mesh, adding acetone to the filtrate to form a precipitate, and then filtering, washing and drying the obtained precipitate.
[0097] The third aspect of the present invention provides a hydroxyl-modified EPDM rubber prepared by the method described above.
[0098] In the following preparation examples and embodiments, the performance measurements involved are as follows:
[0099] (1) The grafting rate was determined by the following method:
[0100] Add measured amounts of ethylene-propylene rubber (W1 / g) and xylene to a nitrogen-protected reaction flask. After the ethylene-propylene rubber is completely dissolved, add the compound derived from the structure shown in formula (2), and then add the catalyst solution of formula (5) in batches. After the reaction is completed for a certain period of time, the reaction product is precipitated with acetone, and the residual reactants in the reaction flask are dissolved with an appropriate amount of xylene and precipitated with acetone. After all the precipitates are extracted with DMF Soxhlet, they are vacuum dried at 60°C to obtain the grafted product. The grafted product is weighed (W2 / g), and the grafting rate is calculated according to the following formula:
[0101]
[0102] (2) The unsaturation of modified EPDM rubber is determined by iodine titration. The specific method is as follows: accurately weigh 2 grams of modified EPDM rubber sample, place it in a 250 mL ground-mouth conical flask, add 50 mL of CCl4 to dissolve the sample, add 20 mL of iodine bromide (IBr) solution with a pipette, shake it thoroughly and place it in a dark place for 1 hour, then add 10 mL of 10 wt% potassium iodide solution, shake it well, and titrate it with 0.1 N sodium thiosulfate standard solution until the solution turns yellow, then add 5 mL of starch indicator, and continue titrating until the blue color disappears, which is the end point. Perform a blank test at the same time. The unsaturation is calculated as follows:
[0103]
[0104] In the formula, V0: the volume of sodium thiosulfate standard solution consumed in the blank test, mL; V: the volume of sodium thiosulfate standard solution consumed by the sample, mL; C: the concentration of sodium thiosulfate standard solution, mol / L; m: the mass of the sample, g. The unit of unsaturation in the formula is mol / kg.
[0105] (3) The weight average molecular weight of the modified EPDM rubber was determined by gel permeation chromatography (GPC) using a Waters 1515 Isocratic HPLC gel chromatograph.
[0106] EPDM ESPRENE 305, purchased from Sumitomo, Japan, the EPDM has an ethylene structural unit content of 65 wt%, a third structural unit content of 7 wt%, a weight average molecular weight of 120,000, and the non-conjugated diene monomer is dicyclopentadiene (DCPD);
[0107] EPDM 3280, purchased from Yanshan Petrochemical Company, the content of ethylene structural units in the EPDM is 55% by weight, the content of the third structural unit provided by the non-conjugated diene monomer is 5% by weight, the weight average molecular weight is 300,000, and the non-conjugated diene monomer is ENB;
[0108] Catalyst I: having the structure shown below, purchased from Bailingwei Technology Co., Ltd.;
[0109] Wherein, PCy3 represents tricyclohexylphosphine, and Ph represents phenyl;
[0110] Catalyst II: having the structure shown below, purchased from Bailingwei Technology Co., Ltd.;
[0111] Wherein, PCy3 represents tricyclohexylphosphine, and Ph represents phenyl;
[0112] Catalyst III: having the structure shown below, purchased from Bailingwei Technology Co., Ltd.;
[0113]
[0114] Among them, L is PCy3 represents tricyclohexylphosphine;
[0115] Carbon black N550, purchased from Shanghai Cabot Chemical Co., Ltd.;
[0116] ASTM103# oil, purchased from Ningbo Xiejin Chemical Co., Ltd.;
[0117] Accelerator TMTD, purchased from Shanghai Jingyi Rubber Technology Co., Ltd.;
[0118] Sulfur, purchased from Shijiazhuang Ruituo Chemical Technology Co., Ltd.;
[0119] Nitrile rubber: 3945, purchased from LANXESS;
[0120] EPDM: 2450, purchased from LANXESS;
[0121] Other raw materials used in the examples and comparative examples are all commercially available.
