A copper-free welding wire and its coating and preparation method
By using coatings of components such as stearate, molybdenum disulfide, colloidal graphite and titanium nitride in copper-free copper wire, the problems of complex coating process and high cost are solved, and the density of the coating is achieved. Conductivity reduces the wear of the conductive nozzle and improves welding performance.
Patent Information
- Application Number
- CN202211320835.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-26
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-10-26
AI Technical Summary
The coating process without copper-coated wire is complex and has high cost. The coating is not dense and easy to fall off, resulting in poor wire feeding and serious wear of the conductive nozzle during welding.
The coating is made of stearate, molybdenum disulfide, colloidal graphite, polytetrafluoroethylene and titanium nitride, and a dense coating is formed through mechanical shelling, rust removal and multiple drawings. Improve the conductivity and bonding strength of the welding wire and reduce the wear of the conductive nozzle.
It improves the drawing smoothness and production efficiency of welding wire, enhances the density and bonding strength of the coating, reduces the wear of the conductive nozzle, and reduces production costs.
Smart Images

Figure CN115555760B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of welding materials, and in particular to a copper-free welding wire and a coating and a preparation method thereof. Background Art
[0002] With the increasing application of non-copper-plated welding wire in the market in recent years, the current development trend is that non-copper-plated welding wire gradually replaces copper-plated welding wire. The copper plating process is omitted in the production of non-copper-plated welding wire, and the surface coating is used to replace the original copper plating layer, so that the welding wire meets the welding process requirements in terms of conductivity, rust prevention, lubrication, etc. At the same time, the non-copper-plated welding wire is energy-saving and environmentally friendly during production and use, which greatly improves the working environment. Compared with copper-plated welding wire, there are still several major problems with domestic non-copper-plated welding wire, mainly manifested in: First, the coating process of non-copper-plated welding wire is complicated and the cost is high; second, the surface coating of non-copper-plated welding wire is not dense and easy to fall off. The falling coating not only makes the wire feeding not smooth during welding, but also blocks the wire feeding system in the welding equipment during use; third, the conductive nozzle is severely worn. Summary of the invention
[0003] In view of the above shortcomings of the prior art, the present invention provides a copper-free welding wire and its coating and preparation method to improve the problems of high preparation cost of coated welding wire, loose coating and severe wear of conductive nozzle.
[0004] To achieve the above-mentioned purpose and other related purposes, the present invention provides a copper-free welding wire coating, which comprises the following components: 70-80% stearate, 10-20% molybdenum disulfide, 3-5% colloidal graphite, 1-2% polytetrafluoroethylene, and 6-10% titanium nitride.
[0005] In one example of the present invention, the stearate is any one or both of calcium stearate and sodium stearate.
[0006] In an example of the present invention, the particle size of the molybdenum disulfide is less than or equal to 0.5 μm, the particle size of the colloidal graphite is 1 to 10 μm, and the particle size of the titanium nitride is 1 to 10 μm.
[0007] The invention provides a copper-free welding wire, comprising a wire rod and a coating. The coating comprises the following components in percentage by mass: 70-80% of stearate, 10-20% of molybdenum disulfide, 3-5% of colloidal graphite, 1-2% of polytetrafluoroethylene and 6-10% of titanium nitride.
[0008] In an example of the present invention, the weight of the coating in the non-copper-plated welding wire is 0.01-0.05% of the total weight of the non-copper-plated welding wire.
[0009] In an example of the present invention, the wire rod is ER50-6 wire rod, and the diameter of the wire rod is 5.5-6.5 mm.
[0010] In an example of the present invention, the diameter of the non-copper-plated welding wire is 0.8-1.6 mm.
[0011] The invention provides a method for preparing a copper-free welding wire, comprising the following steps: providing a wire rod; uniformly mixing the above components to configure a coating; mechanically peeling the wire rod, removing rust and roughening it; applying the configured coating to the wire rod, compressing and applying the coating; and drawing the wire rod multiple times to obtain the copper-free welding wire.
[0012] In one example of the present invention, during the rust removal and roughening treatment, the wire rod is sequentially subjected to rust removal and roughening treatment using a first gauze belt and a second gauze belt, wherein the mesh number of the first gauze belt is 30 to 50, and the mesh number of the second gauze belt is 50 to 80.
[0013] In an example of the present invention, lubricating powder is applied to the surface of the welding wire during the drawing process.
