Metal graphene composite material and preparation method, application and electronic component thereof

By applying pulse current to the metal substrate for surface heat treatment, the problem of difficulty in preparing high-strength dense metal graphene composite materials is solved in the traditional heating process, and efficient preparation and environmentally friendly production are achieved, and suitable for microstructure products.

CN115519840BActive Publication Date: 2024-11-08BEIJING GRAPHENE TECH RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211156816.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-22
Publication Date
2024-11-08
Estimated Expiration
2042-09-22

AI Technical Summary

Technical Problem

Traditional heating processes cannot meet the requirements of high strength and density of metal graphene composites, especially when preparing products with microstructures, it is inefficient and difficult to obtain high strength and dense metal graphene composites.

Method used

The surface heat treatment is carried out by applying pulse current to the metal substrate, and the microstructure of the metal substrate is adjusted through Joule thermal effect and electroplastic effect, the nucleation and growth rate of graphene are improved, and metal graphene composite materials are prepared by laminated sintering.

Benefits of technology

It improves the preparation efficiency of metal graphene composite materials, obtains high-strength and dense materials, which are suitable for the industrial production of microstructured products, and reduces heat loss and environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115519840B_ABST
    Figure CN115519840B_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of composite materials, and in particular to a metal graphene material and its preparation method, application and electronic components. It is used to solve the problem that the traditional heating process in the related technology cannot meet the high strength and high density requirements of the metal graphene composite material. A method for preparing a metal graphene composite material, comprising: S1), growing graphene on the surface of a metal substrate to prepare a metal graphene composite layer; S2), stacking at least two metal graphene composite layers along their thickness direction so that the metal substrates on the two adjacent metal graphene composite layers are facing each other, and preparing a metal graphene composite material by hot pressing and sintering; wherein, in S1), the metal substrate is subjected to surface heat treatment by applying a pulse current to the metal substrate. The present application is used to prepare a metal graphene composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of composite materials, and in particular to a metal graphene material and a preparation method, application and electronic components thereof. Background Art

[0002] Metal materials have been widely studied and applied because of their high specific strength, high specific modulus, high corrosion resistance, excellent electrothermal properties and excellent processing properties. However, with the rapid development of science and technology, especially in some special environments, metal materials can no longer meet the application requirements. Graphene has attracted widespread attention due to its high thermal conductivity, excellent mechanical properties, low thermal expansion coefficient and good chemical stability. By combining metal and graphene, in addition to maintaining the excellent properties of graphene, the synergistic effect of the two can also be utilized, so that the final metal-graphene composite material exhibits superior performance than the individual graphene and metal materials.

[0003] In the related art, when graphene is deposited on a metal surface to obtain a metal graphene composite material, the heat treatment process used is a heating process of chemical fuel combustion. Although this heating process can meet the mass production of large-size products, it is not suitable for the preparation of products with microstructures. For example, when heat treating a product with a microstructure, the heating time of the above-mentioned traditional heat treatment process is long and the efficiency is low, and the strength and density of the obtained metal graphene composite material cannot be effectively guaranteed.

[0004] Especially for metal-graphene composite materials with multiple metal-graphene composite layers, to obtain metal-graphene composite materials with higher strength and density, it is necessary to extend the hot pressing sintering time and improve the hot pressing sintering reaction conditions. On the one hand, the preparation time of the entire metal-graphene composite material is extended, further reducing the efficiency. On the other hand, the improvement methods are limited, and it is difficult to obtain metal-graphene composite materials with higher strength and density, which is not conducive to improving the preparation efficiency and quality of products with microstructures. Summary of the invention

[0005] Based on this, the present application provides a metal graphene material and its preparation method, application and electronic components to solve the problem that the traditional heating process in the related art cannot meet the high strength and high density requirements of the metal graphene composite material.

[0006] In a first aspect of the present application, a method for preparing a metal graphene composite material is provided, comprising:

[0007] S1), growing graphene on the surface of the metal substrate to prepare a metal-graphene composite layer;

[0008] S2), stacking at least two metal-graphene composite layers along their thickness direction so that the metal substrates on two adjacent metal-graphene composite layers face back to back, and preparing the metal-graphene composite material by hot pressing and sintering;

[0009] Wherein, in S1), the surface heat treatment of the metal substrate is performed by applying a pulse current to the metal substrate.

[0010] In a possible implementation of the first aspect, in S1), the surface heat treatment includes a multi-stage heat treatment process, and the heating temperature of the metal substrate in different heat treatment stages is the same, and the pulse current density applied to the metal substrate in different stages is controlled to have the same value range; the heating temperature of the metal substrate in different heat treatment stages is different, and the power supply frequency and duty cycle of the pulse current applied to the metal substrate in different stages are controlled to have the same value range.

[0011] In a possible implementation manner of the first aspect, in S1), applying a pulse current to the metal substrate to perform surface heat treatment on the metal substrate comprises:

[0012] In the pretreatment stage of the metal substrate, a first pulse current is applied to the metal substrate to heat the metal substrate to a first temperature for a first preset time;

[0013] During the graphene deposition stage, a second pulse current is applied to the metal substrate to heat the metal substrate to a second temperature for a second preset time;

[0014] In the graphene growth stage, applying a third pulse current to the metal substrate to heat the metal substrate to the first temperature for a third preset time;

[0015] Among them, the first temperature is the recovery and recrystallization temperature of the metal substrate, and the second temperature is the phase change temperature of the metal substrate; the value range of the pulse current density of the first pulse current and the third pulse current is the same, and the value range of the pulse current density of the first pulse current and the second pulse current is different; the value range of the power supply frequency and duty cycle of the first pulse current, the second pulse current and the third pulse current are all the same.

