A method for reducing pyrite content and COD in hard kaolinite

Through a dry process that combines selective grinding and separation technology, the problem of low removal efficiency of pyrite and organic carbon in hard kaolinite is solved, and efficient pyrite and COD value reduction are achieved, improving the Purity and resource utilization of hard kaolinite.

CN115532409BActive Publication Date: 2024-10-29CHINA UNIV OF GEOSCIENCES (WUHAN) +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202211143764.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-20
Publication Date
2024-10-29
Estimated Expiration
2042-09-20

AI Technical Summary

Technical Problem

The existing technology has the problems of high energy consumption, complex process, and low removal efficiency when removing pyrite and organic carbon from hard kaolinite. It is especially difficult to effectively separate pyrite from coal gangue with uneven particle size, resulting in Resource waste and environmental pollution.

Method used

Using a dry process that combines selective grinding and sorting technology, through steps such as crushing, photoelectric sorting, impact milling and gravity winnowing, fluorescence detection sorting and impact force are used to separate pyrite and kaolinite, reducing yellowing. Iron ore content and chemical oxygen demand (COD value).

Benefits of technology

The pyrite removal rate is 46%~72% and the COD removal rate is 49%~57%, which improves the purity and resource utilization of hard kaolinite and reduces energy consumption and process complexity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115532409B_ABST
    Figure CN115532409B_ABST
Patent Text Reader

Abstract

The present invention provides a method for reducing the pyrite content and COD value in hard kaolinite, and relates to the technical field of hard kaolinite processing. The present invention uses hard kaolinite containing coarse-grained aggregates of pyrite as raw material, and finally reduces the pyrite content and COD value in hard kaolinite through multiple crushing, screening, photoelectric sorting, classification and other steps. The present invention combines the process of selective grinding and sorting technology, and the production process is dry, non-heating, energy-saving and efficient. It is different from conventional magnetic separation, chemical method, and gravity separation iron removal. It combines photoelectric sorting, multi-stage impact crushing and gravity winnowing. The pressing and impact forces are used to separate the pyrite aggregated from the kaolinite. At the same time, because pyrite and organic carbon form oolitic or bean-shaped inclusions, pyrite impurities and organic carbon can be removed efficiently at the same time, and the removal rate of pyrite in hard kaolinite can reach 46%~72%, and the removal rate of COD can reach 49~57%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hard kaolinite processing, in particular to a method for reducing the pyrite content and COD value in hard kaolinite. Background Art

[0002] Hard kaolinite, also known as coal-based kaolin, refers to the solid waste discharged during the mining and washing process of coal. The output of hard kaolinite accounts for about 10% of the total coal output. According to the latest statistics, the current stockpile of gangue in my country has reached more than 4.5 billion tons, and it is increasing at a rate of 300 million tons / year. It is one of the solid wastes with the largest output and stockpile in the industry. The stockpile of hard kaolinite not only causes serious waste of resources, but also causes varying degrees of pollution to the environment such as the atmosphere, soil and water sources. If the research on its comprehensive utilization of resources is strengthened, the gangue can be transformed into useful resources. Hard kaolinite in many places contains a certain amount of pyrite. If the pyrite in the gangue is stripped out, on the one hand, high-quality kaolinite samples can be obtained, which can be used in various high-value-added products such as glass fiber, rock board, and raw materials for metakaolin. On the other hand, the pyrite obtained can be used as the best raw material for the production of sulfuric acid, which can create benefits and increase product added value.

[0003] In current technology, pyrite or organic carbon is usually separated and removed. For example, pyrite is removed by gravity separation, flotation, calcination, magnetic separation, and chemical methods (such as acid leaching); organic carbon is removed by calcination or flotation. The above methods generally have problems such as high energy consumption, complex processes, the need to use a large amount of organic reagents, and limited removal efficiency. Therefore, it is urgent to develop a low-carbon, energy-saving dry processing technology that can remove pyrite impurities in hard kaolinite while reducing its chemical oxygen demand (COD) content and improving the three rates.