[0014] The coated welding wire of the present invention can improve the smoothness of welding wire drawing, improve production efficiency and reduce costs by adding stearate and polytetrafluoroethylene to the coating; molybdenum disulfide has good metal surface adhesion, and adding molybdenum disulfide and colloidal graphite to the coating can enhance the bonding strength between the coating and the wire rod, ensuring that the coating is dense and not easy to fall off; molybdenum disulfide and colloidal graphite have good electrical conductivity and high temperature resistance, and adding molybdenum disulfide and colloidal graphite can reduce the resistance value of the welding wire surface and reduce the temperature of the conductive nozzle during welding; the addition of titanium nitride can effectively reduce the wear of the conductive nozzle. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0016] Figure 1 The present invention is a flow chart of the method for preparing copper-free welding wire. DETAILED DESCRIPTION
[0017] The following is an explanation of the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the features in the following embodiments and the embodiments can be combined with each other without conflict. It should also be understood that the terms used in the embodiments of the present invention are intended to describe specific embodiments, rather than to limit the scope of protection of the present invention. The test methods for which specific conditions are not specified in the following examples are usually carried out under conventional conditions or according to the conditions recommended by the manufacturers.
[0018] It should be noted that "%" and "wt%" in this specification represent mass percentage.
[0019] The invention provides a non-copper-plated welding wire and a coating and a preparation method thereof. The coating of the non-copper-plated welding wire is dense and not easy to fall off, and the wear of the conductive nozzle is small, so the wire has great practical value.
[0020] The copper-free welding wire coating of the present invention comprises the following components, calculated by mass percentage, of stearate 70-80%, molybdenum disulfide 10-20%, colloidal graphite 3-5%, polytetrafluoroethylene 1-2%, and titanium nitride 6-10%.
[0021] The functions of each component in the coating are as follows:
[0022] Stearate: As a lubricating carrier, it can improve the smoothness of drawing the coated welding wire, and at the same time improve the wire feeding stability and arc stability of the welding wire. The mass percentage of the stearate in the present invention is 70-80%, for example, the mass percentage of the stearate can be any value within the range of 70-80%, such as 70%, 73%, 78% or 80%. The stearate in the present invention is any one or both of calcium stearate and sodium stearate.
[0023] Molybdenum disulfide: improves electrical conductivity, reduces the surface resistance of the welding wire, and enhances the bonding strength between the coating and the welding wire substrate. The mass percentage of molybdenum disulfide in the present invention is 10-20%, for example, the mass percentage of molybdenum disulfide can be any value within the range of 10% to 20%, such as 10%, 15% or 20%.
[0024] Colloidal graphite: improves the conductivity of the coating and reduces the surface resistance of the welding wire. The mass percentage of the colloidal graphite in the present invention is 3-5%, for example, the mass percentage of the colloidal graphite can be any value within the range of 3-5%, such as 3%, 4% or 5%.
[0025] Polytetrafluoroethylene: lubrication, reducing drawing resistance and wire feeding resistance during welding. The mass percentage of polytetrafluoroethylene in the present invention is 1-2%, for example, the mass percentage of polytetrafluoroethylene can be any value within the range of 1-2%, such as 1%, 1.5% or 2%.
[0026] Titanium nitride: improves the conductivity of the coating and reduces the wear of the conductive nozzle. The mass percentage of titanium nitride in the present invention is 6-10%, for example, the mass percentage of titanium nitride can be any value within the range of 6-10%, such as 6%, 7.5%, 9% or 10%.
[0027] In one embodiment, the particle size of molybdenum disulfide is less than or equal to 0.5 μm, the particle size of colloidal graphite is 1 to 10 μm, and the particle size of titanium nitride is 1 to 10 μm. For example, the particle size of colloidal graphite can be any value within the range of 1 to 10 μm, such as 1 μm, 5 μm, 8 μm or 10 μm; the particle size of titanium nitride can be any value within the range of 1 to 10 μm, such as 1 μm, 3 μm, 8 μm, 10 μm, etc.
[0028] The copper-free welding wire of the invention comprises a wire rod and a coating, wherein the coating comprises the following components: 70-80% of stearate, 10-20% of molybdenum disulfide, 3-5% of colloidal graphite, 1-2% of polytetrafluoroethylene and 6-10% of titanium nitride.