[0016] In a possible implementation manner of the first aspect, a lower limit value of a value range of the pulse current density of the first pulse current is greater than an upper limit value of a value range of the pulse current density of the second pulse current.

[0017] In a possible implementation manner of the first aspect, the metal substrate is copper;

[0018] The pulse current density of the first pulse current and the third pulse current is in the range of 2000A / mm2 ~2500A / mm 2 ;

[0019] The pulse current density of the second pulse current is in the range of 1200A / mm 2 ~1800A / mm 2 .

[0020] In a possible implementation manner of the first aspect, the metal substrate is nickel;

[0021] The pulse current density of the first pulse current and the third pulse current is in the range of 1000A / mm 2 ~1500A / mm 2 ;

[0022] The pulse current density of the second pulse current is in the range of 500A / mm 2 ~800A / mm 2 .

[0023] In a possible implementation manner of the first aspect, the power supply frequencies of the first pulse current, the second pulse current, and the third pulse current are all in the range of 100 Hz to 1000 Hz.

[0024] In a possible implementation manner of the first aspect, the duty ratios of the first pulse current, the second pulse current, and the third pulse current are all in the range of 0.1 to 0.5.

[0025] In a possible implementation manner of the first aspect, the first preset time and the third preset time have the same value range, both of which are 5 minutes to 10 minutes;

[0026] The value range of the second preset time is different from the value range of the first preset time, and the upper limit value of the value range of the second preset time is less than or equal to the lower limit value of the value range of the first preset time.

[0027] In a possible implementation of the first aspect, the second preset time ranges from 1 min to 5 min.

[0028] In a possible implementation manner of the first aspect, during the pretreatment stage of the metal substrate, the method further includes: introducing hydrogen gas into the reaction chamber, wherein the gas volume flow rate of the hydrogen gas is 10 sccm to 20 sccm.

[0029] In a second aspect of the present application, a metal graphene composite material is provided, which is prepared by the method described in the first aspect.

[0030] In a possible implementation of the second aspect, the metal graphene composite material includes 3 to 5 layers of the metal graphene composite layer.

[0031] In a possible implementation of the second aspect, in the metal graphene composite material, metal substrates included in different layers of the metal graphene composite layers are the same or different.

[0032] In a possible implementation of the second aspect, the metal substrates of different layers are independently selected from a single metal or an alloy composed of multiple metals selected from iron, cobalt, nickel, magnesium, copper, and titanium.

[0033] The third aspect of the present application provides an application of the metal graphene composite material as described in the second aspect in the preparation of electronic components.

[0034] In a fourth aspect of the present application, an electronic component is provided, comprising:

[0035] The metal graphene composite material as described in the second aspect.

[0036] In a possible implementation of the fourth aspect, the electronic component is a printed circuit board, a lithium battery or a transformer.

[0037] In the preparation method of metal graphene composite material provided in the present application, by applying pulse current to the metal substrate, the metal substrate is subjected to surface heat treatment, the Joule heating effect and the electroplastic effect can be used to adjust the microstructure of the metal substrate well, so as to facilitate the effective control of the morphology and evolution rate of the microstructure on the surface of the metal substrate at different heat treatment stages, so as to provide a more favorable microenvironment for graphene nucleation and growth, and improve the nucleation and growth rate of graphene, thereby improving the preparation efficiency of the metal graphene composite material, and reducing the problems of large heat loss, long heating time, low preparation efficiency, and possible environmental pollution caused by the traditional heating method. At the same time, by providing a more favorable surface microenvironment for graphene nucleation and growth, it is also possible to obtain a microstructure with less annealing twins, lower dislocation density, and fine grains, thereby, a metal graphene composite material with higher strength and compactness can be obtained. In addition, it is found through testing that the metal graphene composite material thus obtained has better mechanical properties and is not prone to wrinkles and bends. Moreover, through the stacking and sintering of metal graphene composite materials, the industrialization needs and batch and large-scale production of products with microstructures can be realized, and production efficiency can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 A microstructure morphology image of a metal substrate of a metal-graphene composite layer provided in Example 1;

[0039] Figure 2 A microstructure morphology image of a metal substrate of a metal-graphene composite layer provided in Example 4;

[0040] Figure 3 A microstructure morphology of a metal substrate of a metal-graphene composite layer provided in Comparative Example 1;

[0041] Figure 4 A microstructure morphology of a metal substrate of a metal-graphene composite layer provided in Comparative Example 2;

[0042] Figure 5 The metal substrate is AZ31 magnesium alloy at a pulse current density of 20A / mm 2 Microstructure morphology of the following figure;

[0043] Figure 6 The metal substrate is AZ31 magnesium alloy at a pulse current density of 40A / mm 2 Microstructure morphology of the following figure;

[0044] Figure 7 The metal substrate is AZ31 magnesium alloy at a pulse current density of 80A / mm 2 Microstructure morphology of the following figure;

[0045] Figure 8 The metal substrate is copper alloy at a pulse current density of 1200A / mm 2 Microstructure morphology of the following figure;

[0046] Fig. 9 The metal substrate is copper alloy at a pulse current density of 2200A / mm 2 Microstructure morphology of the following figure;

[0047] Fig.10 The metal substrate is copper alloy at a pulse current density of 3000A / mm 2 Microstructure morphology of the following figure;

[0048] Fig.11 The metal substrate is titanium alloy and the pulse current density is 0A / mm 2 Microstructure morphology of the following figure;

[0049] Fig.12 The metal substrate is titanium alloy and the pulse current density is 100A / mm 2 Microstructure morphology of the following figure;

[0050] Fig.13 The metal substrate is titanium alloy and the pulse current density is 140A / mm 2 Microstructure morphology of the following figure;

[0051] Fig.14 The metal substrate is a rare earth magnesium alloy and the pulse current density is 0A / mm 2Microstructure morphology of the following figure;

[0052] Fig.15 The metal substrate is a rare earth magnesium alloy at a pulse current density of 15A / mm 2 Microstructure morphology of the following figure;

[0053] Fig.16 The metal substrate is a rare earth magnesium alloy at a pulse current density of 40A / mm 2 Microstructure morphology of the following. DETAILED DESCRIPTION

[0054] In order to facilitate the understanding of the present application, the present application will be described more comprehensively with reference to the relevant drawings below. The preferred embodiments of the present application are given in the drawings. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.

