A method for gray-blue multi-color coloring of automobile exterior parts

Through oil removal and wax removal, electrochemical polishing and other processes combined with AC electrolytic coloring, the oxide film layer structure is changed, and the gray-blue uneven and durable problems of automotive exterior parts are solved, and the high temperature resistance of gray-blue automotive exterior parts is achieved. , corrosion resistance and aging resistance, suitable for practical applications.

CN115449879BActive Publication Date: 2024-11-19JIANGSU HEXING AUTOMOTIVE TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211081775.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-06
Publication Date
2024-11-19
Estimated Expiration
2042-09-06

AI Technical Summary

Technical Problem

The prior art is difficult to effectively realize gray-blue color in automotive exterior parts, and the gray-blue color produced is prone to unevenness, cannot pass the strict test conditions, and cannot be directly applied to automotive exterior parts.

Method used

Using oil removal, wax removal, electrochemical polishing, DC anodization, DC electrochemical pore amplification, AC electrolytic coloring, electrophoresis, and curing, electrolytic coloring is performed by solvents of stannous sulfate, magnesium sulfate, and zinc sulfate to change the structure of the oxide film layer , forming a stable gray-blue color.

Benefits of technology

It realizes gray-blue coloring of automotive exterior parts, with high temperature resistance, corrosion resistance and aging resistance, uniform and stable color, and is not easy to fall off or discolor, and is suitable for practical applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003833584400000051
    Figure BDA0003833584400000051
  • Figure BDA0003833584400000061
    Figure BDA0003833584400000061
Patent Text Reader

Abstract

The present invention relates to a method for gray-blue multi-coloring of automobile exterior parts, and belongs to the technical field of automobile parts. The present invention discloses a method for gray-blue multi-coloring of automobile exterior parts, the method comprising sequentially performing oil and wax removal, electrochemical polishing, DC anodizing, DC electrochemical hole expansion, AC electrolytic coloring, electrophoresis, and curing treatment on aluminum parts; during the electrolytic coloring, the AC voltage is 15-18V, the time is 180-200s, and the temperature is 18-20°C; the solvent in the electrolytic coloring process includes stannous sulfate, magnesium sulfate, nickel sulfate, and zinc sulfate in a mass ratio of (2-4): 1:1:1. The present invention also discloses a gray-blue automobile exterior part, the automobile exterior part is blue before electrophoresis, and the automobile exterior part is gray-blue after electrophoresis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of automobile parts and relates to a method for gray-blue multi-color coloring of automobile exterior decoration parts. Background Art

[0002] The colors of automobile exterior parts are mostly common black, silver, champagne, etc.; however, gray-blue is relatively rare, because it is difficult to achieve gray-blue in automobile exterior parts with ordinary processes. At present, gray-blue aluminum parts are obtained by spray painting, film pasting, and dyeing, but the gray exterior parts obtained by these methods are easy to fall off or discolor, and the actual application performance cannot be guaranteed. At present, studies have shown that gray-blue can be obtained by electroplating or electrodeposition, but the gray-blue obtained by the above methods is prone to unevenness; and because it cannot pass a series of rigorous test conditions such as sealing quality, wear resistance test, corrosion resistance test, weather resistance test and light aging test, it still cannot be directly applied to automobile exterior parts. Summary of the invention

[0003] The purpose of the present invention is to address the above-mentioned problems existing in the prior art and to propose a method for gray-blue multi-color coloring of automobile exterior trims, so that the automobile exterior trims can obtain gray-blue color and have high temperature resistance, corrosion resistance and aging resistance.

[0004] The purpose of the present invention can be achieved by the following technical solutions:

[0005] A method for gray-blue multi-color coloring of automobile exterior parts, the method comprising sequentially performing degreasing and dewaxing, electrochemical polishing, direct current anodizing, direct current electrochemical hole expansion, alternating current electrolytic coloring, electrophoresis, and curing treatment on aluminum parts;

[0006] During the electrolytic coloring, the AC voltage is 15-18V, the time is 180-200s, and the temperature is 18-20°C;

[0007] The solvent in the electrolytic coloring process comprises stannous sulfate, magnesium sulfate, nickel sulfate and zinc sulfate in a mass ratio of (2-4):1:1:1.

