A method for identifying the coking properties of coking coal using colloid microstructure

By measuring the optical anisotropic tissue formation rate of colloidal microstructure of coking coal and calculating the P value, the problem that the existing technology cannot accurately judge the coking performance of coking coal is solved, and a simple, reliable and low-cost Methods, guide coal quality evaluation and coal mixing, suitable for coal and coking enterprises.

CN115508167BActive Publication Date: 2024-11-08SINOSTEEL ANSHAN RES INST OF THERMO ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211354593.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-01
Publication Date
2024-11-08
Estimated Expiration
2042-11-01

AI Technical Summary

Technical Problem

The existing technology is difficult to fully reflect the coking performance of coking coal, and conventional indicators cannot accurately judge the difference in coal quality, which affects the quality of coke and blast furnace reactivity.

Method used

By using the colloidal microstructure, the optical anisotropic tissue formation rate is measured, the P value is calculated, and the coking performance of coking coal is judged, providing a simple, reliable and low-cost method.

Benefits of technology

It has achieved rapid and accurate judgment of the coking performance of coking coal, guided coal quality evaluation and coal mixing, and is suitable for coal and coking enterprises and has extensive promotion value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115508167B_ABST
    Figure CN115508167B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for identifying the coking performance of coking coal by using the microstructure of colloid, preparing test samples; carrying out single-coal coking test and obtaining colloid test; measuring the optical organizational structure of coke and colloid, setting OA to characterize the optical anisotropic structure content, using OA=fine grain mosaic content+medium grain mosaic content+coarse grain mosaic content+incomplete fiber content+complete fiber content+flaky content, calculating the optical anisotropic structure contents OA1 and OA2 of coke and colloid; using #imgabs0# to calculate the P value; when P>70%, the coking performance of coking coal is a positive contribution, and when P≤70%, the coking performance of coking coal is a negative contribution. The present invention does not need to detect various indicators of coking coal, and can judge the coking performance of coking coal in a relatively short time, providing a basis for coal quality evaluation and guiding coal blending.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of coal coking chemical industry, and in particular relates to a method for identifying the coking performance of coking coal by utilizing the microstructure of colloid. Background Art

[0002] With the large-scale development of blast furnaces, the role of coke as a supporting skeleton is becoming more and more important, so coking coal needs to have good coking properties. The international coal classification standard shows that the Oya expansion, Ge Jin index and coke slag characteristics are internationally recognized coal coking indicators; the domestic coal coke field believes that the adhesion index G value, the gelatinous layer thickness Y value and the Oya expansion b value are the main indicators of coking, among which the adhesion index G value, the gelatinous layer thickness Y value and the Oya expansion b value are quantitative indicators, and the Ge Jin index and coke slag characteristics are qualitative indicators. Since coal is an organic biological rock with a very complex composition and structure and extremely heterogeneous, the above indicators can only represent the process characteristics of coking coal in one aspect, and are far from reflecting the differences in coal rock components and vitrinite quality brought about by coal-forming plants and coal-forming environments.

[0003] Under the coal rock analyzer, it was observed that the coal contained different microstructures, which were mainly divided into vitrinite, exinite, and inertinite. Among them, vitrinite and exinite can soften and melt to form mesophase spheres during coal distillation and coking. The mesophase spheres are melted and solidified to form optical anisotropic structures with different shapes and structures. The inert components in coal basically do not soften and melt during the pyrolysis process, and maintain their original shape and structure, forming inert component charcoal and flake-like structures in coke. The optical structure of coke has a direct impact on the performance of coke and its reactivity in the blast furnace.

[0004] With the continuous development of coal resources, it is found that many coals have large differences in coking performance when the conventional indicators and coal rock reflectivity are similar. It is necessary to seek new indicators or methods to more reasonably judge the coal quality. The formation and development of the intermediate phase during coal pyrolysis plays an important role in the characteristics of coking coal. Summary of the invention

[0005] The purpose of the present invention is to provide a method for identifying the coking performance of coking coal by using the microstructure of colloid. The method is simple and reliable, low in cost, good in timeliness and suitable for coal and coking enterprises.