[0055] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which the present application belongs. The terms used herein in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0056] In order to solve the problem that the traditional heating process in the related art cannot meet the high strength and high density requirements of the metal graphene composite material, the applicant has sought a new and effective heat treatment process to solve the above problem. The specific implementation method is described as follows:

[0057] Some embodiments of the present application provide a method for preparing a metal-graphene composite material, comprising:

[0058] S1), growing graphene on the surface of the metal substrate to prepare a metal-graphene composite layer;

[0059] S2), stacking at least two metal-graphene composite layers along their thickness direction so that the metal substrates on two adjacent metal-graphene composite layers face back to back, and preparing the metal-graphene composite material by hot pressing and sintering;

[0060] Wherein, in S1), the surface heat treatment of the metal substrate is performed by applying a pulse current to the metal substrate.

[0061] A pulse is a waveform of voltage or current, like the waveform of a pulse on an electrocardiogram. A pulse current is a current that changes suddenly and has a very short action time. It can be periodic or non-periodic.

[0062] According to needs, the waveform of the pulse current includes square wave, triangle wave, sawtooth wave, step wave, etc., which is not specifically limited here.

[0063] As a high-density energy input method, pulse current can, on the one hand, transfer heat densely to the metal substrate, which can rapidly heat up the metal substrate in a very short time, produce Joule heating effect, and effectively avoid the heat loss caused by the traditional heating process, thereby shortening the heating time and improving the heating efficiency, thereby improving the production efficiency of metal graphene composite materials and reducing energy consumption. On the other hand, compared with the traditional heating process, pulse current is more suitable for heating products with microstructures, which can concentrate the heating heat on the surface of the microstructured products, improve the heat utilization efficiency and reduce heat spillover. On the other hand, compared with the traditional heating process that may generate a lot of pollution, electric heating can also reduce exhaust emissions, which has the advantages of energy saving and environmental protection.

[0064] In addition, compared with direct current, which only has current or voltage to adjust, pulse current has three independent parameters: pulse current density, pulse on-time and pulse off-time, which is more conducive to adjusting the heating temperature and the microstructure of the metal substrate surface.

[0065] Specifically, by applying a pulse current to the metal substrate and utilizing the Joule heating effect and the electroplastic effect, the microstructure of the metal substrate can be well adjusted.

[0066] The changes in the microstructure of the metal substrate during heating are as follows:

[0067] After plastic deformation, the metal substrate will be in a thermodynamically unstable high free energy state due to the increase in the density of structural defects such as vacancies and dislocations, as well as the increase in distortion energy (energy stored in crystal defects), and will tend to spontaneously recover to the low free energy state before deformation. However, at room temperature, the atomic activity is small and the recovery is very slow. Once heated, at high temperatures, the atomic diffusion capacity increases, and a series of changes in organization and performance will occur. This change process can be manifested in three stages as the heating temperature increases: recovery stage, recrystallization stage, and grain growth stage.

[0068] In the recovery stage, when the cold plastically deformed metal is heated, some substructure and performance changes will occur before the optical microstructure changes (that is, before the recrystallized grains are formed). During this stage, the strength and hardness of the metal substrate change very little, and the internal stress and resistance decrease significantly.

[0069] In the recrystallization stage, the core of new non-distorted grains is first generated in the area with large distortion, and then gradually consumes the surrounding deformed matrix and grows until the deformed structure is completely reorganized into new, non-distorted fine equiaxed grains. In this stage, the strength and hardness of the metal substrate decrease significantly, the plasticity increases, the density increases sharply, the work hardening is eliminated, and the performance returns to the level before deformation.

[0070] In the grain growth stage, driven by the surface energy of the grain boundaries, new grains engulf each other and grow, and finally obtain grains of relatively stable size. In this stage, the strength and hardness of the metal substrate continue to decrease, and the plasticity continues to increase, and decreases when the coarsening is serious.

[0071] Here, it should be noted that the size of the grains after recrystallization annealing mainly depends on the pre-deformation degree and the annealing temperature. The greater the deformation degree, the finer the grains after annealing, and vice versa, the coarser the grains. In addition, some face-centered cubic metals and alloys such as copper and copper alloys, nickel and nickel alloys, and austenitic stainless steel will have annealing twins after cold deformation and recrystallization annealing. The reason is that these metals have low stacking fault energy and meet the energy conditions for twin growth.

[0072] Based on the above microstructure change process of the metal substrate during heating, by applying a pulse current to the metal substrate, the Joule heating effect and the electroplastic effect can be used to adjust the microstructure of the metal substrate well, so that the morphology and evolution rate of the microstructure on the surface of the metal substrate can be effectively controlled at different heat treatment stages, so that a more favorable microenvironment can be provided for graphene nucleation and growth, and the nucleation and growth rate of graphene can be improved. At the same time, by providing a more favorable surface microenvironment for graphene nucleation and growth, it is also possible to obtain a microstructure with less annealing twins, lower dislocation density, and fine grains, thereby, a metal-graphene composite material with higher strength and compactness can be obtained, which is unattainable in the related art. In addition, it is found through testing that the metal-graphene composite material thus obtained has better mechanical properties and is not prone to wrinkles and bending. And by stacking and sintering metal-graphene composite materials, industrialization needs can also be achieved.