[0004] Patent CN105819454A discloses a method for removing pyrite from quartz, which utilizes high-temperature calcination in an aerobic environment and a magnetic separation process to remove hematite. This process has high energy consumption; Patent CN103657838A discloses a method for recovering pyrite from coal gangue, which includes two-stage closed-circuit crushing of the coal gangue; grinding; and using acidified water glass, butyl xanthate, and No. 2 oil in roughing and concentrating to obtain corresponding concentrates and tailings. This process is relatively complicated and requires a lot of flotation chemical reagents; Patent CN105080702 discloses a dry enrichment process and system for coal-based pyrite. In the process, no crushing operation is performed. A dry heavy medium fluidized bed separator or a composite dry separator combined with a vibrating fluidized bed separator is used for the enrichment process to separate kaolinite and enrich pyrite. The core processing method focuses on the physical separation of the fluidized bed. Patent CN105665122 A provides a beneficiation method for recovering pyrite from coal gangue. The coal gangue is graded by a double-layer vibrating screen. The graded fine-grained products are sorted by a heavy medium vibrating chute to obtain concentrate products and tailings. After the concentrate products are freed from the medium, coarse-grained pyrite and tailings are obtained. The graded fine-grained products are subjected to grinding and classification, and the ore slime is removed. After flotation and sorting, coal + pyrite products and tailings are obtained. The process is relatively complicated and many flotation chemical reagents will be introduced. Patent CN105642433 A discloses a coal-bearing kaolin decarbonization process, including crushing, classification, gravity separation, crushing of intermediate density products of gravity separation or grinding and flotation operations, which are used to remove carbon from coal-bearing kaolin.

[0005] It can be seen that the current typical methods for removing pyrite from coal gangue include physical and chemical methods. The prominent problem of gravity separation is the low recovery rate of mineral processing, a large amount of pyrite is lost in the tailings, and the crushed ore is directly ground, resulting in high mineral processing costs; the extraction of pyrite in the flotation process requires the addition of complex reagents, including pH adjusters, inhibitors, activators, collectors, frothers, etc., and it is difficult to achieve a high grade through roughing, and a fine process is required. At the same time, clay minerals that are easy to mud will be adsorbed on the surface of pyrite, resulting in poor flotation selectivity. Especially for coal gangue with uneven embedded particle size, it is difficult to achieve effective separation simply through gravity separation or flotation; and acid immersion removal requires a large amount of acid solution, resulting in serious waste of raw materials.

[0006] In the process of mineral utilization, the sorting and enrichment of useful minerals is a very important step. Most minerals are embedded in very fine particles, and it is difficult to achieve fine separation by gravity separation. Therefore, mineral sorting mainly adopts the process of "dissociation + sorting". In the processing of hard kaolinite, the current indiscriminate grinding operation is not conducive to the dissociation and sorting of pyrite, organic carbon and kaolinite. The indiscriminate grinding operation will cause a large amount of pyrite, quartz and other conglomerates to be mixed into kaolinite, and because of the mixing of refined carbon powder, the COD value of the product is very high, which reduces the product quality. Dissociation, as a prerequisite for mineral sorting, directly affects the work efficiency of subsequent processes. At present, mineral dissociation is usually completed by crushers and mills. The crusher breaks large minerals into coarse-grained minerals, and the crusher product is deeply dissociated by the mill. The mill includes many types such as rod mills and ball mills. It can be operated alone or combined with a crusher to achieve mineral dissociation. At present, the sorting method is mainly flotation or physical screening to achieve the purpose of component separation. The existing selective grinding process generally operates in the following steps: the screen aperture is reduced from large to small, and multiple screenings are performed in combination with multiple ball millings to form multiple closed-circuit grinding operations. Only then can the selective grinding process be completed and the grade of the required mineral elements in the ore be improved. This results in a relatively complicated process, among which the problem of high energy consumption is particularly prominent. Summary of the invention

[0007] In order to overcome the above problems, the present invention provides a method for reducing the pyrite content and COD value in hard kaolinite, which specifically comprises the following steps:

[0008] The hard kaolinite containing the coarse-grained aggregate of pyrite is crushed to obtain D 97 Particles <40 mm;