[0122] Example 1
[0123] This embodiment is used to illustrate the modified EPDM rubber and the preparation method thereof provided by the present invention.
[0124] 9 g of EPDM rubber (ESPRENE 305, purchased from Sumitomo, Japan, the content of ethylene structural units in the EPDM rubber is 65 wt%, the content of structural units derived from the third monomer is 7 wt%, and the weight average molecular weight is 120,000, the third monomer is dicyclopentadiene (DCPD), 1.1 g of 2-propylene-1-ol (purchased from J&K Technology Co., Ltd., the same below) are dissolved in 100 mL of xylene solution under N2 protection until they are completely dissolved to form a reaction system; at the same time, 0.045 g of a catalyst having a structure represented by formula (5) (purchased from J&K Technology Co., Ltd., the same below) is weighed and dissolved in 10 mL of xylene solution to obtain a catalyst solution C1.
[0125] The obtained reaction system was heated to 70°C, and 2 mL of catalyst solution C1 was first added to the reaction system. After the reaction for 5 minutes, the remaining 8 mL of catalyst solution C1 was evenly divided into 4 parts, and added to the reaction system in the manner of adding one part every 5 minutes. After the last part of catalyst solution C1 was added to the reaction system for 5 minutes, the reaction was stopped. The total reaction time was 30 minutes. After the reaction was completed, the reaction solution was filtered with a nickel mesh while hot, and acetone was added to the filtrate to remove impurities and precipitate. The precipitate was separated and washed with acetone until the filtrate was clear. The precipitate was placed in a vacuum oven at 60°C and dried for 14 hours to obtain modified EPDM rubber A1. The properties of the modified EPDM rubber were analyzed and measured, and the results are shown in Table 1.
[0126]
[0127] Example 2
[0128] The modified EPDM rubber was prepared by the same method as in Example 1, except that the reaction system was heated to 70°C, and then 10 mL of the catalyst solution C1 was added to the reaction system at one time and reacted for 30 min. The modified EPDM rubber A2 was obtained. The properties of the modified EPDM rubber were analyzed and measured, and the results are shown in Table 1.
[0129] Example 3
[0130] The modified EPDM rubber was prepared by the same method as in Example 2, except that the reaction system was heated to 70°C, and then 10 mL of the catalyst solution C1 was added to the reaction system twice, the addition time was when the reaction system was heated to 70°C, i.e., when the reaction started and after the reaction was carried out for 15 minutes, each addition amount was 5 mL, and the reaction was stopped after the reaction for 30 minutes. The modified EPDM rubber A3 was obtained. The properties of the modified EPDM rubber were analyzed and measured, and the results are shown in Table 1.
[0131] Comparative Example 1
[0132] EPDM rubber (ESPRENE 305, purchased from Sumitomo, Japan, the content of ethylene structural units in the EPDM rubber is 65% by weight, the content of structural units derived from the third monomer is 7% by weight, the weight average molecular weight is 120,000, and the third monomer is dicyclopentadiene (DCPD)) that is, unmodified EPDM rubber is used as reference EPDM rubber D1, and the reference EPDM rubber D1 is analyzed and measured. The results are shown in Table 1.
[0133] Example 4
[0134] This embodiment is used to illustrate the modified EPDM rubber and the preparation method thereof provided by the present invention.
[0135] The modified EPDM rubber was prepared by the same method as in Example 1, except that the reaction time was 1 hour, that is, the reaction was stopped 35 minutes after the last catalyst solution was added to the reaction system. The modified EPDM rubber A4 was obtained. The properties of the modified EPDM rubber were analyzed and measured, and the results are shown in Table 1.
[0136] Example 5
[0137] The modified EPDM rubber was prepared by the same method as in Example 1, except that the reaction system was heated to 40° C. to obtain the modified EPDM rubber A5. The properties of the modified EPDM rubber were analyzed and measured, and the results are shown in Table 1.