[0073] Among them, in the preparation process of the metal graphene composite material, according to the different microstructures of the metal substrate at different heat treatment stages, pulse currents with different parameters can be applied to the metal substrate as needed.

[0074] In some embodiments, in S1), the surface heat treatment includes a multi-stage heat treatment process, and according to the same heating temperature of the metal substrate in different heat treatment stages, the value ranges of the pulse current density applied to the metal substrate in different stages are controlled to be the same, according to the different heating temperatures of the metal substrate in different heat treatment stages, the value ranges of the pulse current density applied to the metal substrate in different stages are controlled to be different, and the power supply frequency and duty cycle of the pulse current applied to the metal substrate in different stages are controlled to be the same.

[0075] In a pulse cycle, since the current is only on for part of the time and is zero for the rest of the time, the current density can be divided into average current density and peak current density. The peak current density is also the pulse current density. The pulse current density cannot increase vertically from zero to the peak value, but requires a certain "climbing". The current density "climbs" to the peak value to obtain the pulse current density. The power supply frequency refers to the number of times from one peak to another per second. The duty cycle refers to the percentage of the pulse conduction time in the entire pulse cycle time in a pulse cycle.

[0076] In these embodiments, by controlling the same heating temperature in different heat treatment stages, the same value range of the pulse current density applied to the metal substrate, and the same value range of the power supply frequency and duty cycle of the pulse current applied to the metal substrate in different stages, the parameters of the power supply of the pulse current in different stages can be effectively controlled to reduce the complexity of power supply control. According to the different heating temperatures in different heat treatment stages, the value range of the pulse current density applied to the metal substrate in different stages is controlled to be different, and by combining the pulse current density with the power supply frequency and duty cycle and other parameters, the metal substrate can be heated to the corresponding temperature within a certain time range, and the corresponding microstructure of the metal substrate in different heat treatment stages can be obtained.

[0077] Here, in S1), there is no specific limitation on the parameter setting of the pulse current adopted in different heat treatment stages, as long as the conditions that the heating temperature of the metal substrate in different heat treatment stages is the same, the value range of the pulse current density applied to the metal substrate is the same, the heating temperature of the metal substrate in different heat treatment stages is different, the value range of the pulse current density applied to the metal substrate is different, and the value range of the power frequency and duty cycle applied to the metal substrate in different stages are controlled to be the same can be met.

[0078] In some embodiments, in S1), the surface heat treatment of the metal substrate is performed by applying a pulse current to the metal substrate, comprising:

[0079] In the pretreatment stage of the metal substrate, a first pulse current is applied to the metal substrate to heat the metal substrate to a first temperature for a first preset time;

[0080] During the graphene deposition stage, a second pulse current is applied to the metal substrate to heat the metal substrate to a second temperature for a second preset time;

[0081] In the graphene growth stage, applying a third pulse current to the metal substrate to heat the metal substrate to the first temperature for a third preset time;

[0082] Among them, the first temperature is the recovery and recrystallization temperature of the metal substrate, the second temperature is the phase change temperature of the metal substrate, the pulse current density of the first pulse current and the third pulse current has the same value range, and the pulse current density of the first pulse current and the second pulse current has a different value range; the power supply frequency value range and duty cycle value range of the first pulse current, the second pulse current and the third pulse current are all the same.

[0083] In the embodiment of the present application, in the pretreatment stage of the metal substrate, by applying the first pulse current to the metal substrate, the first pulse current can greatly improve the plasticity of the metal substrate, reduce the forming force, improve the forming limit of the material and improve the surface quality of the metal substrate. Compared with the traditional heating process, it is more conducive to achieving efficient heating and can save energy. In addition, the first pulse current can make the internal grain orientation of the metal substrate tend to be consistent, and can achieve the effect of grain refinement by enhancing the mobility of vacancies and dislocations and the migration of atoms, so that the quality of graphene deposited and grown later can be higher, and the nucleation of graphene can be promoted. In the deposition stage of graphene, by applying the second pulse current to the metal substrate, on the one hand, graphene can be deposited under the action of the pulse current, which has the characteristics of high efficiency and energy saving. On the other hand, the Joule heat and electroplastic effect generated by applying the second pulse current promote dislocation slip, climb and annihilation, and improve the evolution rate of the microstructure, thereby accelerating the recovery and recrystallization process of the metal, so that it can obtain a microstructure with fewer annealing twins, lower dislocation density and fine grains, which can make the metal substrate have better mechanical properties. During the graphene growth stage, by applying a third pulse current to the metal substrate, the problem that the thickness of the composite material decreases as the graphene deposition proceeds and the forming performance gradually decreases can be improved, and the cracking failure caused by uneven deformation during forming can be improved.

[0084] During the whole treatment process, in the pretreatment stage of the metal substrate and the graphene growth stage, by applying the first pulse current and the third pulse current to the metal substrate, the rapid heating of the metal substrate can be achieved through the Joule heating effect, and the recovery and recrystallization rate of the metal substrate when the pulse current is applied can be increased, thereby accelerating the graphene deposition efficiency. In the graphene deposition stage, by applying the second pulse current to the metal substrate, the rapid heating and cooling of the metal substrate can be achieved through the Joule heating effect, and an instantaneous thermal stress is generated in this process, so that the metal substrate on which the graphene is deposited is deposited and formed under the influence of the thermal stress. In this process, by controlling the value range of the pulse current density of the first pulse current to be different from the value range of the pulse current density of the second pulse current, for example, a higher pulse current density can be used to make the formation rate of the crystal nucleus much greater than the growth rate of the original crystal, so that fine crystal grains can be formed, so that the crystal is fine and dense, and the composite material with graphene deposited on the surface can obtain better mechanical properties.

