A preparation method of lithium ion imprinted PVDF membrane based on MOFs
By combining metal organic framework materials with ion imprinting technology and loading them onto PVDF membranes, the problem of reduced selectivity of existing materials when increasing adsorption capacity is solved, and a MOFs-LiⅡPs@PVDF membrane with high selectivity and high adsorption capacity is achieved. , suitable for pollutant removal in complex systems.
Patent Information
- Application Number
- CN202211190325.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-28
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-09-28
AI Technical Summary
While existing ion imprinted materials increase the adsorption capacity, their selectivity will decrease, making it difficult to achieve high adsorption capacity and high selectivity at the same time.
Metal organic framework materials (MOFs) are combined with ion imprinting technology, and the MOFs ion imprinted polymer is loaded onto the polyvinylidene fluoride (PVDF) membrane through in-situ growth method to form a MOFs-LiⅡPs@PVDF membrane. The three-dimensional structure of MOFs is used. The structure increases adsorption sites, and combines polydopamine and silica modification to improve the hydrophilicity and anti-fouling properties of the membrane.
It significantly improves the adsorption capacity and selectivity of ion imprinting, maintains high selectivity, and the preparation process is green and environmentally friendly, reducing the use of dangerous solvents. The adsorption equilibrium time of the membrane is short, making it suitable for practical applications.
Smart Images

Figure CN115445448B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a lithium ion imprinted membrane. Background Art
[0002] Ion imprinting technology evolved from the molecular imprinting process. Its principle is to use ions as templates and polymerized double-bond compounds as functional monomers. The monomers and target ions form prepolymers through covalent and non-covalent interactions, and rigid polymers are prepared by crosslinking or polymerization. After the template ions are eluted, corresponding three-dimensional channels are generated in them for specific identification of target ions. The combination of ion imprinting technology and other polymer preparation technologies not only makes the preparation method of imprinted materials more perfect, but also effectively expands the application range of imprinted materials. Generally, with the increase of adsorption capacity, the selectivity of ion imprinted polymers decreases. This is because the specific adsorption sites formed in the ion imprinting process are not fixed, but increase the channels that can adsorb other ions. Therefore, it is urgent to find a way to fix more imprinted channels, so that the adsorption capacity can be increased while retaining the high selectivity of ion imprinting. Summary of the invention
[0003] The purpose of the present invention is to solve the problem that the existing ion-imprinted molecules cannot have both high adsorption capacity and high selectivity, and to provide a method for preparing a lithium ion-imprinted PVDF membrane based on MOFs.
[0004] In view of the problems existing in the prior art, the present invention creatively proposes a method for removing lithium ions by combining MOFs with ion imprinting technology, and prepares MOFs-LiⅡPs@PVDF membrane to achieve highly selective removal of target pollutants in complex systems.
[0005] The present invention develops a highly selective Li + Imprinted membrane (MOFs-LiⅡPs@PVDF membrane). + The imprinted polymer is the imprinted layer, with 12 crown 4 as the adsorption unit, forming a selective Li+ recognition site and loading the imprinted polymer onto the membrane by the in situ growth method, which is completed in the following steps:
[0006] A method for preparing a lithium ion imprinted PVDF membrane based on MOFs is completed by the following steps:
[0007] 1. Preparation of NH2-UIO-66 zirconium-based organic metal framework:
[0008] First, ZrCl4 and 2-aminoterephthalic acid are dissolved in DMF and stirred at room temperature to obtain a mixed solution; the mixed solution is then poured into a hydrothermal reactor of polytetrafluoroethylene and subjected to a hydrothermal reaction to obtain a suspension; the suspension is then cooled and centrifuged to obtain a solid substance, the solid substance is washed, and finally, a yellow powder is obtained by drying and grinding to obtain the NH2-UIO-66 zirconium-based organic metal framework;
[0009] 2. Preparation of MOFs-LiⅡPs imprinted polymer:
[0010] ①, LiCl, 12-crown ether-4, and anhydrous methanol were mixed, and then prepolymerized in a constant temperature heated magnetic stirrer, and then NH2-UIO-66 zirconium-based organic metal framework was added and shaken, and then α-methylacrylic acid and azobisisobutylcyanide were added, and then shaken under nitrogen atmosphere, 70℃-80℃ water bath and condensation reflux conditions to obtain a solid substance;
[0011] ② Grind and sieve the generated solid material, rinse the resulting powder repeatedly with anhydrous ethanol and deionized water to remove excess organic matter, and then use hydrochloric acid to extract the Li on the imprinted polymer. + , and finally rinsed repeatedly with deionized water, filtered, and the obtained solid was vacuum dried at 343 K, ground, and sieved to obtain MOFs-LiⅡPs imprinted polymer;
[0012] 3. Preparation of SP-PDA@PVDF membrane:
[0013] Dissolve polydopamine in NaAC buffer, add sodium periodate solution, stir evenly to obtain SP-PDA solution; coat the SP-PDA solution on PVDF membrane, and dry to obtain SP-PDA@PVDF membrane;
[0014] 4. Introducing SiO2 nano-intermediate layer:
[0015] ①, mix ethyl orthosilicate, deionized water, anhydrous ethanol and ammonia water to obtain a mixed solution;
[0016] ②, immerse the SP-PDA@PVDF membrane into the mixed solution, take it out and then wash it, to obtain the PVDF membrane after the SiO2 nano-intermediate layer is introduced;
[0017] 5. Preparation of MOFs-LiⅡPs@PVDF membrane:
[0018] The MOFs-LiⅡPs imprinted polymer is dissolved in anhydrous ethanol to obtain a MOFs-LiⅡPs imprinted polymer solution; the PVDF membrane after the introduction of the SiO2 nano-intermediate layer is immersed in the MOFs-LiⅡPs imprinted polymer solution, and then stirred for reaction, taken out and dried to obtain a MOFs-LiⅡPs@PVDF membrane, which is a lithium ion imprinted PVDF membrane based on MOFs.
[0019] Principle of the present invention:
[0020] Metal organic framework is an organic-inorganic hybrid porous material that is self-assembled through coordination bonds with metal ions as nodes and organic ligands as connectors. These materials not only have the activity of metal ions, but also have the flexibility of organic ligands, the selectivity of functional groups and the specific spatial structure formed by coordination, which provides a good basic condition for its application in the fields of adsorption and catalysis. In the present invention, the three-dimensional spatial structure of MOFs material is creatively utilized, combined with ion imprinting, and a large number of ion imprinting holes are loaded in the cavity of MOFs, thereby solving the above problems. The present invention adopts an in-situ growth method to load MOFs ion imprinting polymer onto a polyvinylidene fluoride (PVDF) membrane modified with silicon dioxide particles with polydopamine (DA) as the interface adhesion layer to prepare a MOFs-LiⅡPs@PVDF membrane. The present invention introduces MOFs materials into the field of ion imprinting, and utilizes the interaction between template molecules and metal ions and organic ligands to prepare a MOFs ion imprinting membrane with specific recognition ability. The three-dimensional structure of the MOFs material in the present invention increases the number of ion-imprinted specific adsorption sites, achieving highly selective removal of target pollutants in complex systems. The advantages of the present invention are high adsorption capacity and high selectivity for lithium ions, green and environmentally friendly preparation process, and reduced use of hazardous organic solvents such as DMF and acetone. The MOFs-LiⅡPs@PVDF membrane has excellent anti-pollution performance and hydrophilicity, and a short adsorption equilibrium time, which is more suitable for practical applications.
[0021] Beneficial effects of the present invention:
[0022] 1. At present, one of the disadvantages of the combination of ion imprinting technology with other materials or technologies is that its adsorption capacity is low compared with previous adsorption materials. The present invention utilizes the rich three-dimensional structure of MOFs materials to significantly improve the adsorption capacity of ion imprinting while retaining the excellent selectivity of ion imprinting technology:
[0023] 2. NH2-UIO-66 zirconium-based organic metal framework can show high selective permeability to water molecules during the desalination process, has good hydrophilicity, acid resistance and stability, and has higher durability and reusability in complex systems;
[0024] 3. With polydopamine as the interface adhesion layer, the SP-PDA@PVDF membrane modified with silica has good hydrophilicity and anti-fouling properties. The MOFs-LiⅡPs@PVDF membrane formed by loading the MOFs ion-imprinted polymer onto the modified PVDF membrane has good hydrophilicity and anti-fouling properties. After more than 10 adsorption and desorption processes, its performance only decreased by 5.6%.