[0138] Example 6
[0139] The modified EPDM rubber was prepared in the same manner as in Example 1, except that 0.82 g of 2-propylene-1-ol was added to obtain the modified EPDM rubber A6. The properties of the modified EPDM rubber were analyzed and measured, and the results are shown in Table 1.
[0140] Example 7
[0141] The modified EPDM rubber was prepared by the same method as in Example 1, except that 0.08 g of the catalyst having the structure shown in formula (5) was weighed and dissolved in 10 mL of xylene solution, and the mixture was divided into 5 portions, each of which was added in the same manner as in Example 1 to obtain modified EPDM rubber A7. The properties of the modified EPDM rubber were analyzed and measured, and the results are shown in Table 1.
[0142] Example 8
[0143] This embodiment is used to illustrate the modified EPDM rubber and the preparation method thereof provided by the present invention.
[0144] 9 g of EPDM rubber (ESPRENE 305, purchased from Sumitomo, Japan, the content of ethylene structural units in the EPDM rubber is 65 wt%, the content of structural units derived from the third monomer is 7 wt%, the weight average molecular weight is 120,000, and the third monomer is dicyclopentadiene (DCPD)) and 0.1 g of 2-propylene-1-ol are dissolved in 100 mL of xylene solution under N2 protection until they are completely dissolved to form a reaction system; at the same time, 0.45 g of a catalyst having a structure represented by formula (5) is weighed and dissolved in 10 mL of xylene solution to obtain a catalyst solution C8.
[0145] The reaction system was heated to 20°C, and 2 mL of catalyst solution C8 was first added to the reaction system. After the reaction lasted for 5 minutes, the remaining 8 mL of catalyst solution C8 was evenly divided into 4 portions and added to the reaction system in the manner of adding one portion every 5 minutes. After the last portion of catalyst solution C8 was added to the reaction system for 5 minutes, the reaction was stopped. The total reaction time was 1 hour. After the reaction was completed, the reaction solution was filtered with a nickel mesh while hot, and acetone was added to the filtrate to remove impurities and precipitate. The precipitate was separated and washed with acetone until the filtrate was clear. The precipitate was placed in a vacuum oven at 60°C and dried for 14 hours to obtain modified EPDM rubber A8. The properties of the modified EPDM rubber were analyzed and measured, and the results are shown in Table 1.
[0146] Example 9
[0147] This embodiment is used to illustrate the modified EPDM rubber and the preparation method thereof provided by the present invention.
[0148] 9 g of EPDM rubber (3280, purchased from Yanshan Petrochemical Company, the content of ethylene structural units in the EPDM rubber is 55 wt%, the content of structural units derived from the third monomer is 5 wt%, the weight average molecular weight is 300,000, and the third monomer is ENB) and 0.55 g of 2-propylene-1-ol are dissolved in 100 mL of xylene solution under N2 protection until they are completely dissolved to form a reaction system; at the same time, 0.018 g of a catalyst having a structure represented by formula (5) is weighed and dissolved in 10 mL of xylene solution to obtain a catalyst solution C9.
[0149] The reaction system was heated to 100°C, 2 mL of catalyst solution C9 was added to the reaction system, and after reacting for 15 minutes, the remaining 8 mL of catalyst solution was evenly divided into 4 portions, and added to the reaction system in the manner of adding one portion every 15 minutes. After the last portion of catalyst solution was added to the reaction system for 105 minutes, the reaction was stopped, and the total reaction time was 3 hours. After the reaction was completed, the reaction solution was filtered with a nickel mesh while hot, and acetone was added to the filtrate to remove impurities and precipitate. The precipitate was separated, and the precipitate was washed with acetone until the filtrate was clear. The precipitate was placed in a vacuum oven at 60°C and dried for 14 hours to obtain modified EPDM rubber A9. The properties of the modified EPDM rubber were analyzed and measured, and the results are shown in Table 1.
