Method for preparing efficient water electrolysis electrode based on waste ternary lithium ion battery electrode mixed powder

By directly preparing the mixed powder materials of the positive and negative electrodes of waste lithium batteries into high-performance oxygen evolution electrodes in electrolytic water, the problems of complex lithium battery recycling processes and environmental pollution are solved, achieving efficient catalytic activity and stability, and reducing recycling costs. cost, opening up a path to the industrialization of new catalysts.

CN115425318BActive Publication Date: 2024-10-29HARBIN INST OF TECH +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202211041661.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-29
Publication Date
2024-10-29
Estimated Expiration
2042-08-29

AI Technical Summary

Technical Problem

The existing lithium battery recycling process is complex, serious environmental pollution and high recycling costs, resulting in low recycling efficiency.

Method used

The mixed powder material of the positive electrode and graphite negative electrode of the waste lithium nickel cobalt manganate lithium ion battery is directly prepared into a high-performance oxygen evolution electrode in electrolytic water. It is mechanically crushed, stirred evenly, mixed with a binder, and dried to form a composite The electrode serves as a high-efficiency oxygen evolution electrode for electrolyzing water to produce hydrogen.

Benefits of technology

It simplifies the recycling process, reduces the acid-base leaching steps, achieves efficient oxygen evolution catalytic activity and stability, maximizes the utilization of waste material resources, reduces production costs, and opens up the industrialization path of new catalysts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115425318B_ABST
    Figure CN115425318B_ABST
Patent Text Reader

Abstract

The method for preparing an efficient water electrolysis electrode based on the electrode mixed powder of waste ternary lithium-ion batteries is aimed at solving a series of problems such as the relatively complex process of recycling lithium batteries, environmental pollution and high recycling costs. The method for preparing an efficient water electrolysis electrode: 1. Mechanically crush the waste ternary lithium-ion batteries, stir and mix the collected positive and negative electrode mixed powder materials with a binder to obtain an electrode slurry; 2. Prepare an electrode collector; 3. Coat the electrode slurry on the electrode collector, and then dry it; 4. Directly use the composite electrode obtained in step 3 as an efficient oxygen evolution electrode for hydrogen production by electrolysis of water. The present invention realizes the rational use of electrode mixed powder in waste batteries, and the positive and negative electrodes complement each other. The positive electrode ternary powder recovered from the waste lithium-ion batteries is used as a catalyst material in the electrode, and the graphite in the negative electrode can be used as a conductive network in the electrode. The combination of the two forms an efficient oxygen evolution electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for directly preparing an oxygen evolution electrode in hydrogen production by electrolyzing water using electrode mixed powder (positive electrode and negative electrode) of waste lithium ion batteries. Background Art

[0002] Lithium-ion batteries are widely used in mobile electronic devices, new energy vehicles, aerospace, national defense and military fields due to their advantages such as high energy density, good cycle performance and low self-discharge rate. With the vigorous development of these industries, the use of lithium-ion batteries has shown an increasing trend year by year. According to the global demand for power batteries in recent years, the sales volume of lithium-ion power batteries is expected to reach 125.97GWh by 2023. However, after hundreds of charge and discharge cycles, the materials and structures of general lithium-ion batteries will undergo irreversible changes, leading to their failure, resulting in their service life usually being 3-5 years. Therefore, with the continued rapid growth in the shipment of lithium-ion batteries, how to efficiently achieve the recycling and reuse of waste lithium-ion battery electrode materials is of great significance.