[0025] 4. Compared with the previous patent, the MOFs-based lithium ion imprinted PVDF membrane prepared by the present invention has an 11.6% higher loading rate for MOFs ion imprinted polymer, which correspondingly leads to a significant increase in the adsorption amount; SiO2 modification increases the specific surface area and anti-pollution performance of the membrane, shortens the adsorption equilibrium time, and improves the anti-pollution performance. After 10 consecutive elutions, its performance only decreases by 5.6%, which is 6.1% higher than the prior art. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The graph of the adsorption amount of lithium ions by the MOFs-based lithium ion imprinted PVDF membrane prepared by changing the usage amount of NH2-UIO-66 zirconium-based organic metal framework in Examples 1 to 5;
[0027] Figure 2 The graph of the adsorption amount of lithium ions by the lithium ion imprinted PVDF membrane based on MOFs prepared by changing the stirring reaction time in step 5 in Example 1 and Example 6 to Example 9;
[0028] Figure 3 The relationship between the number of regenerations and the adsorption amount in the simulated water sample of Example 1, where A is K + , B is Na + , C is Li + , D is Ca 2+ , E is Mg 2+ . DETAILED DESCRIPTION
[0029] The present invention is further described in detail below. The specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0030] Specific implementation method 1: In this implementation method, a method for preparing a lithium ion imprinted PVDF membrane based on MOFs is completed by the following steps:
[0031] 1. Preparation of NH2-UIO-66 zirconium-based organic metal framework:
[0032] First, ZrCl4 and 2-aminoterephthalic acid are dissolved in DMF and stirred at room temperature to obtain a mixed solution; the mixed solution is then poured into a hydrothermal reactor of polytetrafluoroethylene and subjected to a hydrothermal reaction to obtain a suspension; the suspension is then cooled and centrifuged to obtain a solid substance, the solid substance is washed, and finally, a yellow powder is obtained by drying and grinding to obtain the NH2-UIO-66 zirconium-based organic metal framework;
[0033] 2. Preparation of MOFs-LiⅡPs imprinted polymer:
[0034] ①, LiCl, 12-crown ether-4, and anhydrous methanol were mixed, and then prepolymerized in a constant temperature heated magnetic stirrer, and then NH2-UIO-66 zirconium-based organic metal framework was added and shaken, and then α-methylacrylic acid and azobisisobutylcyanide were added, and then shaken under nitrogen atmosphere, 70℃-80℃ water bath and condensation reflux conditions to obtain a solid substance;
[0035] ② Grind and sieve the generated solid material, rinse the resulting powder repeatedly with anhydrous ethanol and deionized water to remove excess organic matter, and then use hydrochloric acid to extract the Li on the imprinted polymer. + , and finally rinsed repeatedly with deionized water, filtered, and the obtained solid was vacuum dried at 343 K, ground, and sieved to obtain MOFs-LiⅡPs imprinted polymer;
[0036] 3. Preparation of SP-PDA@PVDF membrane:
[0037] Dissolve polydopamine in NaAC buffer, add sodium periodate solution, stir evenly to obtain SP-PDA solution; coat the SP-PDA solution on PVDF membrane, and dry to obtain SP-PDA@PVDF membrane;
[0038] 4. Introducing SiO2 nano-intermediate layer:
[0039] ①, mix ethyl orthosilicate, deionized water, anhydrous ethanol and ammonia water to obtain a mixed solution;
[0040] ②, immerse the SP-PDA@PVDF membrane into the mixed solution, take it out and then wash it, to obtain the PVDF membrane after the SiO2 nano-intermediate layer is introduced;
[0041] 5. Preparation of MOFs-LiⅡPs@PVDF membrane:
[0042] The MOFs-LiⅡPs imprinted polymer is dissolved in anhydrous ethanol to obtain a MOFs-LiⅡPs imprinted polymer solution; the PVDF membrane after the introduction of the SiO2 nano-intermediate layer is immersed in the MOFs-LiⅡPs imprinted polymer solution, and then stirred for reaction, taken out and dried to obtain a MOFs-LiⅡPs@PVDF membrane, which is a lithium ion imprinted PVDF membrane based on MOFs.