[0150] Comparative Example 2
[0151] EPDM rubber (3280, purchased from Yanshan Petrochemical Company, the content of ethylene structural units in the EPDM rubber is 55% by weight, the content of structural units derived from the third monomer is 5% by weight, the weight average molecular weight is 300,000, and the third monomer is ENB) that is, unmodified EPDM rubber is used as reference EPDM rubber D2, and the reference EPDM rubber D2 is analyzed and measured. The results are shown in Table 1.
[0152] Example 10
[0153] The modified EPDM rubber was prepared by the same method as in Example 1, except that the catalyst having the structure shown in formula (6) (commercially available from J&K Technology Co., Ltd.) was used instead of the catalyst having the structure shown in formula (5), to obtain the modified EPDM rubber A10. The properties of the modified EPDM rubber were analyzed and measured, and the results are shown in Table 1.
[0154]
[0155] In the above formula (6), PCy3 represents tricyclohexylphosphine, and Ph represents a phenyl group.
[0156] Embodiment 11
[0157] The modified EPDM rubber was prepared by the same method as in Example 1, except that the catalyst having the structure shown in formula (7) (commercially available from J&K Technology Co., Ltd.) was used instead of the catalyst having the structure shown in formula (5), to obtain the modified EPDM rubber A11. The properties of the modified EPDM rubber were analyzed and measured, and the results are shown in Table 1.
[0158]
[0159] In the above formula (7), L is PCy3 represents tricyclohexylphosphine.
[0160] Example 12
[0161] The modified EPDM rubber was prepared in the same manner as in Example 1, except that 1.3 g of 4-penten-1-ol (commercially available from J&K Technology Co., Ltd.) was added to obtain the modified EPDM rubber A12. The properties of the modified EPDM rubber were analyzed and measured, and the results are shown in Table 1.
[0162] Example 13
[0163] The modified EPDM rubber was prepared in the same manner as in Example 1, except that 2.2 g of 9-decene-1-ol (commercially available from J&K Technology Co., Ltd.) was added to obtain the modified EPDM rubber A13. The properties of the modified EPDM rubber were analyzed and measured, and the results are shown in Table 1.
[0164] Table 1
[0165]
[0166]
[0167] As can be seen from Table 1, the compound derived from the structure represented by formula (2) can be grafted onto EPDM rubber by adopting the cross-metathesis reaction of olefins, and the grafting rate is relatively high and the reaction is fast.
[0168] Compared with Comparative Example 1 and Comparative Example 2 (unmodified EPDM rubber), respectively, the unsaturation of the modified EPDM rubber obtained in Examples 1 and 9 of the present invention is 0.85 mol / kg and 0.58 mol / kg, which is significantly improved compared with the unmodified EPDM rubber. This is because the side chain double bonds of the EPDM rubber are increased after the olefin cross-metathesis reaction of 2-propylene-1-ol and EPDM rubber in the present invention.
[0169] Comparing Example 1 with Example 2, it can be seen that the grafting rate of the modified EPDM rubber obtained by the method of adding the catalyst in batches is higher. This may be because after the catalyst is added at one time, the catalyst concentration in the system is relatively high, and 2-propylene-1-ol is prone to cross-metathesis side reactions, which reduces the amount of 2-propylene-1-ol participating in the grafting reaction, and ultimately leads to a decrease in the grafting rate. In addition, through Examples 2 to 13, it can be seen that the degree of reaction can be effectively controlled by adjusting the reaction conditions, so that a modified EPDM rubber with a desired grafting rate can be obtained.
[0170] Test Example 1
[0171] The vulcanization properties of the modified EPDM rubbers A1-A13 prepared in Examples 1-13 of the present invention were measured according to the following method.