[0003] As a new type of battery positive electrode material, nickel-cobalt-manganese-oxide ternary positive electrode material has the advantages of low cost, high performance and light pollution, and is considered to be one of the key products for the development of lithium-ion battery positive electrode materials. Waste ternary batteries mainly consist of five parts: metal shell, positive electrode, negative electrode, diaphragm and electrolyte, among which the positive electrode and negative electrode are the main objects of lithium battery recycling. Usually, the positive electrode contains 5% to 20% cobalt, 5% to 10% nickel, 5% to 7% lithium, 15% organic solvent and 7% plastic, which has a high recycling value. The battery-grade graphite in the negative electrode can also be used again as an electrode material for supercapacitors or a conductive additive for battery electrodes after recycling, and it also has a certain recycling value. At present, with the rapid development of the lithium battery recycling industry, when recycling waste lithium-ion battery electrode materials, the battery is first mechanically crushed as a whole by machinery, and then the steel shell in the mixture is separated by a magnetic separator, and the diaphragm is removed by an induced draft fan to obtain a mixed powder of the positive and negative electrodes. Next, the positive and negative electrode powders need to be separated, screened and recycled separately by an airflow separator. Among them, the recovery of the positive electrode of the nickel-cobalt-manganese-oxide lithium ternary positive electrode material can be divided into multiple steps according to the process, including positive electrode pretreatment (alkaline leaching pretreatment, organic solvent pretreatment, pyrolysis pretreatment), valuable metal leaching, valuable metal separation and recovery. The recovery of negative electrode graphite also usually requires calcination acid leaching, mechanical flotation separation and other methods. It can be seen that the current ternary lithium battery recycling and reuse process has the disadvantages of complex recycling process, large amount of strong acid and alkali used in the recycling process, large environmental pollution, low recycling efficiency and high recycling cost. Summary of the invention

[0004] The purpose of the present invention is to solve a series of problems such as the complex process of existing lithium battery recycling, serious environmental pollution and high recycling cost, and to provide a simple and efficient method for directly utilizing waste ternary (nickel cobalt manganese oxide) positive electrode and graphite negative electrode mixed powder material to prepare high-performance oxygen evolution electrode in water electrolysis hydrogen production.

[0005] The method for preparing a high-efficiency water electrolysis electrode based on waste ternary (nickel cobalt manganese oxide) lithium ion battery electrode mixed powder is implemented by the following steps:

[0006] 1. Mechanically crush the waste ternary (nickel cobalt manganese oxide) lithium-ion batteries, collect the positive and negative electrode mixed powder materials of the lithium-ion batteries, and stir and mix the collected positive and negative electrode mixed powder materials with a binder to obtain an electrode slurry;

[0007] 2. Prepare electrode current collector;

[0008] 3. coating the electrode slurry on the electrode current collector, and then drying it to obtain a composite electrode;

[0009] 4. The composite electrode obtained in step 3 is directly used as an efficient oxygen evolution (OER) electrode for hydrogen production by water electrolysis.

[0010] The method of the present invention directly preparing the positive electrode and graphite negative electrode mixed powder material of waste ternary (nickel cobalt manganese oxide) lithium ion battery into an efficient oxygen evolution electrode in water electrolysis hydrogen production has the following advantages compared with the prior art:

[0011] 1. The present invention breaks through the traditional mode of recycling of traditional lithium battery waste, realizes the rational use of electrode mixed powder in waste batteries, and the positive and negative electrodes complement each other. The positive electrode ternary powder recycled from lithium battery waste is used as the catalyst material in the electrode, and the graphite in the negative electrode can be used as the conductive network in the electrode. The combination of the two forms an efficient oxygen evolution electrode.

[0012] 2. In the preparation process of the mixed powder as a high-efficiency electrode, no separation of positive and negative electrode powders or acid-base leaching process is required, which makes the operation process simple, the cycle short, and the process controllable.

[0013] 3. The prepared electrode has high oxygen evolution catalytic activity and good catalytic stability.

[0014] 4. It realizes the resource utilization of waste materials and the reuse of various components in ternary waste batteries to the greatest extent. The catalyst of the present invention can be mass-produced and industrialized, and it also opens up new ideas and ways for the development of new catalysts for water electrolysis. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 11 is a scanning electron microscope (SEM) image of the mixed powder material in step 1 of Example 1, wherein 1 is graphite and 2 is a ternary positive electrode material (lithium nickel cobalt manganese oxide);

[0016] Figure 2 is a scanning electron microscope (SEM) image of the pure carbon cloth after cleaning in step 3 of Example 1;

[0017] Figure 3 is a scanning electron microscope (SEM) image of a composite electrode using carbon cloth as a current collector in step 4 of Example 1;