[0085] In some embodiments, a lower limit value of a value range of the pulse current density of the first pulse current is greater than an upper limit value of a value range of the pulse current density of the second pulse current.

[0086] There is no specific limitation on the specific value ranges of the parameters such as the pulse current density, power frequency and duty cycle of the first pulse current, the second pulse current and the third pulse current, as long as the above-mentioned processing conditions are met.

[0087] In some embodiments, the metal substrate is copper; the pulse current density of the first pulse current and the third pulse current are both in the range of 2000A / mm 2 ~2500A / mm 2 ; The pulse current density of the second pulse current has a value range of 1200A / mm 2 ~1800A / mm 2 .

[0088] In these embodiments, the pulse current density of the first pulse current and the third pulse current may be 2000A / mm 2 ~2500A / mm 2 The pulse current density of the second pulse current can be 1200A / mm 2 ~1800A / mm 2 It can reduce the difficulty of selecting other parameters of the pulse current when the above processing conditions are met.

[0089] In some embodiments, the pulse current density of the first pulse current may be 2000 A / mm 2 、2100A / mm2 、2200A / mm 2 、2300A / mm 2 、2400A / mm 2 and 2500A / mm 2 The pulse current density of the second pulse current can be 1200A / mm 2 、1300A / mm 2 、1400A / mm 2 , 1500A / mm 2 、1600A / mm 2 、1700A / mm 2 and 1800A / mm 2 The pulse current density of the third pulse current can be 2000A / mm 2 、2100A / mm 2 、2200A / mm 2 、2300A / mm 2 、2400A / mm 2 and 2500A / mm 2 Any value in .

[0090] In other embodiments, the metal substrate is nickel; the pulse current density of the first pulse current and the third pulse current are both in the range of 1000A / mm 2 ~1500A / mm 2 The pulse current density of the second pulse current has a value range of 500A / mm 2 ~800A / mm 2 .

[0091] In these embodiments, the pulse current density of the first pulse current and the third pulse current may be 1000 A / mm 2 ~1500A / mm 2 The pulse current density of the second pulse current can be 500A / mm 2 ~800A / mm 2 It can reduce the difficulty of selecting other parameters of the pulse current when the above processing conditions are met.

[0092] In some embodiments, the pulse current density of the first pulse current may be 1000 A / mm 2 、1100A / mm 2 , 1200A / mm 2 、1300A / mm 2 、1400A / mm 2 and 1500A / mm2 The pulse current density of the second pulse current can be 500A / mm 2 、600A / mm 2 、700A / mm 2 、800A / mm 2 The pulse current density of the third pulse current can be 1000A / mm 2 、1100A / mm 2 , 1200A / mm 2 、1300A / mm 2 、1400A / mm 2 and 1500A / mm 2 Any value in .

[0093] In some embodiments, the power supply frequencies of the first pulse current, the second pulse current, and the third pulse current are all in the range of 100 Hz to 1000 Hz.

[0094] In these embodiments, the power supply frequencies of the first pulse current, the second pulse current and the third pulse current are all within the same value range, which can reduce the complexity of controlling the pulse power supply. At the same time, the power supply frequency is within the range of 100 Hz to 1000 Hz, which is easy to implement.

[0095] In some embodiments, the pulse duty cycle of the first pulse current, the second pulse current and the third pulse current are all 0.1 to 0.5. In these embodiments, the duty cycles of the first pulse current, the second pulse current and the third pulse current are all within the same value range, which can reduce the complexity of the control of the pulse power supply. At the same time, the duty cycle value range is within the range of 0.1 to 0.5, which is easy to implement. In some embodiments, the value ranges of the first preset time and the third preset time are the same, both of which are 5min to 10min; the value range of the second preset time is different from the value range of the first preset time, and the upper limit value of the value range of the second preset time is less than or equal to the lower limit value of the value range of the first preset time.

[0096] In these embodiments, by keeping the value range of the first preset time and the third preset time the same, a metal-graphene composite material with higher quality can be obtained, and the entire graphene deposition time can be shortened to the greatest extent, thereby improving efficiency. At the same time, by controlling the upper limit of the value range of the second preset time to be less than or equal to the lower limit of the value range of the first preset time, the quality of the metal-graphene composite material can be effectively controlled, and the preparation time of the metal-graphene composite material can be reduced to the greatest extent, thereby further improving efficiency.

[0097] In some embodiments, it is found through experiments that the value range of the second preset time is 1 min to 5 min.

[0098] In some embodiments, during the pretreatment stage of the metal substrate, the method further includes: introducing hydrogen gas into the reaction chamber, wherein the gas volume flow rate of the hydrogen gas is 10 sccm to 20 sccm.

[0099] In these embodiments, the role of hydrogen is to inhibit carbon from dissolving into the metal substrate, so as to facilitate the deposition of carbon atoms on the surface of the metal substrate. By applying a first pulse current to the metal substrate and heating the metal substrate, the recovery and recrystallization rate of the metal substrate can be increased, and the pretreatment time of the metal substrate can be shortened. In this way, under the same gas volume flow rate of hydrogen, the total amount of hydrogen introduced can be reduced while ensuring a higher quality of the metal-graphene composite material, thereby saving resources.

[0100] In some embodiments, during the graphene deposition stage, the method further includes: introducing a protective gas, an auxiliary gas and a carbon source into the reaction chamber, wherein the gas volume flow rate of the protective gas is 100 sccm to 120 sccm, and the gas volume flow rate of the auxiliary gas is 20 sccm to 100 sccm.