[0043] Specific implementation method 2: The difference between this implementation method and specific implementation method 1 is that in step 1, 1 mmol of ZrCl4 and 1 mmol of 2-aminoterephthalic acid are first dissolved in 50 mL of DMF, stirred at room temperature for 0.5 h, and a mixed solution is obtained; then a hydrothermal reaction is carried out at 120°C for 24 h, and a suspension is obtained by reaction; then, after cooling and centrifugation, a solid substance is obtained, and the solid substance is washed with anhydrous ethanol and deionized water respectively, and finally, after drying and grinding, a yellow powder is obtained to obtain NH2-UIO-66 zirconium-based organic metal framework. The other steps are the same as those in specific implementation method 1.
[0044] Specific implementation method three: This implementation method is different from specific implementation method one or two in that: the volume ratio of the mass of LiCl described in step 2① to anhydrous methanol is 0.3g:100mL; the volume ratio of 12-crown ether-4 described in step 2① to anhydrous methanol is 0.3:100; the volume ratio of the mass of NH2-UIO-66 zirconium-based organic metal framework described in step 2① to anhydrous methanol is (3g~6g):100mL; the volume ratio of α-methyl acrylic acid described in step 2① to anhydrous methanol is 0.3:100; the volume ratio of azobisisobutyl cyanide described in step 2① to anhydrous methanol is 0.03g:100mL. The other steps are the same as specific implementation method one or two.
[0045] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that: in step 2①, LiCl, 12-crown ether-4, and anhydrous methanol are mixed, and then placed in a constant temperature heating magnetic stirrer for prepolymerization for 10min to 13min, the temperature of the constant temperature heating magnetic stirrer is 70℃ to 80℃, and the stirring speed is 80r / min to 100r / min; in step 2①, NH2-UIO-66 zirconium-based organic metal framework is added and shaken for 1min to 2min, and then α-methylacrylic acid and azobisisobutyl cyanide are added, and then shaken for 22h to 24h under nitrogen atmosphere, 70℃ to 80℃ water bath and condensation reflux to obtain a solid substance; the concentration of hydrochloric acid described in step 2② is 1mol / L; the solid obtained in step 1② is vacuum dried at a temperature of 343K for 10h to 12h. The other steps are the same as specific embodiments 1 to 3.
[0046] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that: the mass ratio of polydopamine described in step 3 to the volume ratio of NaAC buffer is: (0.2g-0.25g): (245mL-255mL); the concentration of NaAC buffer described in step 3 is 50mmol-60mmol, and the pH value is 5.0; the concentration of sodium periodate solution described in step 3 is 20mmol-25mmol; the volume ratio of NaAC buffer described in step 3 to sodium periodate solution is (245-255): (5.0-15). The other steps are the same as specific embodiments 1 to 4.
[0047] Specific embodiment 6: This embodiment differs from specific embodiments 1 to 5 in that: the thickness of the PVDF membrane described in step 3 is 15 μm to 22 μm; the thickness of the SP-PDA membrane on the SP-PDA@PVDF membrane described in step 3 is 10 nm to 20 nm. The other steps are the same as specific embodiments 1 to 5.
[0048] Specific implementation method 7: This implementation method is different from specific implementation methods 1 to 6 in that the volume ratio of ethyl orthosilicate, deionized water, anhydrous ethanol and ammonia water in step 4① is 1:5:30:0.5; the mass fraction of ammonia water in step 4① is 28%. The other steps are the same as those in specific implementation methods 1 to 6.
[0049] Specific embodiment eight: This embodiment differs from specific embodiments one to seven in that: in step four ②, the SP-PDA@PVDF membrane is immersed in the mixed solution for 6h to 8h, and after being taken out, it is first washed with anhydrous ethanol 1 to 3 times, and then washed with deionized water 1 to 3 times to obtain a PVDF membrane with a SiO2 nano-intermediate layer introduced. The other steps are the same as those of specific embodiments one to seven.
[0050] Specific embodiment 9: This embodiment differs from specific embodiments 1 to 8 in that the volume ratio of the mass of the MOFs-LiⅡPs imprinted polymer described in step 5 to anhydrous ethanol is (3.5 g to 5.0 g): (245 mL to 250 mL). The other steps are the same as those of specific embodiments 1 to 8.