[0006] To achieve the above object, the present invention adopts the following technical solutions:

[0007] A method for identifying the coking performance of coking coal by using the microstructure of colloids comprises the following steps:

[0008] 1) preparing a coking coal sample and obtaining a colloid sample of the same type of coal as the coking coal sample;

[0009] 2) Carry out a coking test on the single coking coal sample prepared in step 1) in accordance with YB / T4526 "Technical Specifications for Small Coke Ovens for Coking Tests", and prepare slices and determine the coke optical structure content in accordance with "Determination Method of Coke Optical Structure";

[0010] 3) placing the colloid sample obtained in step 1) in a crucible, placing asbestos and an iron block on the surface of the crucible in sequence, and tightly covering the crucible;

[0011] 4) Place the crucible in a muffle furnace and heat it. The temperature control program of the muffle furnace is: from room temperature to 450°C-600°C at 3-10°C / min, and the constant temperature time is ≤5h;

[0012] 5) Take out the crucible, cool it to below 30°C, take out the colloidal sample, slice the colloidal sample according to the "Determination Method of Optical Structure of Coke" and determine the volume percentage of each optical structure;

[0013] 6) Setting the optical anisotropy content OA, and setting OA = fine-grain mosaic content + medium-grain mosaic content + coarse-grain mosaic content + incomplete fiber content + complete fiber content + flake content;

[0014] 7) Calculate the optical anisotropy content OA of the coking coal sample using the formula in step 6) 1 and optical anisotropy of colloid samples and tissue content OA 2 ;

[0015] 8) Set the P value to represent the formation rate of the optical anisotropic structure of the colloid, and let

[0016] Calculate the P value;

[0017] 9) Identify the coking properties of coking coal. When P>70%, the coking performance of coking coal has a positive contribution. When P≤70%, the coking performance of coking coal has a negative contribution.

[0018] In the above step 1), the particle size of the coking coal sample is controlled to be less than 3 mm in size accounting for 78% to 90%, and the particle size of the obtained colloid sample is less than 1 mm.

[0019] In the above step 1), the weight of the coking coal sample is 20-300 kg, and the weight of the colloid sample is 20-300 g.

[0020] The mass of the iron block in the above step 3) is 100-130g.

[0021] The method is applicable to single types of coal including gas coal, gas fat coal, fat coal, 1 / 3 coking coal, coking coal, lean coal, poor lean coal. The technical principle of the present invention is:

[0022] After long-term research, it was found that the performance of the colloid is a key factor affecting the coking property of coking coal. The present invention is a coking property identification method for coking coal developed based on the coking theory. Due to the different properties and quantities of colloids in different bituminous coals, the strength of the bonding is different; due to the difference in the petrographic composition, the rate at which the bituminous coal forms anisotropic structures during pyrolysis is different, and finally cokes of different qualities and different optical structures are formed. Therefore, the higher the formation rate of the optical anisotropic structure of the colloid, the better the performance of the colloid, which is conducive to the production of high-quality coke.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1) The present invention does not need to test various indicators of coking coal, and can judge the coking performance of coking coal in a relatively short time, which can provide a reliable basis for coal quality evaluation and guidance of coal blending;

[0025] 2) The method of the present invention is simple and reliable, low in cost, and has good timeliness, is suitable for coal and coking enterprises, and has wide promotion value. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0027] The invention discloses a method for identifying the coking performance of coking coal by utilizing the microstructure of colloid, and the coking performance of coking coal is identified by obtaining the index of the formation rate of the optical anisotropy structure of the colloid.

[0028] The coking coal applicable to the present invention includes gas coal, gas fat coal, fat coal, 1 / 3 coking coal, coking coal, lean coal and poor lean coal.

[0029] The formation of optical structure is closely related to the macromolecular structure of coal. For coking coal, when the aromatic ring in the coal molecular structure is larger and the degree of branching is smaller, the coking performance is better. For coal with the above structural characteristics, the colloid is easy to form an optical anisotropic structure during pyrolysis. The formation rate of optical anisotropic structure is large, that is, the rate of optical anisotropy formation is fast, which means that the system activity is appropriate, the viscosity is large, the colloid performance is good, and it is conducive to the production of good quality coke.

[0030] In order to illustrate the technical solution of the present invention, a detailed description is given below in conjunction with specific embodiments.