[0101] In these embodiments, similar to the above-mentioned introduction of hydrogen into the reaction chamber, by applying a second pulse current to the metal substrate to heat the metal substrate, the deposition rate of graphene can be increased and the deposition time can be shortened. In this way, when the gas volume flow of the protective gas and the auxiliary gas remains unchanged, the total amount of the protective gas and the auxiliary gas introduced can be reduced while ensuring the quality of the metal-graphene composite material, which can also save resources. At the same time, since it is more conducive to the deposition of the carbon source, the carbon source can be saved and the utilization efficiency of the carbon source can be improved.

[0102] The carbon source may be a gaseous carbon source, a liquid carbon source or a solid carbon source, which is not specifically limited here.

[0103] In some embodiments, the carbon source may be a gaseous carbon source such as methane, ethylene, etc. At this time, the gas volume flow rate of the carbon source may be 5 sccm.

[0104] In some embodiments, the protective gas may be argon, nitrogen, helium, etc. The auxiliary gas may be hydrogen.

[0105] The material of the metal substrate is not specifically limited and can be any metal single substance or alloy with high electrical conductivity.

[0106] In some embodiments, the metal substrate can be independently selected from a single metal or an alloy composed of multiple metals selected from iron, cobalt, nickel, magnesium, copper, and titanium.

[0107] In the above hot pressing sintering process, the metal substrates included in the at least two metal-graphene composite layers may be the same or different.

[0108] In some embodiments, after the metal graphene composite layer is prepared, before at least two metal graphene composite layers are sintered, the metal graphene composite layer is cut into a rectangle with certain size requirements, and ultrasonically cleaned in acetic acid, deionized water, and ethanol solution for 5 minutes. Some embodiments of the present application provide a metal graphene composite material prepared by the method as described above. The metal graphene composite material comprises at least two layers of metal graphene composite layers.

[0109] In some embodiments, the metal graphene composite material comprises 3 to 5 metal graphene composite layers.

[0110] Among the at least two metal-graphene composite layers, the metal substrates included in different layers of the metal-graphene composite layers may be the same or different, which is not specifically limited here.

[0111] In some embodiments, in the metal graphene composite material, different layers of the metal graphene composite layer contain different metal substrates.

[0112] For example, when the metal-graphene composite material includes three metal-graphene composite layers, the materials of the metal substrates included in the metal-graphene composite layers arranged sequentially from bottom to top may be copper, cobalt and nickel, respectively.

[0113] Some embodiments of the present application provide a use of the metal graphene composite material as described above in the preparation of electronic components.

[0114] In some embodiments, the electronic component may be a circuit board, a super capacitor, etc.

[0115] Metal graphene composites can be used as conductive layers in circuit boards and supercapacitors. In addition to having higher strength, they also have better electrothermal properties than metal and graphene alone.

[0116] Some embodiments of the present application provide an electronic component, including: the metal graphene composite material as described above.

[0117] In some embodiments, the electronic component may be a printed circuit board, a lithium battery, or a transformer.

[0118] When the electronic components include printed circuit boards, the metal graphene composite material can be the conductive layer in the printed circuit board; when the electronic components include lithium batteries, the metal graphene composite material can be the electrodes in the lithium batteries; when the electronic components include transformers, the metal graphene composite material can be the capacitor plates in the transformers.

[0119] The above introduces the specific implementation methods of the present application. In order to objectively illustrate the technical effects produced by the present application, the following examples and comparative examples will be used for description.

[0120] In the following examples and comparative examples, all raw materials can be purchased in commercial form, and in order to maintain the reliability of the experiment, the raw materials used in the following examples and comparative examples have the same physical and chemical parameters or are processed in the same way.

[0121] Example 1

[0122] Preparation of metal graphene composites:

[0123] Step 1) Pretreatment of metal substrate: Select copper foil as the growth substrate of graphene, pretreat the copper foil, introduce 10sccm hydrogen, and adjust the pulse power supply to make the pulse current density reach 2000A / mm 2 , adjust the pulse power frequency to 100Hz, adjust the pulse duty cycle to 0.1, under this environment, the copper foil temperature reaches 800℃, and the current is continuously passed for 5 minutes to complete the recrystallization of the copper foil surface to remove impurity elements.

[0124] Step 2), graphene deposition: 100 sccm of argon, 100 sccm of hydrogen and 5 sccm of methane are continuously introduced into the surface of the copper foil, and the pulse power supply is adjusted to make the pulse current density reach 1200A / mm 2 , adjust the pulse power frequency to 100Hz, adjust the pulse duty cycle to 0.1, under this environment, the copper foil temperature reaches 300℃, and the current is continuously passed for 1min to complete the deposition of graphene on the copper foil surface.

[0125] Step 3), graphene growth: Post-process the copper foil with graphene deposited on the surface, continuously introduce 100sccm of argon gas, and adjust the pulse power supply to make the pulse current density reach 2000A / mm 2 , adjust the pulse power frequency to 100Hz, and adjust the pulse duty cycle to 0.1. Under this environment, the copper foil temperature reaches 800℃, and the current is continuously passed for 5 minutes. At this time, the copper foil with the graphene film deposited is deformed under the action of thermal compression stress, completing the growth of graphene, thereby completing the preparation of the copper-graphene composite film material.

[0126] Step 4), the obtained copper-graphene composite film material is subjected to three-layer stacking sintering, and two adjacent layers of the copper-graphene composite film material are contact-formed under vacuum conditions to obtain a metal-graphene composite material, and the sintering time is 2 hours.