[0018] Figure 4 is an X-ray energy spectrum (EDS) diagram of the composite electrode using carbon cloth as the current collector in step 4 of Example 1;

[0019] Figure 5 1 is a linear sweep voltammetry (LSV) diagram of the composite electrode with carbon cloth as the current collector and the pure carbon cloth after cleaning in Example 1, wherein 1 is the composite electrode and 2 is the pure carbon cloth;

[0020] Figure 6 The composite electrode with carbon cloth as current collector after cleaning in Example 1 is 10mA cm -2 Test stability diagram under constant current conditions;

[0021] Figure 7 is a scanning electron microscope (SEM) image of the nickel foam after cleaning in Example 2;

[0022] Figure 8 is a scanning electron microscope (SEM) image of the composite electrode with nickel foam as the current collector after cleaning in Example 2;

[0023] Fig. 9 1 represents the composite electrode with nickel foam as the current collector, nickel foam, and the ruthenium dioxide composite electrode with nickel foam as the current collector after cleaning in Example 2, wherein 1 represents the composite electrode with nickel foam as the current collector, 2 represents nickel foam, and 3 represents the ruthenium dioxide composite electrode with nickel foam as the current collector;

[0024] Fig.10 is a Tafei slope diagram of the composite electrode with nickel foam as the current collector, nickel foam, and the ruthenium dioxide composite electrode with nickel foam as the current collector after cleaning in Example 2, wherein 1 represents the composite electrode with nickel foam as the current collector, 2 represents nickel foam, and 3 represents the ruthenium dioxide composite electrode with nickel foam as the current collector;

[0025] Fig.11 This is a test diagram of double-layer capacitance of the composite electrode with nickel foam as the current collector and nickel foam after cleaning in Example 2, wherein 1 represents the composite electrode with nickel foam as the current collector, and 2 represents nickel foam;

[0026] Fig.12 The composite electrode with nickel foam as the current collector after cleaning in Example 2 is 10 mA cm -2 Test stability diagram under constant current conditions. DETAILED DESCRIPTION

[0027] Specific implementation method 1: This implementation method is based on the waste ternary (nickel cobalt manganese oxide) lithium ion battery electrode mixed powder to prepare a high-efficiency water electrolysis electrode according to the following steps:

[0028] 1. Mechanically crush the waste ternary (nickel cobalt manganese oxide) lithium-ion batteries, collect the positive and negative electrode mixed powder materials of the lithium-ion batteries, and stir and mix the collected positive and negative electrode mixed powder materials with a binder to obtain an electrode slurry;

[0029] 2. Prepare electrode current collector;

[0030] 3. coating the electrode slurry on the electrode current collector, and then drying it to obtain a composite electrode;

[0031] 4. The composite electrode obtained in step 3 is directly used as an efficient oxygen evolution (OER) electrode for hydrogen production by water electrolysis.

[0032] The ternary cathode material of the present embodiment is composed of a variety of transition elements, and transition element compounds can be used as effective catalysts in water electrolysis hydrogen production, so the waste ternary cathode material has the basis for obtaining a good water electrolysis hydrogen production catalyst material. But its own shortcomings are also more obvious, that is, poor electrical conductivity, and considering that the ternary negative electrode material (graphite) just has good electrical conductivity. Therefore, the present embodiment breaks through the traditional mode of recycling waste lithium-ion batteries, and directly prepares the electrode mixed powder (positive and negative electrodes) produced during the disassembly of waste lithium-ion batteries as an efficient electrode for oxygen evolution (OER) in water electrolysis hydrogen production. Using this method, on the one hand, a new way for the direct use of lithium battery mixed powder is opened up, and on the other hand, a new and efficient electrode material is provided for water electrolysis hydrogen production from the perspective of turning waste into treasure, which is of great significance for environmental protection and resource reuse.

[0033] Specific embodiment 2: This embodiment is different from specific embodiment 1 in that the positive electrode material described in step 1 is layered lithium manganate, lithium cobaltate, lithium manganate, lithium ferrous phosphate, lithium manganese phosphate, lithium iron silicate, lithium manganese silicate or lithium cobalt silicate.