[0008] Preferably, the degreasing and dewaxing treatment uses a weak alkaline agent with a concentration of 60-70 g / L and a pH of 9.0-10.0, a treatment temperature of 60-80° C., an ultrasonic treatment time of 100-300 s, and an ultrasonic single group current of 3-5A.

[0009] Preferably, the electrochemical polishing is carried out in a tri-acid system of sulfuric acid / phosphoric acid / chromic acid, with a DC voltage of 30 to 33 V, a time of 800 to 1500 s, and a temperature of 50 to 60°C.

[0010] Compared with the double acid system of sulfuric acid / phosphoric acid, the triple acid system of sulfuric acid / phosphoric acid / chromic acid of the present invention does not add nitric acid that is easy to pollute the environment, but uses more environmentally friendly chromic acid, which can reduce pollution to the environment while better polishing; in addition, the triple acid system is more suitable for the preparation process of the present invention and is more conducive to obtaining the materials required by the present invention.

[0011] Preferably, the anodization adopts a DC constant voltage of 12 to 16 V, a temperature of 15 to 20° C., a dilute sulfuric acid concentration of 160 to 180 g / L, and a time of 1500 to 1700 s.

[0012] Further preferably, the anode oxygen uses a rectifier with a voltage range of 0 to 26V and a current range of 0 to 4000A.

[0013] Preferably, the electrochemical pore expansion time is 120 to 180 seconds, the DC voltage is 2.5 to 3.5 V, and the sulfuric acid concentration is 20 to 50 g / L.

[0014] Preferably, the solid content of the solvent in the electrolytic coloring is 20±2 g / L.

[0015] Preferably, the electrophoresis is carried out in an acrylic resin agent with a conductivity of 600 to 750 us / cm and a pH of 8.3±0.2.

[0016] More preferably, the DC voltage of electrophoresis is 100-130 V, the time is 110-130 s, and the temperature is 20±1° C.

[0017] Preferably, the curing process is carried out at 160-200° C. for 30-60 minutes.

[0018] The invention also discloses a gray-blue automobile exterior decoration part. The automobile exterior decoration part is blue before electrophoresis and gray-blue after electrophoresis.

[0019] The aluminum part of the present invention is blue before electrophoresis, with a glossiness of 60 to 80 GU, a blue scale, a color value, and a brightness color Lab of (9.15 to 16.15).(-0.02 to -0.23).(-8.28 to -12.55), and a uniform and stable color; after electrophoresis, the color is gray-blue, with a glossiness of 85 to 135 GU, and a color, Lab of (9.15 to 16.15).(-0.4 to 0.11).(-1.15 to -4.15), and a uniform and stable color.

[0020] The gray-blue color prepared by the present invention is cold gray, but it is blue before electrophoresis; this is because the blue product of electrolytic coloring changes the structure of the oxide film layer after the electrophoresis is energized, and then appears gray-blue.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1. The present invention adopts the methods of oil and wax removal, electrochemical polishing, DC anodizing, DC electrochemical hole expansion, AC electrolytic coloring, electrophoresis and curing to make the automobile exterior parts have gray-blue color and have high temperature resistance, corrosion resistance and aging resistance.

[0023] 2. The aluminum part of the present invention is blue before electrophoresis treatment and gray-blue after electrophoresis. The blue color produced by electrolytic coloring is energized again through electrophoresis to change the structure of the oxide film layer, so that the product color appears gray-blue.

[0024] 3. The method for gray-blue multi-color coloring of automobile exterior parts of the present invention is simple and controllable, has a stable process, is easy to promote and mass-produce, and has broad application prospects.

[0025] 4. The gray-blue automobile exterior trim produced by the present invention has bright color, uniform color, and is not easy to fall off or change color. DETAILED DESCRIPTION

[0026] The following are specific embodiments of the present invention, which further describe the technical solutions of the present invention, but the present invention is not limited to these embodiments.

