An electrochromic functional layer and an electrochromic device containing the same

By using a synergistic effect of single-core metal complexes with ionic conductors and counter electrode materials in electrochromic devices, the problem of insufficient color variation and stability of existing electrochromic materials is solved, and the electrochromic devices are realized Colorful, controllable color conversion and high stability, suitable for applications such as color-changing glass.

CN115557994BActive Publication Date: 2024-12-03FUYAO GLASS IND GROUP CO LTD
View PDF 0 Cites -1 Cited by

Patent Information

Application Number
CN202211207526.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-30
Publication Date
2024-12-03
Estimated Expiration
2042-09-30

AI Technical Summary

Technical Problem

The existing electrochromic materials lack diversity in color changes, and the cycle reversibility and stability in electrochromic devices are poor, making it difficult to achieve colorful and controllable color conversion.

Method used

Using single-core metal complex as electrochromic material, the electrochromic functional layer is formed through synergistic effects with ionic conductors and counter electrode materials, and the color change effect is achieved, and the material is improved through specific preparation methods and structural optimization. Stability and electrochromic properties.

Benefits of technology

The reversible and controllable conversion between "transparent light-colored state" and "dark blue tint state" is achieved, which improves the cyclic reversibility and stability of electrochromic devices, and has broad application prospects in fields such as color-changing glass.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115557994B_ABST
    Figure CN115557994B_ABST
Patent Text Reader

Abstract

The present invention provides an electrochromic functional layer and an electrochromic device comprising the same, wherein the electrochromic functional layer contains an electrochromic material; the electrochromic material is a mononuclear metal complex, and its general structural formula is: [M(A)(X1)(X2)]; wherein M is selected from manganese, cobalt, nickel, zinc, copper, iron or ruthenium; X1 and X2 are independently selected from F, Cl, Br, I, or PF6; the structure of A is shown in Formula I: #imgabs0# R1 and R2 are independently selected from saturated hydrocarbon groups, unsaturated hydrocarbon groups, aromatic groups or heteroatom-containing groups. The electrochromic device can achieve a multi-color effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of electrochromism, and in particular relates to an electrochromic functional layer and an electrochromic device comprising the same. Background Art

[0002] Electrochromism (EC for short) refers to the phenomenon that the optical properties (reflectivity, transmittance, absorptivity, etc.) of materials undergo reversible changes under the action of an external electric field. There are many types of such materials, and metal complexes are one of them. Metal complexes are a type of inorganic-organic hybrid compounds formed by coordination bonds between metals and ligands. When they are combined with ion conductors and counter electrode materials with complementary electrode potentials, they can be made into electrochromic functional layers. Add a conductive layer and a transparent substrate layer to assemble an electrochromic device. When connected to an external power supply, the device can achieve colorful color changes. If such electrochromic devices are applied to vehicle glass, they can be used for dimming, display, atmosphere and other products. Summary of the invention

[0003] The object of the present invention is to provide an electrochromic functional layer and an electrochromic device comprising the same, wherein the electrochromic functional layer can achieve a multi-color effect through a synergistic effect on electrode materials.

[0004] In order to achieve the above object, the present invention provides an electrochromic functional layer, which contains an electrochromic material, wherein the electrochromic material is a mononuclear metal complex;

[0005] The general structural formula of the mononuclear metal complex is: [M(A)(X1)(X2)];

[0006] wherein M is selected from manganese, cobalt, nickel, zinc, copper, iron or ruthenium;

[0007] X1, X2 are each independently selected from F, Cl, Br, I or PF6;

[0008] A is a bipyridine ligand, and its structure is shown in Formula I:

[0009]

[0010] R1 and R2 are each independently selected from a saturated hydrocarbon group, an unsaturated hydrocarbon group, an aromatic group or a heteroatom-containing group.

[0011] According to a specific embodiment of the present invention, preferably, the structure of the mononuclear metal complex is as shown in Formula II:

[0012]

[0013] In formula II, the spatial positions of X1 and X2 are not particularly limited, and the dotted bonds and bold black bonds are used only to distinguish the relative positions of X1 and X2 in the complex structure.

[0014] According to a specific embodiment of the present invention, preferably, the electrochromic material is a crystal of the mononuclear metal complex.

[0015] According to a specific embodiment of the present invention, preferably, R1 and R2 are each independently selected from a saturated hydrocarbon group or an aromatic group.

[0016] According to a specific embodiment of the present invention, preferably, the saturated hydrocarbon group is a straight chain alkyl group or a branched chain alkyl group having a carbon number of 1 to 20. More preferably, the saturated hydrocarbon group is a methyl group, an ethyl group, a n-butyl group, a tert-butyl group, a n-heptyl group, a tert-octyl group or a n-tridecyl group.