[0031] Taking the coking coal used by a certain enterprise as an example, the coal quality analysis results of coking coal A to coking coal D are shown in Table 1;

[0032] Table 1 Coal quality analysis of single coal

[0033]

[0034] Embodiment 1:

[0035] 1) Prepare 40 kg of coking coal A sample and obtain 25 g of a colloid sample of the same type as coking coal A;

[0036] 2) Carry out a 40kg coking test on coking coal A in accordance with YB / T4526 "Technical Specifications for Small Coke Ovens for Coking Tests", and prepare slices and measure the coke optical structure content in accordance with "Determination Method of Coke Optical Structure";

[0037] 3) Place the colloidal sample obtained above in a crucible, place asbestos and an iron block on its surface in sequence, the mass of the iron block is 110 g, and cover the crucible tightly;

[0038] 4) Place the crucible in a muffle furnace and heat it. The temperature control program of the muffle furnace is: increase the temperature from room temperature to 500°C at 3°C / min and keep the temperature constant for 0.5h;

[0039] 5) Take out the crucible and cool it to below 30°C, then take out the colloid, slice the colloid according to the "Determination Method of Optical Structure of Coke" and determine the volume percentage of each optical structure;

[0040] 6) Calculate the OA of coke A according to the formula OA = fine particle mosaic content + medium particle mosaic content + coarse particle mosaic content + incomplete fiber content + complete fiber content + flake content 1 The value was 68.76% and the OA of colloid A 2 The value is 36.16%; the optical structure content of coke A and colloid A is shown in Table 2;

[0041] 7) According to the formula The calculated P value was 52.6%;

[0042] 8) Identify the coking performance of coking coal. The P value of coking coal A is 52.6%, which is a type of coal with negative contribution to coking performance.

[0043] Table 2 Optical structure content of Example 1

[0044]

[0045] Embodiment 2:

[0046] 1) Prepare 200 kg of coking coal B sample and obtain 100 g of colloid sample of the same type as coking coal B;

[0047] 2) Carry out a 200kg coking test on coking coal B in accordance with YB / T4526 "Technical Specifications for Small Coke Ovens for Coking Tests", and prepare slices and determine the coke optical structure content in accordance with "Determination Method of Coke Optical Structure";

[0048] 3) Place the colloidal sample obtained above in a crucible, place asbestos and an iron block on its surface in sequence, the mass of the iron block is 110 g, and cover the crucible tightly;

[0049] 4) Place the crucible in a muffle furnace and heat it. The temperature control program of the muffle furnace is: increase the temperature from room temperature to 550°C at 5°C / min and keep the temperature constant for 0.5h.

[0050] 5) Take out the crucible, cool it to below 30°C, take out the colloid, slice the colloid according to the "Determination Method of Optical Structure of Coke" and measure the volume percentage of each optical structure;

[0051] 6) Calculate the OA of coke B and colloid B according to the formula OA = fine particle mosaic content + medium particle mosaic content + coarse particle mosaic content + incomplete fiber content + complete fiber content + flake content 1 The value is 84.27% and OA 2 The value is 77.48%; the optical structure content of coke B and colloid B is shown in Table 3;

[0052] 7) According to the formula The calculated P value was 91.9%;

[0053] 8) Identify the coking performance of coking coal. The P value of coking coal B is 91.9%, which is a type of coal that contributes positively to coking performance.

[0054] Table 3 Optical structure content of Example 2

[0055]

[0056] Embodiment 3:

[0057] 1) Prepare 40 kg of coking coal C sample and obtain 150 g of colloid sample of the same type as coking coal C;

[0058] 2) Carry out a 40kg coking test on coking coal C in accordance with YB / T4526 "Technical Specifications for Small Coke Ovens for Coking Tests", and prepare slices and measure the coke optical structure content in accordance with "Determination Method of Coke Optical Structure";

[0059] 3) Place the colloidal sample obtained above in a crucible, place asbestos and an iron block on its surface in sequence, the mass of the iron block is 110 g, and cover the crucible tightly;

[0060] 4) Place the crucible in a muffle furnace and heat it. The temperature control program of the muffle furnace is: increase the temperature from room temperature to 600°C at 8°C / min and keep the temperature constant for 0.5h;

[0061] 5) Take out the crucible, cool it to below 30°C, take out the colloid, slice the colloid according to the "Determination Method of Optical Structure of Coke" and measure the volume percentage of each optical structure;

[0062] 6) Calculate the OA of coke C and colloid C according to the formula OA = fine particle mosaic content + medium particle mosaic content + coarse particle mosaic content + incomplete fiber content + complete fiber content + flake content 1 The value is 82.05% and OA 2 The value is 53.61%; the optical structure content of coke C and colloid C is shown in Table 4;

[0063] 7) According to the formula The calculated P value is 65.3%,

[0064] 8) Identify the coking performance of coking coal. The P value of coking coal C is 65.3%, which is a type of coal with negative contribution to coking performance.