[0027] Example 1

[0028] The aluminum parts were degreased and dewaxed using a weak alkaline agent with a concentration of 60 g / L and pH 9.1±0.1, a treatment temperature of 70°C, an ultrasonic treatment time of 280 s, and an ultrasonic single group current of 4 A; then they were placed in a three-acid system of sulfuric acid / phosphoric acid / chromic acid for electrochemical polishing with a DC voltage of 32 V, a time of 1000 s, and a temperature of 52°C; after the electrochemical polishing was completed, an oxidation treatment was performed, and the sulfuric acid concentration in the oxidation tank was adjusted to 170 g / L, the temperature to 17°C, the power-on time to 1600 s, a DC constant voltage was used, and the power-on voltage was 15 V; then a DC pore expansion treatment was performed with a sulfuric acid concentration of 40 g / L, a time of 130 s, and a voltage of 3 V; then the aluminum parts were placed in an electrolytic coloring tank containing stannous sulfate in a mass ratio of 3:1:1:1, the coloring temperature was 19°C, the time was 190 s, and the AC voltage was 17 V; the aluminum parts obtained at this time were blue. Transfer to electrophoresis treatment, electrophoresis is carried out in an acrylic resin agent with a conductivity of 610us / cm and a pH of 8.2; the DC voltage is 127V, the time is 120s, and the temperature is 20±1°C; then it is cured at 180°C for 30min; a gray-blue aluminum part is obtained. The obtained aluminum part is tested according to the conventional test method in the art, and the performance results are shown in Table 1.

[0029] Example 2

[0030] Compared with Example 1, the difference is that the electrochemical pore expansion voltage is 3.5V.

[0031] Example 3

[0032] Compared with Example 1, the difference is that the electrochemical pore expansion voltage is 2.5V.

[0033] Example 4

[0034] Compared with Example 1, the difference is that the electrolytic coloring temperature is 18°C.

[0035] Example 5

[0036] Compared with Example 1, the difference is that the electrolytic coloring temperature is 20°C.

[0037] Example 6

[0038] Compared with Example 1, the difference is that the electrolytic coloring time is 200s.

[0039] Example 7

[0040] Compared with Example 1, the difference is that the electrolytic coloring time is 180s.

[0041] Example 8

[0042] Compared with Example 1, the difference is that the electrophoresis voltage is 130V.

[0043] Example 9

[0044] Compared with Example 1, the difference is that the electrophoresis time is 130 s.

[0045] Example 10

[0046] Compared with Example 1, the difference is that the electrophoresis time is 100 s.

[0047] Embodiment 11

[0048] Compared with Example 1, the difference is that the electrophoresis voltage is 133V.

[0049] Example 12

[0050] Compared with Example 1, the difference is that the electrochemical pore expansion voltage is 2V.

[0051] Example 13

[0052] Compared with Example 1, the difference is that the electrochemical pore expansion voltage is 4V.

[0053] Embodiment 14

[0054] Compared with Example 1, the difference is that the electrochemical polishing is carried out under a dual acid system of sulfuric acid / phosphoric acid.

[0055] Comparative Example 1

[0056] Compared with Example 1, the difference is that during electrolytic coloring, a direct current of 16V is first applied for 3min; and then an alternating current of 16V is applied for 2min.

[0057] Comparative Example 2

[0058] Compared with Example 1, the difference is that the electrolytic coloring temperature is 17°C.

[0059] Comparative Example 3

[0060] Compared with Example 1, the difference is that the electrolytic coloring temperature is 21°C.

[0061] Comparative Example 4

[0062] Compared with Example 1, the difference is that the electrolytic coloring time is 170s.

[0063] Comparative Example 5

[0064] Compared with Example 1, the difference is that the electrolytic coloring time is 210s.

[0065] Comparative Example 6

[0066] Compared with Example 1, the difference is that the electrolytic coloring voltage is 14V.

[0067] Comparative Example 7

[0068] Compared with Example 1, the difference is that the electrolytic coloring voltage is 19V.

[0069] Comparative Example 8

[0070] Compared with Example 1, the difference is that the solvent in the electrolytic cell is only stannous sulfate.