[0029] In one embodiment, the coating rate of the coating in the coated welding wire, that is, the weight of the coating, is 0.01-0.05% of the total weight of the coated welding wire. For example, the coating rate can be any value within the range of 0.01-0.05%, such as 0.01%, 0.02%, 0.04%, 0.05%, etc.
[0030] In one embodiment, the wire rod of the coated welding wire is ER50-6 wire rod, and the diameter of the wire rod is 5.5-6.5 mm. For example, the diameter of the wire rod can be any value within the range of 5.5-6.5 mm, such as 5.5 mm, 6 mm or 6.5 mm.
[0031] In one embodiment, the diameter of the coated welding wire is 0.8-1.6 mm. For example, the diameter of the coated welding wire can be any value within the range of 0.8-1.6 mm, such as 0.8 mm, 1.1 mm, 1.3 mm or 1.6 mm.
[0032] See also Figure 1 The present invention provides a method for preparing a copper-free welding wire, comprising the following steps:
[0033] S1. Provide a wire rod;
[0034] S2, mixing the components of the coating evenly according to the above proportions;
[0035] S3, mechanically peeling the wire rod, removing rust and roughening it;
[0036] S4, applying the prepared coating to the wire rod, and compressing the coating;
[0037] S5. Drawing multiple times to obtain copper-free welding wire.
[0038] Wherein, in step S1, the wire rod is ER50-6 wire rod, and the diameter of the wire rod is 5.5-6.5 mm. For example, the diameter of the wire rod can be any value within the range of 5.5-6.5 mm, such as 5.5 mm, 6 mm or 6.5 mm.
[0039] In step S2, the components in the coating are mixed and stirred uniformly according to the following proportions: 70-80% stearate, 10-20% molybdenum disulfide, 3-5% colloidal graphite, 1-2% polytetrafluoroethylene, and 6-10% titanium nitride.
[0040] In step S3, the wire rod is first mechanically shelled, and then the shelled wire rod is rust-removed and roughened. During the roughening treatment, the wire rod is treated with a first gauze belt and a second gauze belt in sequence, the mesh number of the first gauze belt is 30 to 50 meshes, and the mesh number of the second gauze belt is 50 to 80 meshes. For example, the mesh number of the first gauze belt can be any value within the range of 30 to 50 meshes, such as 30 meshes, 40 meshes or 50 meshes, and the second gauze belt can be any value within the range of 50 to 80 meshes, such as 50 meshes, 60 meshes, 70 meshes or 80 meshes. Roughening the wire rod can increase the roughness of the wire rod, enhance the bonding strength between the coating and the wire rod, and ensure that the coating is dense and not easy to fall off.
[0041] In step S4, the configured coating is applied to the surface of the wire rod, and the wire rod coated with the coating is placed in a mold and drawn. During the drawing process, the coating is squeezed firmly on the surface of the wire rod.
[0042] In step S5, lubricating powder can be used during the drawing process to increase the lubricity and make the drawing smoother.
[0043] The method for preparing a copper-free welding wire provided by the present invention is to apply a coating on the surface of a wire rod before the first drawing, and then draw the wire rod, and then apply lubricating powder to the wire rod coated with the coating when drawing to improve the smoothness of drawing. Because molybdenum disulfide, colloidal graphite and other ingredients are added to the coating, the coating can form a dense and uniform film on the surface of the wire rod, isolating the wire rod from the lubricating powder, and the lubricating powder can be easily wiped off after the drawing is completed, ensuring that the surface of the welding wire coating is smooth, dense, and has a low shedding rate.
[0044] The present invention is described in detail below through some specific examples. The drugs used in the following examples can all be obtained through common commercial means.
[0045] Example 1
[0046] The copper-free welding wire of this embodiment includes a wire rod and a coating coated on the surface of the wire rod, wherein the coating includes the following components by mass percentage: 70% calcium stearate, 20% molybdenum disulfide, 3% colloidal graphite, 1% polytetrafluoroethylene, and 6% titanium nitride. The wire rod is a 6.5 mm ER50-6 wire rod, and the wire rod is roughened with a first gauze tape of 30 mesh and a second gauze tape of 50 mesh in sequence, and then the coating is mixed and evenly coated on the surface of the wire rod, and the coating is compressed and applied, and the welding wire is obtained after multiple drawing. The coating coating rate is 0.049%, and the diameter of the welding wire is 1.6 mm.