[0034] Specific implementation method three: This implementation method is different from specific implementation methods one or two in that the negative electrode material described in step one is graphite, hard carbon, soft carbon or graphene.

[0035] Specific implementation method 4: This implementation method is different from any one of specific implementation methods 1 to 3 in that the mass ratio of the positive electrode material to the negative electrode material in the mixed powder material in step 1 is 1:1 to 5:1.

[0036] Specific implementation method five: This implementation method is different from specific implementation methods one to four in that the mixed powder material of waste ternary positive and negative electrodes is sifted in step one.

[0037] In this embodiment, large-sized impurities are removed after screening, and the size is 20 to 40 mesh.

[0038] Specific implementation method 6: This implementation method is different from specific implementation methods 1 to 5 in that the stirring and mixing time in step 1 is 45 to 70 minutes.

[0039] The mixing temperature in this embodiment is between 25°C and 85°C.

[0040] Specific embodiment seven: This embodiment differs from any one of specific embodiments one to six in that the binder described in step one is polyvinylidene fluoride (PVDF), polyacrylic acid (PAA), styrene-butadiene rubber (SBR), polyamide-imide (PAI), polyvinyl alcohol (PVA) or polyethyleneimine (PEI).

[0041] Specific implementation eight: This implementation differs from any one of specific implementations one to seven in that the electrode current collector described in step two is carbon paper, foam copper, foam aluminum, foam iron, foam magnesium, foam titanium, foam steel or foam lead.

[0042] Specific embodiment 9: This embodiment is different from specific embodiments 1 to 8 in that the temperature of the drying process in step 3 is 60-100°C.

[0043] Specific implementation method ten: This implementation method is different from any one of specific implementation methods one to nine in that the coating method in step three is dripping, spraying or scraping.

[0044] Example 1: This example is based on waste ternary (nickel cobalt manganese oxide Li (NiCoMn) O2) lithium ion battery electrode mixed powder (such as Figure 1 The method for preparing an efficient water electrolysis electrode is implemented by the following steps:

[0045] 1. Use a rubber-tipped dropper to weigh 3 mL of N-methylpyrrolidone (NMP) and slowly add it to a beaker, and use a balance to weigh 0.1 g of polyvinylidene fluoride (PVDF) and add it to the beaker. Place the beaker on a magnetic stirrer and stir for 30 minutes to obtain a binder.

[0046] 2. Filter the collected waste ternary Li (NiCoMn) O2 positive electrode and graphite negative electrode mixed powder material into fine powder with a sieve, weigh 0.8g, where the mass ratio of positive electrode material to negative electrode material is 5:1, put it into a beaker and continue stirring for 8h to obtain electrode slurry;

[0047] 3. Cut a piece of carbon cloth current collector, the specific microscopic morphology is shown in Figure 2 As shown;

[0048] 4. Use a syringe to evenly drip the electrode slurry obtained in step 2 onto the carbon cloth obtained in step 3 (7.7 mg cm -2 ), put it into an oven at 80℃ and dry it for 3h to obtain a composite electrode with carbon cloth as the current collector (such as Figure 3 shown);

[0049] 5. The composite electrode obtained in step 4 is placed in 1 mol / L KOH for OER test, wherein Hg / HgO, the composite electrode prepared in step 4, and the carbon rod are used as reference electrode, working electrode, and comparison electrode, respectively;

[0050] 6. The composite electrode and pure carbon cloth (as a comparative electrode sample) obtained in step 5 are ultrasonically cleaned with acetone, and then cleaned with anhydrous ethanol and deionized water in turn, and then dried to obtain the cleaned samples.

[0051] First, cyclic voltammetry (CV) was used to test the voltage between 0 and 1.2 V (vs RHE) until a stable curve was obtained. Linear sweep voltammetry (LSV) curves were measured at 50, 30, 10, and 5 mV s -1 The scanning rate was 10mVs -1 , 15mVs -1 , 20mVs -1 , 25mVs -1 、30mVs -1 、35mVs - 1 40mVs -1 , 45mVs -1 , 50mVs -1 ) and calculate C dl To evaluate the active area of ​​the composite electrode. dl The linear fitting slope of is the double-layer capacitance of the corresponding sample. -2 Long-term stability tests were carried out.