[0009] The pellets are crushed and screened for the second time to obtain D 97 For particles <10 mm, the material on the sieve is crushed and sieved again;

[0010] The undersize material in step (2) is subjected to photoelectric separation to obtain pyrite and hard kaolinite with low pyrite content;

[0011] The present invention utilizes fluorescence detection sorting technology to classify ores with different pyrite grades, and selects ores with different pyrite contents by adjusting the material conveying speed and the nozzle controlled by the magnetic valve, wherein the ores with low pyrite content enter the next step of sorting, and the ores with high pyrite content can be used for other purposes;

[0012] The hard kaolinite with low pyrite content is subjected to two-stage impact and screening;

[0013] The present invention utilizes the difference in hardness and density between kaolinite and pyrite particles to break the minerals into different particle sizes under impact force, and then uses a screen of specific specifications to achieve the purpose of screening;

[0014] The secondary screen material in step (4) is subjected to gravity air separation and collected by a bag dust collector to obtain hard kaolinite with low COD value and low pyrite content.

[0015] Furthermore, the pyrite in the hard kaolinite is in the form of oolitic or bean-shaped inclusions.

[0016] Furthermore, the optical sorting is performed using an optical sorter, and the photoelectric sorting machine is an ultraviolet sorting machine or an X-ray sorting machine.

[0017] Furthermore, the material conveying speed in the photoelectric sorting process is 2 m / s to 5 m / s.

[0018] Furthermore, in the two-stage impact, the linear speed of the first-stage impact hammer is 50 m / s or 60 m / s, and the linear speed of the second-stage impact hammer is 75 m / s or 120 m / s.

[0019] Furthermore, the D of the hard kaolinite particles after secondary screening is 97 2 μm or 15 μm.

[0020] Furthermore, the air selection frequency is 16 Hz~32 Hz.

[0021] Furthermore, the hard kaolinite particles with low pyrite content and low COD value have a particle size of 2 μm or 10 μm.

[0022] The present invention also provides hard kaolinite with low pyrite content and COD value prepared according to the above method.

[0023] The present invention firstly utilizes the optical separation method to separate the hard kaolinite containing different grades of pyrite, so as to enrich the impurities of pyrite of different grades; after crushing, the photoelectric separation is utilized to first separate the different raw ores containing pyrite, so as to avoid the problem that the pyrite is not easy to be separated later due to the direct grinding of the pyrite; it is particularly suitable for coal-based kaolinite with uneven pyrite distribution particle size, and the pyrite resources therein are graded to greatly improve the recovery rate of kaolinite minerals; then the present invention utilizes the selective grinding technology, including the use of roller pressing and impact action mode, the use of pressure to dissociate the particles from the kaolinite, and the combination of impact grinding and screening mode to selectively grind and grade the kaolinite and pyrite of different hardness, and further separate the kaolinite. Pyrite, improve the purity of kaolinite; the use of impact mill is beneficial to prevent the impurities therein from being too finely ground, which is beneficial to the separation of the target ore kaolinite and the gangue pyrite. Selective grinding can not only reduce the formation of secondary ore slime, but also make the target mineral fully monomeric. However, there are many factors affecting selective grinding, such as the shape and size of the grinding medium, the ratio of various medium sizes, the rotation speed of the mill and the movement state of the medium, the discharge method of the mill, the diameter-to-length ratio of the mill, and the grinding concentration, etc. Therefore, the core of this method lies in the combination of impact force selection and screening; finally, the present invention utilizes the different movement trajectories of materials with different densities and particle sizes in the spiral medium flow for separation, such as using wind cyclone to separate pyrite and hard kaolinite.

[0024] Compared with the prior art, the beneficial technical effects of the present invention are:

[0025] The present invention develops a process combining selective grinding and sorting technology. The production process is dry, non-heating, energy-saving and efficient. Different from conventional magnetic separation, chemical method and gravity separation for iron removal, it combines photoelectric sorting, multi-stage impact crushing and sorting methods, and utilizes pressing and impact forces to separate the pyrite and kaolinite with aggregated particles. At the same time, because pyrite and organic carbon form oolitic or bean-shaped inclusions, pyrite impurities and organic carbon can be efficiently removed at the same time. Finally, the removal rate of pyrite in hard kaolinite is 46%-72%, and the removal rate of COD reaches 49%-57%. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The present invention will be further described below in conjunction with the accompanying drawings.