[0047] Example 2
[0048] The copper-free welding wire of this embodiment includes a wire rod and a coating coated on the surface of the wire rod, wherein the coating includes the following components by mass percentage: 80% sodium stearate, 10% molybdenum disulfide, 3% colloidal graphite, 1% polytetrafluoroethylene, and 6% titanium nitride. The wire rod is a 6.5 mm ER50-6 wire rod, and the wire rod is roughened with a first gauze tape of 40 mesh and a second gauze tape of 60 mesh in sequence, and then the coating is mixed and evenly coated on the surface of the wire rod, and the coating is compressed and applied, and the welding wire is obtained after multiple drawing. The coating coating rate is 0.035%, and the diameter of the welding wire is 1.2 mm.
[0049] Example 3
[0050] The copper-free welding wire of this embodiment includes a wire rod and a coating coated on the surface of the wire rod, wherein the coating includes the following components by mass percentage: 75% stearate (including 15% calcium stearate and 60% sodium stearate), 15% molybdenum disulfide, 3% colloidal graphite, 1% polytetrafluoroethylene, and 6% titanium nitride. The wire rod is a 6.5mm ER50-6 wire rod, which is roughened with a first gauze tape of 50 mesh and a second gauze tape of 80 mesh in sequence, and then the coating is mixed and evenly coated on the surface of the wire rod, and the coating is compressed and applied, and the welding wire is obtained after multiple drawing. The coating coating rate is 0.021%, and the diameter of the welding wire is 1.2mm.
[0051] Example 4
[0052] The copper-free welding wire of this embodiment includes a wire rod and a coating coated on the surface of the wire rod, wherein the coating includes the following components by mass percentage: 70% stearate (including 10% calcium stearate and 60% sodium stearate), 14% molybdenum disulfide, 5% colloidal graphite, 1% polytetrafluoroethylene, and 10% titanium nitride. The wire rod is a 6.5mm ER50-6 wire rod, and the wire rod is roughened with a first gauze tape of 50 mesh and a second gauze tape of 70 mesh in sequence, and then the coating is mixed and evenly coated on the surface of the wire rod, and the coating is compressed and applied, and the welding wire is obtained after multiple drawing. The coating coating rate is 0.022%, and the diameter of the welding wire is 1.2mm.
[0053] Example 5
[0054] The copper-free welding wire of this embodiment includes a wire rod and a coating coated on the surface of the wire rod, wherein the coating includes the following components by mass percentage: 70% stearate (including 20% calcium stearate and 50% sodium stearate), 18% molybdenum disulfide, 4% colloidal graphite, 2% polytetrafluoroethylene, and 6% titanium nitride. The wire rod is a 6.5mm ER50-6 wire rod, and the wire rod is roughened with a first gauze tape of 40 mesh and a second gauze tape of 80 mesh in sequence, and then the coating is mixed and evenly coated on the surface of the wire rod, and the coating is compressed and applied, and the welding wire is obtained after multiple drawing. The coating coating rate is 0.048%, and the diameter of the welding wire is 1.2mm.
[0055] Example 6
[0056] The copper-free welding wire of this embodiment includes a wire rod and a coating coated on the surface of the wire rod, wherein the coating includes the following components by mass percentage: 75% stearate (including 20% calcium stearate and 55% sodium stearate), 11% molybdenum disulfide, 4% colloidal graphite, 2% polytetrafluoroethylene, and 8% titanium nitride. The wire rod is a 5.5mm ER50-6 wire rod, and the wire rod is roughened with a first gauze tape of 50 mesh and a second gauze tape of 80 mesh in sequence, and then the coating is mixed and evenly coated on the surface of the wire rod, and the coating is compressed and applied, and the welding wire is obtained after multiple drawing. The coating coating rate is 0.01%, and the diameter of the welding wire is 0.8mm.
[0057] Example 7
[0058] The copper-free welding wire of this embodiment includes a wire rod and a coating coated on the surface of the wire rod, wherein the coating includes the following components by mass percentage: 72% stearate (including 36% calcium stearate and 36% sodium stearate), 14% molybdenum disulfide, 4% colloidal graphite, 2% polytetrafluoroethylene, and 8% titanium nitride. The wire rod is a 5.5mm ER50-6 wire rod, and the wire rod is roughened with a first gauze tape of 40 mesh and a second gauze tape of 80 mesh in sequence, and then the coating is mixed and evenly coated on the surface of the wire rod, and the coating is compressed and applied, and the welding wire is obtained after multiple drawing. The coating coating rate is 0.015%, and the diameter of the welding wire is 1.0mm.