[0065] Table 4 Optical structure content of Example 3

[0066]

[0067] Embodiment 4:

[0068] 1) Prepare 20 kg of coking coal D sample and obtain 25 g of colloid sample of the same type as coking coal D;

[0069] 2) Carry out a 20kg coking test on coking coal D in accordance with YB / T4526 "Technical Specifications for Small Coke Ovens for Coking Tests", and prepare slices and determine the coke optical structure content in accordance with "Determination Method of Coke Optical Structure";

[0070] 3) Place the colloidal sample obtained above in a crucible, place asbestos and an iron block on its surface in sequence, the mass of the iron block is 110 g, and cover the crucible tightly;

[0071] 4) Place the crucible in a muffle furnace and heat it. The temperature control program of the muffle furnace is: increase the temperature from room temperature to 500°C at 4°C / min and keep the temperature constant for 1 hour.

[0072] 5) Take out the crucible, cool it to below 30°C, take out the colloid, slice the colloid according to the "Determination Method of Optical Structure of Coke" and measure the volume percentage of each optical structure;

[0073] 6) Calculate the OA of coke D and colloid D according to the formula OA = fine particle mosaic content + medium particle mosaic content + coarse particle mosaic content + incomplete fiber content + complete fiber content + flake content 1 The value is 66.07% and OA 2 The value is 65.56%; the optical structure content of coke D and colloid D is shown in Table 5;

[0074] 7) According to the formula The calculated P value was 99.2%;

[0075] 8) Identify the coking performance of coking coal. The P value of coking coal D is 99.3%, which is a type of coal that contributes positively to coking performance.

[0076] Table 5 Optical structure content of Example 4

[0077]

[0078] The present invention can accurately, simply and quickly judge the coking performance of coking coal. The colloid is the essential factor affecting the coking characteristics of coal. Therefore, research and development from the source can accurately judge the coking performance of coking coal, thereby guiding coal quality evaluation and coal blending.

[0079] The above description is only a preferred specific implementation mode of the present invention. The present invention is not limited to the above described embodiments. Simple modifications and combinations within the values ​​and ranges described in the present invention shall be regarded as the disclosure of the present invention and belong to the protection scope of the present invention.

Claims

1. A method for identifying the coking performance of coking coal using the microstructure of colloid, characterized in that: The steps include: 1) preparing a coking coal sample and obtaining a colloid sample of the same type of coal as the coking coal sample; 2) Carry out a coking test on the single coking coal sample prepared in step 1) in accordance with YB / T4526 "Technical Specifications for Small Coke Ovens for Coking Tests", and prepare slices and determine the coke optical structure content in accordance with "Determination Method of Coke Optical Structure"; 3) placing the colloid sample obtained in step 1) in a crucible, placing asbestos and an iron block on the surface of the crucible in sequence, and tightly covering the crucible; 4) Place the crucible in a muffle furnace and heat it. The temperature control program of the muffle furnace is: from room temperature to 450°C-600°C at 3-10°C / min, and the constant temperature time is ≤5h; 5) Take out the crucible, cool it to below 30°C, take out the colloidal sample, slice the colloidal sample according to the "Determination Method of Optical Structure of Coke" and determine the volume percentage of each optical structure; 6) Setting the optical anisotropy content OA, and setting OA = fine-grain mosaic content + medium-grain mosaic content + coarse-grain mosaic content + incomplete fiber content + complete fiber content + flake content; 7) using the formula in step 6), respectively calculating the optical anisotropy content OA1 of the coking coal sample and the optical anisotropy content OA2 of the colloid sample; 8) Set the P value to represent the formation rate of the optical anisotropic structure of the colloid, and let Calculate the P value; 9) Identify the coking properties of coking coal. When P>70%, the coking performance of coking coal is a positive contribution. When P≤70%, the coking performance of coking coal is a negative contribution. The coking coal applicable to the method includes gas coal, gas fat coal, fat coal, 1 / 3 coking coal, coking coal, lean coal and poor lean coal.

2. The method for identifying the coking performance of coking coal by using the microstructure of colloid according to claim 1, characterized in that: In the above step 1), the particle size of the coking coal sample is controlled to be less than 3 mm in size accounting for 78% to 90%, and the particle size of the obtained colloid sample is less than 1 mm.

3. The method for identifying the coking performance of coking coal by using the microstructure of colloid according to claim 1, characterized in that: The weight of the coking coal sample in the above step 1) is 20-300 kg, and the weight of the colloid sample in the above step 1) is 20-300 g.

4. The method for identifying the coking performance of coking coal by using the microstructure of colloid according to claim 1, characterized in that: The mass of the iron block in the above step 3) is 100-130g.