[0027] Figure 1 The process flow chart of the method for reducing the pyrite content and COD value in hard kaolinite of the present invention;

[0028] Figure 2 This is the XRD diagram of the hard kaolinite sample 1 of the present invention;

[0029] Figure 3 This is an optical microscope image of the hard kaolinite original sample 1 of the present invention;

[0030] Figure 4 This is the XRD pattern of the hard kaolinite sample 1 prepared in the present invention;

[0031] Figure 5 This is the XRD pattern of the hard kaolinite sample 2 of the present invention;

[0032] Figure 6 This is an optical microscope image of the hard kaolinite original sample 2 of the present invention;

[0033] Figure 7 This is the XRD pattern of the hard kaolinite sample 2 prepared in the present invention;

[0034] Figure 8 This is the XRD diagram of the hard kaolinite sample 3 of the present invention;

[0035] Fig. 9 This is an optical microscope image of the hard kaolinite original sample 3 of the present invention;

[0036] Fig.10 This is the XRD spectrum of the hard kaolinite sample 3 prepared in the present invention. DETAILED DESCRIPTION

[0037] The technical solution provided by the present invention is further described below in conjunction with embodiments. Example

[0038] A method for reducing the pyrite content and COD value in hard kaolinite, the steps are as follows:

[0039] Take hard kaolinite containing coarse-grained aggregates of pyrite, in which the pyrite may be in the form of oolitic or pea-shaped inclusions; select hard kaolinite samples, Figure 2 The XRD diagram of the selected hard kaolinite original sample 1 shows that the pyrite mineral phase content is 20.62% and the COD value is 88632 mg / kg. Figure 3 This is an optical microscope picture of the selected hard kaolinite sample 1;

[0040] The hard kaolinite ore was added into the jaw crusher and the ore sample was crushed to a particle size (D97) < 40 mm;

[0041] The above-mentioned fine particles are sent to the next step roller crusher for secondary crushing. After being controlled by the screening machine, the particles with a particle size (D97) <10 mm enter the next step of processing, and the crushed samples of the sieve are homogenized in the warehouse before grinding; the particles above 10 mm enter the roller crusher again;

[0042] The above-mentioned crushed particles under the sieve are sent to the photoelectric sorter through a conveyor belt. The selected photoelectric sorter is an ultraviolet or X-ray photoelectric sorter. The fluorescence phenomenon produced by the action of ultraviolet and X-ray light sources on pyrite is used, and the fluorescence detection sorting technology is used to classify ores with different pyrite grades. By adjusting the material conveying speed by 2 m / s, ores with different pyrite contents are sorted out, and the ores with low pyrite content enter the next step of sorting;

[0043] The hard kaolinite mineral with low pyrite content sorted by the above-mentioned photoelectric sorter is fed into an impact ultrafine grinding mill with a screen through a double screw feeder for selective grinding. The difference in hardness and density between kaolinite and pyrite particles will cause the mineral to be broken into different particle sizes under the impact force. The impact ultrafine grinding mill is equipped with a screen with adjustable sieve holes for two impacts and screening. By adjusting the impact hammer speed of the impact ultrafine grinding mill and the speed ratio of the two-stage hammer heads, the sieve holes are adjusted at the same time to control the first-stage hammer head linear speed to 60 m / s, the first-stage screening control; the second-stage hammer head linear speed is 120 m / s, the second-stage screening control, to form hard kaolinite ore particles (D97) in the range of 2 μm.

[0044] The secondary screen material is sent to the classifier, which is characterized by gravity air separation. By adjusting the parameters of the air separation equipment, 16 Hz, the kaolinite particle size is controlled to 2 μm.