[0172] 100 parts by weight of the modified EPDM rubber A1 prepared in the embodiment of the present invention were placed on a double-roll rubber mixer, and at a temperature of 35±5°C, 5 parts by weight of active zinc oxide, 1 part by weight of stearic acid, 80 parts by weight of carbon black (N550, Shanghai Cabot Chemical Co., Ltd.), 50 parts by weight of ASTM103# oil (Ningbo Xiejin Chemical Co., Ltd.), 1 part by weight of accelerator TMTD (Shanghai Jingyi Rubber Technology Co., Ltd.), and 1.5 parts by weight of sulfur (Shijiazhuang Ruituo Chemical Technology Co., Ltd.) were added successively, and the mixture was uniformly mixed and kneaded for 21 minutes to obtain a blend. The blend was then vulcanized on a hydraulic flat vulcanizer at a temperature of 160°C and a pressure of 15MPa for 15 minutes to obtain a vulcanized EPDM rubber film.
[0173] The vulcanized EPDM rubber film was tested according to the method in GB / T16584-1996, and the vulcanization speed parameter positive vulcanization time TC90 was recorded. The test results are shown in Table 2.
[0174] The vulcanization properties of modified EPDM rubber A1-A13 were tested according to the above method. The test results are shown in Table 2.
[0175] Comparative test example 1
[0176] The EPDM rubber film was prepared in the same manner as in Test Example 1, except that commercially available EPDM rubber D1 (ESPRENE 305, purchased from Sumitomo, Japan, the content of ethylene structural units in the EPDM rubber is 65% by weight, the content of structural units derived from the third monomer is 7% by weight, the weight average molecular weight is 120,000, and the third monomer is dicyclopentadiene (DCPD)) was used instead of the modified EPDM rubber. The test results are shown in Table 2.
[0177] Comparative test example 2
[0178] The EPDM rubber film was prepared in the same manner as in Test Example 1, except that commercially available EPDM rubber D2 (3280, purchased from Yanshan Petrochemical Company, the content of ethylene structural units in the EPDM rubber is 55% by weight, the content of structural units derived from the third monomer is 5% by weight, the weight average molecular weight is 300,000, and the third monomer is ENB) was used instead of the modified EPDM rubber. The test results are shown in Table 2.
[0179] Table 2
[0180]
[0181] Note: The unit of TC90 is min.
[0182] It can be seen from the data in Table 2 that the vulcanization speed of the modified EPDM rubber provided by the present invention is significantly improved compared with that of the unmodified EPDM rubber. This is mainly due to the introduction of the hydroxyl-containing compound shown in formula (1) into the modified EPDM rubber, and the unsaturation degree is also improved to a certain extent.
[0183] Test Example 2
[0184] The modified EPDM rubbers A1-A13 prepared in Examples 1-13 of the present invention were tested for compatibilization properties according to the following method.
[0185] Taking the combination of EPDM and nitrile rubber as an example, the carbon black masterbatch mixing process was used to preliminarily investigate the volume-increasing effect of EPDM grafted with the compound of the structure shown in formula (2) on the EPDM / nitrile rubber blend. The basic formula (parts by mass) is as follows: nitrile rubber (3945, LANXESS) 70, EPDM (2450, LANXESS) 30, modified EPDM 5, antioxidant (commercially available) MB 1, stearic acid (commercially available) 0.5, paraffin (commercially available) 1, carbon black (brand N 330, product of Shanghai Cabot Chemical Co., Ltd.) 40, polystyrene (commercially available) 10, dioctyl phthalate (commercially available) 12, diisopropyl peroxide (commercially available) 3, trimethylolpropane trimethacrylate 1 (commercially available), trimethylolmethylamine (commercially available) 0.5, triallyl isocyanurate (commercially available) 2.
[0186] The tensile strength was tested according to the method in GB 528-1998. The test results are shown in Table 3.
[0187] According to the method in GB / T16584-1996, the vulcanized EPDM rubber and nitrile rubber film were tested, and the vulcanization speed parameter positive vulcanization time TC90 was recorded. The test results are shown in Table 3.
[0188] Comparative test example 3
[0189] The same method as in Test Example 2 was used to prepare a blend of EPDM and NBR, except that no modified EPDM was added during the test. The test results are shown in Table 3.