[0017] According to a specific embodiment of the present invention, preferably, the aryl group is a monocyclic or polycyclic aromatic group having a carbon number of 6 to 20. More preferably, the aryl group is a phenyl group or a naphthyl group.

[0018] According to a specific embodiment of the present invention, preferably, the unsaturated hydrocarbon group is a straight chain unsaturated hydrocarbon group or a branched chain unsaturated hydrocarbon group having a carbon number of 1 to 20. More preferably, the unsaturated hydrocarbon group is an allyl group.

[0019] According to a specific embodiment of the present invention, preferably, the heteroatom-containing group is a functional group containing N, O, S, Si or P. More preferably, the heteroatom-containing group is an ester group, an ether bond, an amide group or a conjugated group containing a heteroatom.

[0020] According to a specific embodiment of the present invention, preferably, R1 and R2 are each independently selected from methyl, n-butyl, n-tridecyl or phenyl.

[0021] According to a specific embodiment of the present invention, preferably, the M is selected from manganese, cobalt, nickel or zinc; and the X1 and X2 are each independently selected from Cl or Br.

[0022] According to a specific embodiment of the present invention, preferably, the electrochromic material is selected from one of the following structures:

[0023]

[0024] According to a specific embodiment of the present invention, preferably, the method for preparing the above-mentioned mononuclear metal complex or its crystal comprises the following steps: reacting ligand A and metal salt MX1X2 in an organic solvent to obtain the mononuclear metal complex or its crystal.

[0025] According to a specific embodiment of the present invention, preferably, in the above preparation method, the organic solvent is one or a combination of two or more of nitriles, alcohols and halogenated hydrocarbons, such as acetonitrile or methanol.

[0026] According to a specific embodiment of the present invention, preferably, in the above preparation method, the molar ratio of MX1X2 to A is 0.9-1.1:1.0-2.0, more preferably 1:1.

[0027] According to a specific embodiment of the present invention, preferably, in the above preparation method, the reaction is carried out at 25-100°C, more preferably 80-85°C; and the reaction time is 2-6h.

[0028] According to a specific embodiment of the present invention, preferably, in the above preparation method, a recrystallization purification step is further included after the reaction is completed.

[0029] According to a specific embodiment of the present invention, the above-mentioned mononuclear metal complex crystal belongs to the orthorhombic system. Taking [Mn((CH3)2NPhN(CH2py)2)Cl2] crystal as an example, the space group is P212121, and the unit cell parameters are α=β=γ=90°, z=4.

[0030] According to a specific embodiment of the present invention, preferably, the electrochromic functional layer further comprises an ion conductor and a counter electrode material, wherein the ion conductor is used to transport ions.

[0031] According to a specific embodiment of the present invention, preferably, the ion conductor is a fluid state ion conductor or a gel state ion conductor.

[0032] According to a specific embodiment of the present invention, preferably, the fluidic ion conductor comprises a salt and a solvent.

[0033] According to a specific embodiment of the present invention, preferably, the gel-state ion conductor comprises a polyacrylate compound containing hydroxyl groups or primary amino groups, a salt and a solvent.

[0034] According to a specific embodiment of the present invention, preferably, in the fluidized ion conductor and the gel ion conductor, the salt is an organic salt or an inorganic salt, more preferably one or a combination of two or more of an ionic liquid, a tetrabutylammonium salt, a hexafluorophosphate, a lithium bis(trifluorosulfonyl)imide and a lithium bis(trifluoromethanesulfonyl)imide.

[0035] According to a specific embodiment of the present invention, preferably, in the fluidized ion conductor and the gelled ion conductor, the concentration of the salt in the solvent is 0.1 mol / L to 3 mol / L.

[0036] According to a specific embodiment of the present invention, preferably, in the fluidized ion conductor and the gelled ion conductor, the solvent is one or a combination of two of an ionic liquid and an organic solvent.

[0037] According to a specific embodiment of the present invention, preferably, in the solvent involved in the above-mentioned ion conductor, the ionic liquid is 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt or pyrrole salt ionic liquid, and the organic solvent is propylene carbonate and / or N-methylpyrrolidone.

[0038] According to a specific embodiment of the present invention, preferably, the polyacrylate compound containing hydroxyl or primary amino group is obtained by polymerizing the acrylic ester compound containing hydroxyl or primary amino group under the action of an initiator, and can be used directly; the obtained system can also be further cross-linked and cured by heating; the system can also be covalently cross-linked by adding a cross-linking agent to the monomer; in some special application scenarios, a heat stabilizer or a light stabilizer can be added to the system to reduce the damage to the material by heat and light; the initiator is a thermal initiator and / or a photoinitiator.