[0052] In the electrochemical test, the composite electrode formed by loading the catalyst material prepared in this example on the carbon cloth and the pure carbon cloth were selected and the electrochemical performance was evaluated at 5 mV s -1Their performance was compared by linear sweep voltammetry (LSV) at a scan rate of 10 mA cm -2 The current density of the sample in this embodiment requires an overpotential (η) of only 320 mV, which is much lower than that of the carbon cloth (η 10 =680mV). The lower the overpotential, the better the catalytic performance of the surface material. This also shows that the catalytic performance of the carbon cloth itself is very poor. Here it mainly plays the role of current collector. The performance of this composite electrode mainly comes from the catalyst formed by the mixed powder ( Figure 5 In this embodiment, the mixed powder electrode can show excellent catalytic performance. In addition to the complementary performance of the positive and negative electrode materials, another important reason is the reasonable distribution of the positive and negative electrode materials in the mixed powder ( Figure 1 As shown in the figure). The graphite material, due to its larger particles and stronger bonding ability, spontaneously agglomerates to form the skeleton of the electrode mixed powder (tens of microns), while the ternary positive electrode material with small particles (~1 micron) can "rivet" on the surface of the graphite particles to form catalytic active points. This microscopic morphology is similar to the microscopic morphology of high-performance composite electrodes prepared by electrodeposition or impregnation methods, which is conducive to the full performance of these two conductive and catalyst materials.

[0053] In addition to its excellent catalytic performance in water electrolysis, the electrode also exhibits good stability. -2 Under the condition of , the prepared catalyst maintained a stable potential in the 680-hour continuous catalytic water decomposition oxygen reaction test, while the stability of electrode OER reported in the literature generally ranges from tens to hundreds of hours, which fully demonstrates that this electrode has excellent long-term activity and stability ( Figure 6 ).

[0054] Embodiment 2: The method for preparing a high-efficiency water electrolysis electrode based on waste ternary lithium-ion battery electrode mixed powder in this embodiment is implemented according to the following steps:

[0055] 1. Filter the collected waste ternary Li (NiCoMn) O2 positive electrode and graphite negative electrode mixed powder material into fine powder with a sieve, weigh 0.7g, where the mass ratio of positive electrode material to negative electrode material is 5:1, put it into a beaker, add appropriate amount of alcohol and stir on a magnetic stirrer for 30 minutes;

[0056] 2. Weigh 0.5g of polytetrafluoroethylene (PDFE) and slowly add it to the beaker and continue stirring for 2h. Finally, put it into an oven at 80℃ and dry it for 8h. After taking it out, add a small amount of alcohol and stir it until it becomes a slurry to obtain electrode slurry.

[0057] 3. Cut a piece of nickel foam current collector. The specific microscopic morphology is shown in Figure 7 ;

[0058] Fourth, the electrode slurry was evenly scraped onto the nickel foam current collector obtained in step 3 with a scraper, and placed in an 80°C oven for 3 hours to obtain a composite electrode with nickel foam as the current collector (such as Figure 8 shown);

[0059] 5. The electrode sample obtained in step 4 is placed in 1 mol / L KOH for OER test, wherein Hg / HgO, the composite electrode prepared in step 4, and the carbon rod are used as the reference electrode, the working electrode, and the comparison electrode, respectively;

[0060] 6. The composite electrode obtained in step 5 and the pure nickel foam (as a comparative electrode sample) were ultrasonically cleaned with acetone, and then cleaned with anhydrous ethanol and deionized water in turn, and dried to obtain the cleaned samples.