[0190] Table 3
[0191] Example A1 D3 A2 A3 A4 A5 A6 A7 A8 A9 A10 A11 A12 A13 Strength 12.9 10.1 11.8 12.5 13 12.2 12.6 13.1 11 11.3 12.4 12.6 12.8 12.9 TC90 10.5 13.5 11.5 10.9 10.4 11.1 10.8 10.3 12.8 12 10.9 10.8 10.7 10.8
[0192] The unit of strength (tear strength) is MPa; the unit of TC90 is min.
[0193] From the data in Table 3, it can be seen that when a small amount of modified graft copolymer is added to the rubber blended with EPDM and nitrile rubber, the vulcanization speed is significantly improved, and the tensile strength of the vulcanized rubber is also significantly improved. This shows that the modified EPDM rubber provided by the present invention does have a good compatibilization effect.
[0194] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A hydroxyl-modified EPDM rubber, characterized in that: The hydroxyl-modified EPDM rubber contains a first structural unit provided by ethylene, a second structural unit provided by propylene and a third structural unit provided by a non-conjugated diene monomer, and at least part of the third structural unit contains a grafted group derived from a compound having a structure represented by formula (1); Wherein, in formula (1), n1 is an integer of 1-20, and m1 is an integer of 2-40; Based on the weight of the modified EPDM rubber, the grafting rate of the modified EPDM rubber is 1.1-13.5 weight %.
2. The modified EPDM rubber according to claim 1, wherein In formula (1), n1 is an integer of 3-10, and m1 is an integer of 6-20.
3. The modified EPDM rubber according to claim 1, wherein The grafted group of the compound of the structure shown in formula (1) is selected from one or more of 4-pentenyl-1-ol, 9-decenyl-1-ol, 2-propenyl-1-ol, 5-hexenyl-1-ol and 7-octenyl-1-ol.
4. The modified EPDM rubber according to claim 1, wherein The non-conjugated diene monomer is selected from one or more of 1,4-hexadiene, dicyclopentadiene and 5-ethylidene-2-norbornene.
5. The modified EPDM rubber according to claim 1, wherein The non-conjugated diene monomer is dicyclopentadiene, and at least part of the third structural unit containing the grafted group has a structure shown in formula (I), In formula (I), n1 is an integer of 1-20, and m1 is an integer of 2-40.
6. The modified EPDM rubber according to claim 1, wherein The unsaturation degree of the modified EPDM rubber is 0.56-1 mol / kg.
7. The modified EPDM rubber according to claim 6, wherein The unsaturation degree of the modified EPDM rubber is 0.56-0.87 mol / kg.
8. The modified EPDM rubber according to claim 1, wherein Based on the weight of the modified EPDM rubber, the content of the first structural unit provided by ethylene is 50-70wt%, and the content of the third structural unit provided by the non-conjugated diene monomer is 4-8wt%.
9. The modified EPDM rubber according to any one of claims 1 to 8, wherein The weight average molecular weight of the modified EPDM rubber is 100,000-400,000.
10. The modified EPDM rubber according to claim 9, wherein: The weight average molecular weight of the modified EPDM rubber is 120,000-300,000.
11. A method for preparing hydroxyl-modified EPDM rubber, characterized in that: The preparation method comprises: contacting ethylene propylene diene rubber with a compound derived from the structure represented by formula (2) in an organic solvent in the presence of a ruthenium carbene catalyst under the conditions of olefin cross-metathesis reaction, wherein the amount of the compound derived from the structure represented by formula (2) is 0.05-40 parts by weight, and the amount of the catalyst is 0.05-10 parts by weight relative to 100 parts by weight of the ethylene propylene diene rubber; the ethylene propylene diene rubber comprises a first structural unit provided by ethylene, a second structural unit provided by propylene, and a third structural unit provided by a non-conjugated diene monomer; In formula (2), n2 is an integer of 1-20, and m2 is an integer of 2-40.
12. The preparation method according to claim 11, wherein n2 is an integer of 3-10, and m2 is an integer of 6-20.
13. The preparation method according to claim 11, wherein: The compound of the structure represented by formula (2) is selected from one or more of 4-penten-1-ol, 9-decen-1-ol, 2-propen-1-ol, 5-hexen-1-ol and 7-octen-1-ol.