[0039] According to a specific embodiment of the present invention, preferably, the thermal initiator is dibenzoyl peroxide and / or an azo compound.

[0040] According to a specific embodiment of the present invention, preferably, the photoinitiator is an acylphosphine oxide, a benzophenone derivative, an oxime ester photoinitiator, a benzoylformate, an azo compound or an α-hydroxyketone derivative.

[0041] According to a specific embodiment of the present invention, preferably, the ion conductor is a gel ion conductor, the weight of the mixture formed by the solvent and the salt accounts for 30% to 80% of the weight of the gel ion conductor, and the weight of the polyacrylate compound containing hydroxyl groups or primary amino groups accounts for 20% to 70% of the weight of the gel ion conductor.

[0042] In the present invention, the counter electrode material is a material that can match the redox potential of the electrochromic material in the electrochromic device, compensate for the gain / loss of electrons by the electrochromic material, and improve the cyclic reversibility of the electrochromic device. If the electrochromic material is used as a cathode in the device, this counter electrode material can be used as an anode; if the electrochromic material is used as an anode in the device, this counter electrode material can be used as a cathode. If this counter electrode material has electrochromic properties, it is not limited to only one type in the device, and can be a plurality of different materials, which can synergize with the electrochromic material in the device, and two or even more colors can be superimposed to adjust the overall color of the device, which is the key to the device to achieve colorful changes. According to a specific embodiment of the present invention, preferably, the counter electrode material is an electrochromic material or a non-electrochromic material.

[0043] According to a specific embodiment of the present invention, preferably, the counter electrode material is a substance with weaker oxidizing property than the electrochromic material, such as N,N'-diethyl-4,4'-bipyridinium salt.

[0044] The present invention also provides an electrochromic device, which comprises a transparent substrate layer, a conductive layer, an electrochromic functional layer, a conductive layer, and a transparent substrate layer stacked in sequence; wherein the electrochromic functional layer is the above-mentioned electrochromic functional layer.

[0045] According to a specific embodiment of the present invention, preferably, the electrochromic material, ion conductor and counter electrode material in the electrochromic functional layer are independently stacked in the electrochromic device, or a combination of any two or more of the three are mixed in the electrochromic device.

[0046] Compared with the prior art, the present invention has the following advantages:

[0047] Metal complexes, as a type of inorganic-organic hybrid compounds formed by coordination bonds between metals and ligands, have the advantages of inorganic stability and electrochemical reversibility, as well as the advantages of colorful color changes of organics, sensitive electrochromic response, good film-forming properties, and low driving voltage. As a new type of electrochromic material, it is expected to overcome the inherent disadvantages of traditional inorganic and organic electrochromic materials, and provide a unique development path for the large-scale and low-cost application of electrochromic technology. In view of this, the present invention provides an electrochromic functional layer, which comprises an electrochromic material of a mononuclear metal complex, has good photothermal stability and excellent electrochromic performance, and has broad application prospects in the fields of electrochromic glass. Specifically:

[0048] 1) The mononuclear metal complex contained in the electrochromic functional layer of the present invention has excellent stability.

[0049] 2) The mononuclear metal complex contained in the electrochromic functional layer of the present invention has obvious electrochromic properties and can achieve reversible and controllable conversion between a "transparent light-colored state" and a "dark blue colored state", and thus has great application prospects in the fields of color-changing glass;

[0050] 3) The electrochromic device of the present invention can achieve the effect of reversible color change. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 is the X-ray single crystal diffraction pattern of the electrochromic material;

[0052] Figure 2 is a thermogravimetric curve of the electrochromic material;

[0053] Figure 3This is a diagram of the color change behavior of the electrochromic device at a voltage of 1.1V. DETAILED DESCRIPTION

[0054] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.

[0055] The “-”, dotted bond or bold black bond in the chemical formula involved in the present invention only indicates the connection between groups and does not specifically refer to a single bond. For example, the connection relationship between the groups can be a single bond connection, a coordination connection, etc., or a combination of a single bond connection and a coordination connection, etc.

[0056] Preparation Example 1

[0057] This preparation example provides an electrochromic material [Mn((CH3)2NPhN(CH2py)2)Cl2], which is prepared by the following steps:

[0058] (1) Ligand preparation:

[0059] Under N2 atmosphere, 4-amino-N,N-dimethylaniline (3.01 g, 22.11 mmol) was dissolved in 200 ml of redistilled methanol, pyridine-2-carboxaldehyde (9.64 g, 90.01 mmol) was added, and then acetic acid (6.91 g, 115.08 mmol) was added to form a brown-green solution. The mixture was stirred overnight at room temperature, and NaBH3CN (1.42 g, 22.63 mmol) was added for reduction. The mixture was reacted for 5 hours, and a saturated aqueous sodium bicarbonate solution was added for neutralization. The mixture was extracted with dichloromethane, and column chromatography was selected for purification. The developing solvent was ethyl acetate and petroleum ether in a ratio of 3:1 (EA:PE=3:1). The mixture was further purified by recrystallization to obtain the ligand (CH3)2NPhN(CH2py)2.