[0071] Comparative Example 9

[0072] Compared with Example 1, the difference is that the solvent in the electrolytic cell is only stannous sulfate and magnesium sulfate in a mass ratio of 3:1.

[0073] Table 1. Performance test table of automobile exterior parts

[0074]

[0075]

[0076] The automobile exterior parts prepared by the present invention are blue in color before electrophoresis and gray-blue in color after electrophoresis, have good glossiness, uniform and stable color, and Lab is (9.15-16.15).(-0.4-0.11).(-1.15--4.15).

[0077] According to the above table, the method for gray-blue multi-color coloring of automobile exterior parts as in Examples 1 to 9 of the present invention can make automobile exterior parts have a relatively uniform and stable color, a gray-blue appearance, and maintain good corrosion resistance, high temperature resistance, and aging resistance. Examples 10 to 13 have performance degradation, uneven color, and a certain color difference due to the parameters in the preparation process exceeding the scope of the present invention. In Comparative Example 1, due to the use of direct current-alternating current for electrolytic coloring, the color is significantly different, and the color is close to yellow; in Comparative Examples 2 to 7, the electrolytic coloring parameters exceed the scope of this application, resulting in a slight change in color, and affecting the corrosion resistance, high temperature resistance, and aging resistance; Comparative Examples 8 and 9 have large color differences due to the change of the solvent components in the electrolytic cell, and the color is close to ordinary brown; and the performance is slightly reduced.

[0078] In summary, the automobile exterior accessories prepared by the method for gray-blue multi-color coloring of automobile exterior accessories of the present invention are gray-blue in color with uniform luster, and have good corrosion resistance, high temperature resistance, and aging resistance, and can meet practical application requirements.

[0079] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways, but they will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.

Claims

1. A method for gray-blue multi-color coloring of automobile exterior parts, characterized in that: The method includes degreasing and waxing, electrochemical polishing, DC anodizing, DC electrochemical pore expansion, AC electrolytic coloring, electrophoresis, and curing; During the electrolytic coloring, the AC voltage is 15-18V, the time is 180-200s, and the temperature is 18-20°C; The electrolytic coloring agent in the electrolytic coloring process includes stannous sulfate, magnesium sulfate, nickel sulfate, and zinc sulfate in a mass ratio of (2-4): 1:1:1; The electrochemical pore expansion time is 120-180s, the voltage is 2.5-3.5V, and the sulfuric acid concentration is 20-50g / L; The electrophoresis is carried out in an acrylic resin agent with a conductivity of 600-750 us / cm and a pH of 8.3±0.2; The DC voltage of electrophoresis is 100~130V, the time is 110~130s, and the temperature is 20±1℃.

2. The method according to claim 1, characterized in that: The solid content of the electrolytic colorant in electrolytic coloring is 20±2g / L.

3. The method according to claim 1, characterized in that The oil and wax removal uses a weak alkaline agent with a concentration of 60-70 g / L and a pH of 9.0-10.0, a treatment temperature of 60-80° C., an ultrasonic treatment time of 100-300 s, and an ultrasonic single group current of 3-5A.

4. The method according to claim 1, characterized in that: The electrochemical polishing is carried out in a tri-acid system of sulfuric acid / phosphoric acid / chromic acid, with a DC voltage of 30-33V, a time of 800-1500s, and a temperature of 50-60°C.

5. The method according to claim 1, characterized in that The anodic oxidation adopts a direct current constant voltage, the voltage is 12-16V; the temperature is 15-20°C, the concentration of dilute sulfuric acid is 160-180g / L, and the time is 1500-1700s.

6. The method according to claim 1, characterized in that The curing process is kept at 160~200℃ for 30~60min.

7. A gray-blue automobile exterior trim, characterized in that: Prepared according to the method according to any one of claims 1 to 6, wherein the automobile exterior trim is blue before electrophoresis and gray-blue after electrophoresis.

Citation Information

Patent Citations

  • Method for improving light aging resistance of colorful colored exterior trimming part of automobile

    CN113622005A

  • Method for improving adhesiveness of electrophoresis layer of colorful colored exterior trimming part of automobile

    CN113668030A