14. The preparation method according to claim 11, wherein: The catalyst has a structure shown in formula (3); In formula (3), R1 is hydrogen, C2-C 20 Substituted or unsubstituted alkenyl, C2-C 20 Substituted or unsubstituted alkynyl, C1-C 20 Substituted or unsubstituted alkyl, C6-C 20 Substituted or unsubstituted aryl, C2-C 20 Substituted or unsubstituted carboxylate group, C1-C 20 Substituted or unsubstituted alkoxy, C2-C 20 Substituted or unsubstituted alkenyloxy, C2-C 20 Substituted or unsubstituted alkynyloxy, C6-C 20 Substituted or unsubstituted aryloxy, C1-C 20 Substituted or unsubstituted alkylthio, C1-C 20 Substituted or unsubstituted alkylsulfonyl or C1-C 20 a substituted or unsubstituted alkylsulfinyl group; X1 and X2 are each independently anionic ligands; L1 and L2 are each independently a neutral ligand, and optionally L1 and L2 can be linked to each other to form a di-coordinated neutral ligand.
15. The preparation method according to claim 14, wherein: R1 is C6-C 20 a substituted or unsubstituted aryl group; X1 and X2 are each independently a halogen ion; L1 and L2 are each independently a phosphine, an amine, a thioether, a carbene, or a substituted or unsubstituted imidazolidine.
16. The preparation method according to claim 15, wherein: R1 is phenyl; X1 and X2 are chloride ions; L1 and L2 are each independently a phosphine, a carbene, or a substituted or unsubstituted imidazolidine.
17. The preparation method according to claim 15 or 16, wherein: R1 is phenyl, L1 is substituted or unsubstituted imidazolidine, L2 is phosphine, and X1 and X2 are chloride ions.
18. The preparation method according to claim 17, wherein: The phosphine is a trialkylphosphine.
19. The preparation method according to claim 17, wherein: The imidazolidine is an imidazolidine having a structure shown in formula (4), In formula (4), R2 and R3 are each independently C6-C 20 A substituted or unsubstituted aryl group.
20. The preparation method according to claim 19, wherein: R2 and R3 are each independently R4, R5, R6, R7 and R8 are each independently selected from hydrogen or C1-C5 substituted or unsubstituted alkyl.
21. The preparation method according to claim 20, wherein R2 and R3 are 22. The preparation method according to claim 11, wherein The non-conjugated diene monomer is selected from one or more of 1,4-hexadiene, dicyclopentadiene and 5-ethylidene-2-norbornene.
23. The preparation method according to claim 22, wherein: The non-conjugated diene monomer is dicyclopentadiene.
24. The preparation method according to claim 11, wherein The content of ethylene structural units in the EPDM rubber is 50-70 wt %, and the content of structural units derived from the third monomer is 4-8 wt %.
25. The preparation method according to claim 11 or 24, wherein: The weight average molecular weight of the EPDM rubber is 100,000-400,000.
26. The preparation method according to claim 11, wherein The conditions of the olefin cross-metathesis reaction include: the olefin cross-metathesis reaction is carried out under an inert atmosphere, the reaction temperature is 0-150° C., and the reaction time is 0.1-5 h.
27. The preparation method according to claim 11 or 14, wherein: The catalyst is added to the reaction system in a one-time addition or in multiple additions.
28. The preparation method according to claim 27, wherein The catalyst is added to the reaction system in 2-6 times, and the time interval between two adjacent additions is 3-15 minutes, and the difference in the amount of the catalyst added in any two times accounts for less than 5 weight% of the total amount of the catalyst added.
29. The preparation method according to claim 11, wherein The organic solvent is toluene, xylene, chlorobenzene, C6-C 12 Cycloalkanes, C5-C 10 One or more of straight-chain alkanes, tetrahydrofuran, acetone and 1,4-dioxane.
30. A hydroxy-modified ethylene propylene diene monomer rubber prepared by the preparation method according to any one of claims 11 to 29.