[0059] Various welding tests were conducted on the copper-free welding wires of the above-mentioned embodiments 1 to 7 according to relevant standards and specifications. The welding process parameters are shown in Table 1 below, and the welding performance is shown in Table 2 below.
[0060] Table 1 Welding process parameters
[0061]
[0062] Table 2 Welding process performance
[0063]
[0064] The test results of Examples 1 to 7 show that the copper-free welding wire of the present invention has a lower wear rate of the conductive nozzle during welding, good wire feedability and arc stability, and its comprehensive performance is better than that of commercially available copper-free welding wire and copper-coated welding wire.
[0065] The copper-free welding wire of the present invention can improve the smoothness of wire drawing and improve production efficiency by adding stearate and polytetrafluoroethylene to the coating; molybdenum disulfide has good metal surface adhesion, and adding molybdenum disulfide and colloidal graphite to the coating can enhance the bonding strength between the coating and the wire rod, ensuring that the coating is dense and not easy to fall off; molybdenum disulfide and colloidal graphite have good electrical conductivity and high temperature resistance, and adding molybdenum disulfide and colloidal graphite can reduce the resistance value of the welding wire surface and reduce the temperature of the conductive nozzle during welding; the addition of titanium nitride can effectively reduce the wear of the conductive nozzle; and the preparation process is simple, which can greatly reduce the cost and is conducive to industrial production. Therefore, the present invention effectively overcomes some practical problems in the prior art and has high utilization value and use significance.
[0066] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A copper-free welding wire coating, characterized in that: Calculated by mass percentage of the coating, the coating consists of the following components: 70-80% stearate, 10-20% molybdenum disulfide, 3-5% colloidal graphite, 1-2% polytetrafluoroethylene, and 6-10% titanium nitride.
2. The copper-free welding wire coating according to claim 1, characterized in that: The stearate is any one or both of calcium stearate and sodium stearate.
3. The copper-free welding wire coating according to claim 1, characterized in that: The particle size of the molybdenum disulfide is less than or equal to 0.5 μm, the particle size of the colloidal graphite is 1 to 10 μm, and the particle size of the titanium nitride is 1 to 10 μm.
4. A copper-free welding wire, characterized in that: The invention comprises a wire rod and a coating. The coating is composed of the following components in terms of mass percentage: 70-80% of stearate, 10-20% of molybdenum disulfide, 3-5% of colloidal graphite, 1-2% of polytetrafluoroethylene and 6-10% of titanium nitride.
5. The copper-free welding wire according to claim 4, characterized in that: The weight of the coating in the copper-free welding wire is 0.01-0.05% of the total weight of the copper-free welding wire.
6. The copper-free welding wire according to claim 4, characterized in that: The wire rod is ER50-6 wire rod, and the diameter of the wire rod is 5.5~6.5mm.
7. The copper-free welding wire according to claim 4, characterized in that: The diameter of the non-copper-plated welding wire is 0.8-1.6 mm.
8. A method for preparing a copper-free welding wire, characterized in that: The steps include: Provide a coil; The components according to claim 1 are mixed uniformly to prepare a coating; The wire rod is mechanically shelled, rust-removed and roughened; applying the configured coating onto the wire rod, compressing the coating; The copper-free welding wire is obtained by multiple drawing.
9. The method for preparing a copper-free welding wire according to claim 8, characterized in that: During the rust removal and roughening treatment, the wire rod is subjected to rust removal and roughening treatment using a first gauze belt and a second gauze belt in sequence, wherein the mesh number of the first gauze belt is 30-50 meshes, and the mesh number of the second gauze belt is 50-80 meshes.
10. The method for preparing a copper-free welding wire according to claim 8, characterized in that: Lubricating powder is applied to the surface of the welding wire during the drawing process.
Citation Information
Patent Citations
Feeding lubricant for cored welding electrode, cored welding electrode and gmaw process
CN102844149A
Copper-plated-free ER50-6 gas-shielded solid welding wire
CN108941979A
Anti-corrosion hydraulic vulcanizing machine
CN109836855A
Nano-coating welding wire without copper plating and processing technology thereof
CN114769944A
Anti-corrosion and / or anti-scaling coating for metals (especially steel) is applied by wet methods and heat treated to give a weldable coating
DE102005059614A1