[0045] The kaolinite sample was collected by using a bag dust collector to obtain a hard kaolinite sample 1 with low pyrite and low COD content. Figure 4 This is the XRD spectrum of hard kaolinite sample 1. The pyrite content is 5.76%, and the removal rate is 72%; the COD value is 38319 mg / kg, and the removal rate is 57%. Example

[0046] Take hard kaolinite containing coarse-grained aggregates of pyrite, in which the pyrite may be in the form of oolitic or pea-shaped inclusions; select hard kaolinite samples, Figure 5 The XRD diagram of the selected hard kaolinite sample 2, in which the pyrite phase content is 2.24%, COD15552 mg / kg, Figure 6 This is an optical microscope picture of the selected hard kaolinite sample 2;

[0047] The hard kaolinite ore was added into the jaw crusher and the ore sample was crushed to a particle size (D97) < 40 mm;

[0048] The above-mentioned fine particles are sent to the next step roller crusher for secondary crushing. After being controlled by the screening machine, the particles with a particle size (D97) <10 mm enter the next step of processing, and the crushed samples of the sieve are homogenized in the warehouse before grinding; the particles above 10 mm enter the roller crusher again;

[0049] The above-mentioned crushed particles under the sieve are sent to the photoelectric sorter through a conveyor belt. The selected photoelectric sorter is an ultraviolet or X-ray photoelectric sorter. The fluorescence phenomenon produced by the action of ultraviolet and X-ray light sources on pyrite is used, and the fluorescence detection sorting technology is used to classify ores with different pyrite grades. By adjusting the material conveying speed to 3 m / s, ores with different pyrite contents are sorted out, and the ores with low pyrite content enter the next step of sorting;

[0050] The hard kaolinite mineral with low pyrite content sorted by the above-mentioned photoelectric sorter is fed into an impact ultrafine powder mill with a screen through a double screw feeder for selective grinding. The difference in hardness and density between kaolinite and pyrite particles will cause the mineral to be broken into different particle sizes under the impact force. The impact ultrafine powder mill is equipped with a screen with adjustable sieve holes for two impacts and screening. By adjusting the impact hammer speed of the impact ultrafine powder mill and the speed ratio of the two-stage hammer heads, the sieve holes are adjusted at the same time to control the first-stage hammer head linear speed to 50 m / s and the first-stage screening control; the second-stage hammer head linear speed is 75 m / s and the second-stage screening control, so as to form hard kaolinite ore particles (D97) in the range of 15 μm.

[0051] The secondary screen material is sent to the classifier, which is characterized by gravity air separation. By adjusting the parameters of the air separation equipment, 25 Hz, the kaolinite particle size is controlled to be 10 μm.

[0052] The kaolinite sample was collected by using a bag dust collector to obtain a hard kaolinite sample 2 with low pyrite and low COD content. Figure 7 This is the XRD diagram of hard kaolinite sample 2. The pyrite mineral phase content is about 1.21%, and the removal rate is 46%; the COD value is 6961 mg / kg, and the removal rate is 55%. Example

[0053] Take hard kaolinite containing coarse-grained aggregates of pyrite, in which the pyrite may be in the form of oolitic or pea-shaped inclusions; select hard kaolinite samples, Figure 8 The XRD diagram of the selected hard kaolinite sample 3 shows that the pyrite mineral phase content is about 0.72%, COD is 3090 mg / kg, Fig. 9 This is an optical microscope picture of the selected hard kaolinite sample 3.

[0054] The hard kaolinite ore was added into the jaw crusher and the ore sample was crushed to a particle size (D97) < 40 mm;

[0055] The above-mentioned fine particles are sent to the next step roller crusher for secondary crushing. After being controlled by the screening machine, the particles with a particle size (D97) <10 mm enter the next step of processing, and the crushed samples of the sieve are homogenized in the warehouse before grinding; the particles above 10 mm enter the roller crusher again;

[0056] The crushed particles under the sieve are sent to the photoelectric sorter through a conveyor belt. The selected photoelectric sorter is an ultraviolet or X-ray photoelectric sorter. The fluorescence phenomenon produced by the interaction of ultraviolet and X-ray light sources with pyrite is used, and the fluorescence detection sorting technology is used to classify ores with different pyrite grades. By adjusting the material conveying speed to 5 m / s, ores with different pyrite contents are sorted out, and the ores with low pyrite content enter the next step of sorting.