[0127] Example 2

[0128] The preparation method of Example 2 is basically the same as the preparation method of Example 1, except that: in step 1), the gas volume flow rate of hydrogen is adjusted to 12 sccm, and the pulse current density is adjusted to 2500 A / mm 2 , adjust the pulse power frequency to 500Hz, adjust the pulse duty cycle to 0.5, the copper foil temperature to 1000℃~1083℃, and continuously pass the pulse current for 10min. In step 2), adjust the gas volume flow rate of argon to 200sccm, the gas volume flow rate of hydrogen to 20sccm, the gas volume flow rate of methane to 30sccm, adjust the pulse current density to 1800A / mm2, adjust the pulse power frequency to 500Hz, adjust the pulse duty cycle to 0.5, the copper foil temperature to 500℃, and continuously pass the pulse current for 5min. In step 3), adjust the gas volume flow rate of argon to 200sccm, and adjust the pulse power supply to make the pulse current density reach 2500A / mm 2 , the pulse power frequency is adjusted to 100 Hz, the pulse duty ratio is adjusted to 0.1, the temperature of the copper foil is 1000°C to 1083°C, and the pulse current is continuously supplied for 10 minutes. In step 4), the copper-graphene composite film material is sintered in 5 layers for 2 hours.

[0129] Example 3

[0130] The preparation method of Example 3 is basically the same as the preparation method of Example 1, except that: in step 1), the gas volume flow rate of hydrogen is adjusted to 11 sccm, and the pulse current density is adjusted to 2300 A / mm 2 , the pulse power frequency is adjusted to 1000Hz, the pulse duty ratio is adjusted to 0.3, the copper foil temperature is 1000℃~1083℃, and the pulse current is continuously supplied for 10min. In step 2), the gas volume flow rate of argon gas is adjusted to 150sccm, the gas volume flow rate of hydrogen gas is adjusted to 50sccm, the gas volume flow rate of methane gas is adjusted to 30sccm, and the pulse current density is adjusted to 1500A / mm 2 , adjust the pulse power frequency to 1000Hz, adjust the pulse duty cycle to 0.3, the temperature of the copper foil to 500℃, and continue to pass the pulse current for 3min. In step 3), adjust the gas volume flow rate of the introduced argon gas to 150sccm, adjust the pulse power supply, and make the pulse current density reach 2300A / mm 2, the pulse power frequency is adjusted to 200 Hz, the pulse duty ratio is adjusted to 0.2, the temperature of the copper foil is 1000°C to 1083°C, and the pulse current is continuously supplied for 8 minutes. In step 4), the copper-graphene composite film material is sintered in 4 layers for 2 hours.

[0131] Example 4

[0132] The preparation method of Example 4 is basically the same as that of Example 1, except that nickel is used as the growth substrate of graphene in step 1), and the pulse current density is adjusted to 1200 A / mm 2 , the temperature of nickel is 1400℃~1453℃, and the pulse current is continuously applied for 5min. In step 2), the pulse current density is adjusted to 800A / mm 2 , the nickel temperature is 800°C, and the pulse current is continuously applied for 1 min. In step 3), the pulse power supply is adjusted to make the pulse current density reach 1200A / mm 2 , the temperature of nickel is 1400° C. to 1453° C. In step 4), the copper-graphene composite film material is sintered in 10 layers for 2 hours.

[0133] Example 5

[0134] The preparation method of Example 5 is basically the same as that of Example 4, except that: in step 1), the pulse current density is adjusted to 1000 A / mm 2 , the temperature of nickel is 1400℃~1453℃, and the pulse current is continuously applied for 8min. In step 2), the pulse current density is adjusted to 600A / mm 2 , the nickel temperature is 800°C, and the pulse current is continuously applied for 5 minutes. In step 3), the pulse power supply is adjusted to make the pulse current density reach 1000A / mm 2 , the temperature of nickel is 1400° C. to 1453° C. In step 4), the copper-graphene composite film material is sintered in 10 layers for 2 hours.

[0135] Example 6

[0136] The preparation method of Example 6 is basically the same as that of Example 4, except that: in step 1), the pulse current density is adjusted to 1500 A / mm 2 , the temperature of nickel is 1400℃~1453℃, and the pulse current is continuously applied for 10min. In step 2), the pulse current density is adjusted to 900A / mm 2, the nickel temperature is 800°C, and the pulse current is continuously applied for 2 minutes. In step 3), the pulse power supply is adjusted to make the pulse current density reach 1500A / mm 2 , the temperature of nickel is 1400° C. to 1453° C. In step 4), the copper-graphene composite film material is sintered in 10 layers for 2 hours.

[0137] Comparative Example 1

[0138] The preparation method of Comparative Example 1 is substantially the same as that of Example 1, except that the metal substrate is heat treated by fuel combustion, and the laminate sintering time is 2 hours.

[0139] Comparative Example 2

[0140] The preparation method of Comparative Example 1 is substantially the same as that of Example 4, except that the metal substrate is heat treated by fuel combustion, and the laminate sintering time is 2 hours.

[0141] The metal substrate microstructure of the metal graphene composite layer obtained by the preparation method of Example 1 is as follows: Figure 1 As shown, the microscopic morphology of the metal substrate of the metal graphene composite layer obtained by the preparation method of Example 4 is as follows Figure 2 As shown, the metal substrate microstructure of the metal graphene composite layer obtained by the preparation method of Comparative Example 1 is as follows Figure 3 As shown, the metal substrate microstructure of the metal graphene composite layer obtained by the preparation method of Comparative Example 2 is as follows Figure 4 shown.

[0142] Depend on Figure 1 and Figure 3 It can be seen that, compared with Comparative Example 1, the metal substrate in Example 1 has finer grains and a denser texture.

[0143] Depend on Figure 2 and Figure 4 It can be seen that compared with Comparative Example 2, the metal substrate of Example 2 has finer grains and a denser texture.

[0144] It should be noted here that, for the same metal, within a certain range of pulse current density, as the pulse current density increases, the grains of the metal substrate become finer and the texture becomes denser.