[0061] The test conditions of Example 2 are the same as those of Example 1. In the electrochemical test, the composite electrode prepared by the present invention with the catalyst material loaded on nickel foam, pure nickel foam, and a ruthenium dioxide composite electrode with nickel foam as the current collector are selected and the electrochemical performance is tested in 1 M KOH at 5 mV s -1 Their performance was compared by linear sweep voltammetry (LSV) at a scan rate of 10 mA cm -2 The current density of the sample of the present invention requires an overpotential (η) of only 340 mV, which is lower than that of the current collector nickel foam (η 10 =420mV), and can even be used with the precious metal RuO2 (η 10 =340mV) is comparable to ( Fig. 9 In addition to the excellent electrochemical catalytic performance, the Tafel slope of the catalyst electrode material prepared in this example is 76.9 mVdec -1 , better than RuO2 (158mVdec -1 ) and nickel foam (133.4mVdec -1 )( Fig.10 ), the smaller Tafel slope indicates that the sample prepared by the present invention has a faster oxygen evolution reaction rate when used as a catalyst, and the kinetic process is more favorable. Since the electrochemical active area of ​​the catalyst is proportional to the double-layer capacitance, the electrochemical double-layer capacitance (C dl ) was tested to evaluate the electrochemically active surface area (ECSA) of the catalyst ( Fig.11 The double layer capacitance of the sample with nickel foam as the current collector is 4.8 mF, which is better than nickel foam (1.61 mF). In addition, the current density in 1 M KOH is 10 mA cm -2In the case of , the prepared catalyst electrode maintained a stable potential in the 180-hour continuous catalytic water decomposition oxygen reaction test, which was consistent with the result of the composite electrode with carbon cloth as the current collector in Example 1, which once again proved that the electrode catalysis prepared with this mixed powder as raw material has intrinsic long-term activity and stability ( Fig.12 ).

Claims

1. A method for preparing an efficient water electrolysis electrode based on a mixture of waste ternary lithium-ion battery electrode powders, characterized in that The method for preparing a high-efficiency water electrolysis electrode is implemented according to the following steps:

1. Mechanically crush the waste ternary lithium-ion batteries, collect the positive and negative electrode mixed powder materials of the lithium-ion batteries, and stir and mix the collected positive and negative electrode mixed powder materials with a binder to obtain an electrode slurry; 2. Prepare electrode current collector; 3. coating the electrode slurry on the electrode current collector, and then drying it to obtain a composite electrode; Fourth, the composite electrode obtained in step 3 is directly used as an efficient oxygen evolution electrode for hydrogen production by electrolysis of water; The positive electrode material in step 1 is layered lithium manganese oxide, lithium cobalt oxide, lithium manganese oxide, lithium ferrous phosphate, lithium manganese phosphate, lithium iron silicate, lithium manganese silicate or lithium cobalt silicate; the negative electrode material in step 1 is graphite, hard carbon, soft carbon or graphene; In step 1, the mass ratio of the positive electrode material to the negative electrode material in the mixed powder material is 5:

1.

2. The method for preparing a high-efficiency water electrolysis electrode based on waste ternary lithium-ion battery electrode mixed powder according to claim 1, characterized in that In step 1, the waste ternary positive electrode and negative electrode mixed powder material is sieved.

3. The method for preparing a high-efficiency water electrolysis electrode based on waste ternary lithium-ion battery electrode mixed powder according to claim 1, characterized in that The stirring and mixing time in step 1 is 45 to 70 minutes.

4. The method for preparing a high-efficiency water electrolysis electrode based on waste ternary lithium-ion battery electrode mixed powder according to claim 1, characterized in that The binder described in step 1 is polyvinylidene fluoride, polyacrylic acid, styrene-butadiene rubber, polyamide-imide, polyvinyl alcohol or polyethylene imine.

5. The method for preparing a high-efficiency water electrolysis electrode based on waste ternary lithium-ion battery electrode mixed powder according to claim 1, characterized in that The electrode current collector described in step 2 is carbon paper, foam copper, foam aluminum, foam iron, foam magnesium, foam titanium, foam steel or foam lead.

6. The method for preparing a high-efficiency water electrolysis electrode based on waste ternary lithium-ion battery electrode mixed powder according to claim 1, characterized in that The temperature of the drying treatment in step 3 is 60~100°C.

7. The method for preparing a high-efficiency water electrolysis electrode based on waste ternary lithium-ion battery electrode mixed powder according to claim 1, characterized in that The coating method in step 3 is dripping, spraying or scraping.

Citation Information

Patent Citations

  • Method for recycling positive electrode material of waste lithium ion battery as electrocatalyst

    CN113611876A