[0051] Specific embodiment 10: This embodiment differs from specific embodiments 1 to 9 in that the stirring reaction time in step 5 is 5 to 7 hours. The other steps are the same as those in specific embodiments 1 to 9.
[0052] The following examples are used to verify the beneficial effects of the present invention:
[0053] Example 1: A method for preparing a lithium ion imprinted PVDF membrane based on MOFs, which is specifically completed by the following steps:
[0054] 1. Preparation of NH2-UIO-66 zirconium-based organic metal framework:
[0055] First, 1 mmol of ZrCl4 and 1 mmol of 2-aminoterephthalic acid were dissolved in 50 mL of DMF and stirred at room temperature for 0.5 h to obtain a mixed solution; the mixed solution was then poured into a polytetrafluoroethylene hydrothermal reactor and subjected to a hydrothermal reaction at 120 ° C for 24 h. The suspension obtained by the reaction was cooled and centrifuged to obtain a solid substance, which was washed three times with anhydrous ethanol and deionized water respectively. Finally, after drying and grinding, a yellow powder was obtained, which was the NH2-UIO-66 zirconium-based organic metal framework;
[0056] 2. Preparation of MOFs-LiⅡPs imprinted polymer:
[0057] ①, 0.3g LiCl, 0.3mL 12-crown ether-4, 100mL anhydrous methanol were mixed, and then placed in a constant temperature heating magnetic stirrer for prepolymerization, and then 3.0g NH2-UIO-66 zirconium-based organic metal framework was added and shaken for 2min, and then 0.3mL α-methylacrylic acid and 0.03g azobisisobutylcyanide were added, nitrogen was introduced for 10min, and then shaken for 22h under nitrogen atmosphere, 75°C water bath and condensation reflux conditions to obtain a solid substance;
[0058] ② Grind and sieve the generated solid material, rinse the resulting powder repeatedly with anhydrous ethanol and deionized water to remove excess organic matter, and then use 1 mol / L hydrochloric acid to extract the Li on the imprinted polymer. + , and finally rinsed repeatedly with deionized water, filtered, and the obtained solid was vacuum dried at 343 K for 10 h, ground, and sieved to obtain MOFs-LiⅡPs imprinted polymer;
[0059] 3. Preparation of SP-PDA@PVDF membrane:
[0060] 0.2 g of polydopamine was dissolved in 240 mL of NaAC buffer, and then 10 mL of sodium periodate solution was added and stirred evenly to obtain an SP-PDA solution; the SP-PDA solution was coated on a PVDF membrane and then dried to obtain an SP-PDA@PVDF membrane;
[0061] The concentration of the NaAC buffer described in step 3 is 50 mmol and the pH value is 5.0;
[0062] The concentration of the sodium periodate solution described in step 3 is 20 mmol;
[0063] The thickness of the SP-PDA film on the SP-PDA@PVDF film described in step 3 is 20 nm;
[0064] 4. Introducing SiO2 nano-intermediate layer:
[0065] ①, Mix 1.0 mL of ethyl orthosilicate, 5.0 mL of deionized water, 30 mL of anhydrous ethanol and 0.5 mL of aqueous ammonia to obtain a mixed solution;
[0066] The mass fraction of the ammonia water described in step 4① is 28%;
[0067] ②, immerse the SP-PDA@PVDF membrane in the mixed solution for 6 hours, take it out and wash it twice with anhydrous ethanol, and then wash it twice with deionized water to obtain the PVDF membrane with the SiO2 nano-intermediate layer introduced;
[0068] 5. Preparation of MOFs-LiⅡPs@PVDF membrane:
[0069] The MOFs-LiⅡPs imprinted polymer was dissolved in anhydrous ethanol to obtain a MOFs-LiⅡPs imprinted polymer solution; the PVDF membrane after the SiO2 nano-intermediate layer was introduced was immersed in the MOFs-LiⅡPs imprinted polymer solution, and then stirred for reaction for 6 hours, and then taken out and dried to obtain a MOFs-LiⅡPs@PVDF membrane, which is a lithium ion imprinted PVDF membrane based on MOFs;
[0070] The mass ratio of the MOFs-LiⅡPs imprinted polymer described in step 5 to the volume ratio of anhydrous ethanol is 3.5g:250mL.