[0145] like Figure 5 , Figure 6 and Figure 7 As shown in the figure, when the metal substrate is AZ31 magnesium alloy, the metal substrate is subjected to a pulse current density of 20A / mm 2 , 40A / mm 2 、80A / mm 2Microstructure morphology of the structure. Figure 5 , Figure 6 and Figure 7 It can be seen that as the pulse current density increases, the density of the metal substrate of AZ31 magnesium alloy continues to increase.

[0146] like Figure 8 , Fig. 9 and Fig.10 As shown in the figure, when the metal substrate is a copper alloy, the metal substrate is subjected to a pulse current density of 1200A / mm 2 、2200A / mm 2 、3000A / mm 2 Microstructure morphology of the structure. Figure 8 , Fig. 9 and Fig.10 It can be seen that as the pulse current density increases, the density of the metal substrate of the copper alloy tends to increase continuously.

[0147] like Fig.11 , Fig.12 and Fig.13 As shown in the figure, when the metal substrate is a titanium alloy, the metal substrate is respectively 2 , 100A / mm 2 , 140A / mm 2 Microstructure morphology of the structure. Fig.11 , Fig.12 and Fig.13 It can be seen that as the pulse current density increases, the density of the metal substrate of the titanium alloy tends to increase continuously.

[0148] like Fig.14 , Fig.15 and Fig.16 As shown in the figure, when the metal substrate is a rare earth magnesium alloy, the metal substrate is respectively 2 , 15A / mm 2 , 40A / mm 2 Microstructure morphology of the structure. Fig.14 , Fig.15 and Fig.16 It can be seen that as the pulse current density increases, the density of the metal substrate of the rare earth magnesium alloy tends to increase continuously.

[0149] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0150] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.

Claims

1. A method for preparing a metal graphene composite material, characterized in that: include: S1), growing graphene on the surface of the metal substrate to prepare a metal-graphene composite layer; S2), stacking at least two of the metal-graphene composite layers along their thickness direction so that the metal substrates on the two adjacent metal-graphene composite layers face each other, and preparing the metal-graphene composite material by hot pressing and sintering; Wherein, in S1), the surface heat treatment of the metal substrate is performed by applying a pulse current to the metal substrate; In S1), the metal substrate is subjected to surface heat treatment by applying a pulse current to the metal substrate, comprising: In the pretreatment stage of the metal substrate, a first pulse current is applied to the metal substrate to heat the metal substrate to a first temperature for a first preset time; In the graphene deposition stage, applying a second pulse current to the metal substrate to heat the metal substrate to a second temperature for a second preset time; In the graphene growth stage, applying a third pulse current to the metal substrate to heat the metal substrate to the first temperature for a third preset time; Among them, the first temperature is the recovery and recrystallization temperature of the metal substrate, and the second temperature is the phase change temperature of the metal substrate; the value range of the pulse current density of the first pulse current and the third pulse current is the same, and the value range of the pulse current density of the first pulse current and the second pulse current is different; the value range of the power supply frequency and the value range of the duty cycle of the first pulse current, the second pulse current and the third pulse current are all the same.

2. The method according to claim 1, characterized in that A lower limit value of a value range of the pulse current density of the first pulse current is greater than an upper limit value of a value range of the pulse current density of the second pulse current.

3. The method according to claim 1 or 2, characterized in that: The metal substrate is copper; The pulse current density of the first pulse current and the third pulse current is in the range of 2000A / mm 2 ~2500A / mm 2 ; The pulse current density of the second pulse current is in the range of 1200A / mm 2 ~1800A / mm 2 .

4. The method according to claim 1 or 2, characterized in that: The metal substrate is nickel; The pulse current density of the first pulse current and the third pulse current is in the range of 1000A / mm 2 ~1500A / mm 2 ; The pulse current density of the second pulse current is in the range of 500A / mm 2 ~800A / mm 2 .

5. The method according to claim 1 or 2, characterized in that: The power supply frequencies of the first pulse current, the second pulse current and the third pulse current all range from 100 Hz to 1000 Hz.

6. The method according to claim 1 or 2, characterized in that: The duty ratios of the first pulse current, the second pulse current and the third pulse current are all in the range of 0.1 to 0.

5.

7. The method according to claim 1 or 2, characterized in that: The first preset time and the third preset time have the same value range, both of which are 5 minutes to 10 minutes; The value range of the second preset time is different from the value range of the first preset time, and an upper limit value of the value range of the second preset time is less than or equal to a lower limit value of the value range of the first preset time.

8. The method according to claim 7, characterized in that The second preset time has a value range of 1 minute to 5 minutes.

9. The method according to claim 1 or 2, characterized in that: In the pretreatment stage of the metal substrate, the method further includes: introducing hydrogen into the reaction chamber, wherein the gas volume flow rate of the hydrogen is 10 sccm to 20 sccm.

10. A metal graphene composite material, characterized in that: It is prepared by the method according to any one of claims 1 to 9.

11. The metal graphene composite material according to claim 10, characterized in that: The metal graphene composite material comprises 3 to 5 metal graphene composite layers.

12. The metal graphene composite material according to claim 10, characterized in that: In the metal graphene composite material, the metal substrates included in different layers of the metal graphene composite layer are the same or different.

13. The metal graphene composite material according to claim 12, characterized in that: The metal substrates of different layers are independently selected from a single metal or an alloy composed of multiple metals among iron, cobalt, nickel, magnesium, copper and titanium.

14. Use of the metal graphene composite material according to any one of claims 10 to 13 in the preparation of electronic components.

15. An electronic component, characterized in that: include: The metal graphene composite material according to any one of claims 10 to 13.

16. The electronic component according to claim 15, characterized in that: The electronic components are printed circuit boards, lithium batteries or transformers.