[0057] The hard kaolinite mineral with low pyrite content sorted by the above-mentioned photoelectric sorter is fed into an impact ultrafine grinding mill with a screen through a double screw feeder for selective grinding. The difference in hardness and density between kaolinite and pyrite particles will cause the mineral to be broken into different particle sizes under the impact force. The impact ultrafine grinding mill is equipped with a screen with adjustable sieve holes for two impacts and screening. By adjusting the impact hammer speed of the impact ultrafine grinding mill and the speed ratio of the two-stage hammer heads, the sieve holes are adjusted at the same time to control the first-stage hammer head linear speed to 60m / s, the first-stage screening control; the second-stage hammer head linear speed is 120 m / s, the second-stage screening control, to form hard kaolinite ore particles (D97) in the range of 2 μm.

[0058] The secondary screen material is sent to the classifier, which is characterized by gravity air separation. By adjusting the parameters of the air separation equipment, 32Hz, the kaolinite particle size is controlled to 2 μm.

[0059] The kaolinite sample was collected by using a bag dust collector to obtain a hard kaolinite sample 3 with low pyrite and low COD content. Fig.10 This is the XRD diagram of hard kaolinite sample 3. The pyrite mineral phase content is about 0.31%, and the removal rate is 57%; the COD value is 1582 mg / kg, and the removal rate is 49%.

[0060] The principles and implementation methods of the present invention are described in this article using specific examples. The description of the above embodiments is only used to help understand the method and core idea of ​​the present invention. At the same time, for those skilled in the art, according to the idea of ​​the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A method for reducing the pyrite content and COD value in hard kaolinite, It is characterized in that The following steps are involved: (1) The hard kaolinite containing the coarse-grained aggregate of pyrite is crushed to obtain D 97 Particles <40 mm; (2) The pellets are crushed and screened to obtain D 97 For particles <10 mm, the material on the sieve is crushed and sieved again; (3) subjecting the undersize material in step (2) to photoelectric separation to obtain pyrite and hard kaolinite with low pyrite content; (4) subjecting hard kaolinite with low pyrite content to two-stage impact and screening; (5) The secondary screen material in step (4) is subjected to gravity air separation and collected by a bag dust collector to obtain hard kaolinite with low COD value and low pyrite content.

2. A method for reducing pyrite content and COD value in hard kaolinite according to claim 1, It is characterized in that The pyrite in the hard kaolinite is in the form of oolite or bean-shaped inclusions.

3. A method for reducing pyrite content and COD value in hard kaolinite according to claim 1, It is characterized in that The photoelectric separation is performed using a photoelectric separator, which is an ultraviolet light separator or an X-ray separator.

4. A method for reducing pyrite content and COD value in hard kaolinite according to claim 1, It is characterized in that The material conveying speed in the photoelectric sorting process is 2 m / s~5 m / s.

5. A method for reducing pyrite content and COD value in hard kaolinite according to claim 1, It is characterized in that The linear speed of the first-stage impact hammer in the two-stage impact is 50 m / s or 60 m / s, and the linear speed of the second-stage impact hammer is 75 m / s or 120 m / s.

6. A method for reducing pyrite content and COD value in hard kaolinite according to claim 1, It is characterized in that D of hard kaolinite particles after secondary screening 97 2 μm or 15 μm.

7. A method for reducing pyrite content and COD value in hard kaolinite according to claim 1, It is characterized in that The air selection frequency is 16 Hz~32 Hz.

8. A method for reducing pyrite content and COD value in hard kaolinite according to claim 1, It is characterized in that The hard kaolinite particles with low COD value and low pyrite content have a particle size of 2 μm or 10 μm.

Citation Information

Patent Citations

  • Method for recovering pyrite from coal gangue

    CN103657838A

  • Decarbonization process for coal series kaolin

    CN105642433A

  • Beneficiation method for recovering pyrites from coal gangue

    CN105665122A

  • Method for removing pyrite impurity from quartz

    CN105819454A

  • Method for raising grade of hematite by biologically reducing and magnetizing and dressing

    CN102319621A