[0071] Example 2: The difference between this example and Example 1 is that in step 2①, 3.5 g of NH2-UIO-66 zirconium-based organic metal framework is added and shaken for 2 minutes. The other steps and parameters are the same as those in Example 1.
[0072] Example 3: The difference between this example and Example 1 is that 4.0 g of NH2-UIO-66 zirconium-based organic metal framework is added in step 2① and shaken for 2 minutes. The other steps and parameters are the same as those in Example 1.
[0073] Example 4: The difference between this example and Example 1 is that in step 2①, 4.5 g of NH2-UIO-66 zirconium-based organic metal framework is added and shaken for 2 minutes. The other steps and parameters are the same as those in Example 1.
[0074] Example 5: The difference between this example and Example 1 is that in step 2①, 5.0 g of NH2-UIO-66 zirconium-based organic metal framework is added and shaken for 2 minutes. The other steps and parameters are the same as those in Example 1.
[0075] Example 6: The difference between this example and Example 1 is that in step 5, the PVDF membrane after the SiO2 nano-intermediate layer is immersed in the MOFs-LiⅡPs imprinted polymer solution, and then stirred for 5 hours. The other steps and parameters are the same as those in Example 1.
[0076] Example 7: The difference between this example and Example 1 is that in step 5, the PVDF membrane after the SiO2 nano-intermediate layer is immersed in the MOFs-LiⅡPs imprinted polymer solution, and then stirred for 5.5 hours. The other steps and parameters are the same as those in Example 1.
[0077] Example 8: The difference between this example and Example 1 is that in step 5, the PVDF membrane after the SiO2 nano-intermediate layer is immersed in the MOFs-LiⅡPs imprinted polymer solution, and then stirred for 6.5 hours. The other steps and parameters are the same as those in Example 1.
[0078] Example 9: The difference between this example and Example 1 is that in step 5, the PVDF membrane after the SiO2 nano-intermediate layer is immersed in the MOFs-LiⅡPs imprinted polymer solution, and then stirred for 7 hours. The other steps and parameters are the same as those in Example 1.
[0079] Figure 1 The graph of the adsorption amount of lithium ions by the MOFs-based lithium ion imprinted PVDF membrane prepared by changing the usage amount of NH2-UIO-66 zirconium-based organic metal framework in Examples 1 to 5;
[0080] from Figure 1 It can be seen that the optimal usage of NH2-UIO-66 zirconium-based organic metal framework is 5.5g. In this experiment, an ion imprinted membrane with a size of 0.5cm×0.5cm was used to test the adsorption capacity. When the membrane size is sufficient, the adsorption rate can reach 99.9%.
[0081] Figure 2 The graph of the adsorption amount of lithium ions by the lithium ion imprinted PVDF membrane based on MOFs prepared by changing the stirring reaction time in step 5 in Example 1 and Example 6 to Example 9;
[0082] from Figure 2 It can be seen that the optimal stirring time in step five is 6h.
[0083] Figure 3 The relationship between the number of regenerations and the adsorption amount in the simulated water sample of Example 1, where A is K + , B is Na + , C is Li + , D is Ca 2+ , E is Mg 2+ ;
[0084] from Figure 3 It can be seen that the adsorption capacity of lithium ions on the imprinted membrane is significantly higher than that on Na + , K + Mg 2+ , Ca 2+ Common competing ions such as Li + / Na + , Li + / K + , Li + / Mg 2+ , Li + / Ca 2+ The selectivity coefficients are 6.72, 7.4, 8.2 and 8.7 respectively. It can be seen that while ensuring high adsorption capacity, the selectivity is also significantly improved.
Claims
1. A method for preparing a lithium ion imprinted PVDF membrane based on MOFs, characterized in that The MOFs-based lithium ion imprinted PVDF membrane prepared by the preparation method has good performance on Li + The adsorption rate can reach 99.9%, and it has good hydrophilicity and anti-pollution performance. After more than 10 adsorption and desorption processes, its performance only decreased by 5.6%. + / Na + , Li + / K + , Li + / Mg 2+ , Li + / Ca 2+ The selectivity coefficients are 6.72, 7.4, 8.2 and 8.7 respectively. The three-dimensional structure of MOFs material increases the number of ion imprinting specific adsorption sites, achieving highly selective removal of target pollutants in complex systems. The preparation method is specifically completed in the following steps:
1. Preparation of NH2-UIO-66 zirconium-based organic metal framework: First, 1 mmol of ZrCl4 and 1 mmol of 2-aminoterephthalic acid were dissolved in 50 mL of DMF and stirred at room temperature for 0.5 h to obtain a mixed solution; the mixed solution was then poured into a polytetrafluoroethylene hydrothermal reactor and subjected to a hydrothermal reaction at 120 ° C for 24 h. The suspension obtained by the reaction was cooled and centrifuged to obtain a solid substance, which was washed three times with anhydrous ethanol and deionized water respectively. Finally, after drying and grinding, a yellow powder was obtained, which was the NH2-UIO-66 zirconium-based organic metal framework; 2. Preparation of MOFs-LiⅡPs imprinted polymer: ①, 0.3g LiCl, 0.3mL 12-crown ether-4, 100mL anhydrous methanol were mixed, and then placed in a constant temperature heating magnetic stirrer for prepolymerization, and then 3.0g NH2-UIO-66 zirconium-based organic metal framework was added and shaken for 2min, and then 0.3mL α-methylacrylic acid and 0.03g azobisisobutylcyanide were added, nitrogen was introduced for 10min, and then shaken for 22h under nitrogen atmosphere, 75°C water bath and condensation reflux conditions to obtain a solid substance; ② Grind and sieve the generated solid material, rinse the resulting powder repeatedly with anhydrous ethanol and deionized water to remove excess organic matter, and then use 1 mol / L hydrochloric acid to extract the Li on the imprinted polymer. + , and finally rinsed repeatedly with deionized water, filtered, and the obtained solid was vacuum dried at 343 K for 10 h, ground, and sieved to obtain MOFs-LiⅡPs imprinted polymer; 3. Preparation of SP-PDA@PVDF membrane: 0.2 g of polydopamine was dissolved in 240 mL of NaAC buffer, and then 10 mL of sodium periodate solution was added and stirred evenly to obtain an SP-PDA solution; the SP-PDA solution was coated on a PVDF membrane and then dried to obtain an SP-PDA@PVDF membrane; The concentration of the NaAC buffer described in step 3 is 50 mmol and the pH value is 5.0; The concentration of the sodium periodate solution described in step 3 is 20 mmol; The thickness of the SP-PDA film on the SP-PDA@PVDF film described in step 3 is 20 nm; 4. Introducing SiO2 nano-intermediate layer: ①, Mix 1.0 mL of ethyl orthosilicate, 5.0 mL of deionized water, 30 mL of anhydrous ethanol and 0.5 mL of aqueous ammonia to obtain a mixed solution; The mass fraction of the ammonia water described in step 4① is 28%; ②, immerse the SP-PDA@PVDF membrane in the mixed solution for 6 hours, take it out and wash it twice with anhydrous ethanol, and then wash it twice with deionized water to obtain the PVDF membrane with the SiO2 nano-intermediate layer introduced; 5. Preparation of MOFs-LiⅡPs@PVDF membrane: The MOFs-LiⅡPs imprinted polymer was dissolved in anhydrous ethanol to obtain a MOFs-LiⅡPs imprinted polymer solution; the PVDF membrane after the introduction of the SiO2 nano-intermediate layer was immersed in the MOFs-LiⅡPs imprinted polymer solution, and then stirred for reaction for 6 hours, and then taken out and dried to obtain a MOFs-LiⅡPs@PVDF membrane, which is a lithium ion imprinted PVDF membrane based on MOFs; the mass ratio of the MOFs-LiⅡPs imprinted polymer described in step five to the volume ratio of anhydrous ethanol is 3.5g:250mL.
Citation Information
Patent Citations
Lithium-ion imprinted polyvinylidene fluoride (PVDF) membrane as well as preparation method and application of lithium-ion imprinted PVDF membrane
CN107344095A
Catalytic membrane reactor on basis of nuclear track membranes and method for preparing catalytic membrane reactor
CN108144559A
Preparation method and application of temperature response type bionic lithium ion imprinted composite membrane
CN113351180A
Preparation method and application of magnetic lithium ion imprinted nano composite membrane with high adsorption capacity and high selectivity
CN113509913A
Preparation method of lithium ion imprinted composite nanofiber membrane based on MOFs (Metal-Organic Frameworks)
CN114797799A