[0060] 1 H NMR (400MHz,CDCl3):δ=8.56(s,2H),7.61(dt,2H),7.31(d,2H),7.15(dd,2H),6.75~6.63(m,4H,benzene ring hydrogen),4.76(s,4H,-CH2),2.80(s,6H,-CH3);

[0061] (2) Preparation of electrochromic material: Under nitrogen atmosphere, MnCl2 (272.1 mg, 2.16 mmol) and ligand (CH3)2NPhN(CH2py)2 (643.9 mg, 2.02 mmol) were added to a mixed solution of 30 ml of acetonitrile and 5 ml of methanol. The reaction mixture was heated to 82°C and allowed to react for 4 h before being cooled. The reaction mixture was left uncovered in a fume hood to obtain pale yellow crystals through natural evaporation of the solvent. The yield was 73%.

[0062] Elemental analysis (C 20 H 22 Calculated for Cl2MnN4: N, 12.61; C, 54.07; H, 4.99. Measured: N, 12.69; C, 53.38; H, 5.00.

[0063] High resolution mass spectrum m / z: 408.0897 [M-Cl] + .

[0064] The product was characterized by X-ray single crystal diffraction and the specific results are shown in Table 1.

[0065] The data in Table 1 show that the target product [Mn((CH3)2NPhN(CH2py)2)Cl2] was obtained in this preparation example. Figure 1 shown.

[0066] Table 1 Crystallographic parameters of [Mn((CH3)2NPhN(CH2py)2)Cl2]

[0067]

[0068] Figure 2 The thermogravimetric curve of the mononuclear metal complex prepared in Example 1 is shown in FIG. Figure 2 It can be seen that the mononuclear metal complex has excellent thermal stability, and its decomposition temperature is about 290°C in an air or nitrogen atmosphere.

[0069] Preparation Example 2

[0070] This preparation example provides an electrochromic material [Co((CH3)2NPhN(CH2py)2)Cl2], which is prepared by the following steps:

[0071] (1) Preparation of ligand: the same as the preparation of ligand in Preparation Example 1;

[0072] (2) Preparation of electrochromic material: CoCl2 (83.0 mg, 0.64 mmol) and ligand (CH3)2NPhN(CH2py)2 (216.5 mg, 0.68 mmol) were added to 10 ml of acetonitrile under nitrogen atmosphere, and the reaction mixture was heated to 82°C and allowed to react for 4 hours before cooling down. The reaction mixture was left open in a fume hood, and blue-purple crystals were obtained through natural evaporation of the solvent, with a yield of 68%.

[0073] Elemental analysis (C 20 H 22 Calculated for Cl2CoN4: N, 12.50; C, 53.59; H, 4.95. Measured: N, 12.56; C, 53.02; H, 5.01.

[0074] High resolution mass spectrum m / z: 412.0854 [M-Cl] + .

[0075] The product was characterized by X-ray single crystal diffraction and the specific results are shown in Table 2.

[0076] Table 2 Crystallographic parameters of [Co((CH3)2NPhN(CH2py)2)Cl2]

[0077]

[0078] The above data show that the target product [Co((CH3)2NPhN(CH2py)2)Cl2] was obtained in this preparation example.

[0079] Preparation Example 3

[0080] This preparation example provides an electrochromic material [Ni((CH3)2NPhN(CH2py)2)Cl2], which is prepared by the following steps:

[0081] (1) Preparation of ligand: the same as the preparation of ligand in Preparation Example 1;

[0082] (2) Preparation of electrochromic material: Under nitrogen atmosphere, NiCl2·6H2O (227.1 mg, 0.96 mmol) and ligand (CH3)2NPhN(CH2py)2 (302.6 mg, 0.95 mmol) were added to 10 ml of acetonitrile. The reaction mixture was heated to 82°C and allowed to react for 4 h before cooling. The reaction mixture was left uncovered in a fume hood and the solvent evaporated naturally to give a green crystalline product with a yield of 75%.

[0083] Elemental analysis (C 20 H 22Calculated for Cl2NiN4: N, 12.51; C, 53.62; H, 4.95. Measured: N, 12.67; C, 54.04; H, 4.90.

[0084] High resolution mass spectrum m / z: 411.0879 [M-Cl] + .

[0085] The product was characterized by X-ray single crystal diffraction and the specific results are shown in Table 3.

[0086] Table 3 Crystallographic parameters of [Ni((CH3)2NPhN(CH2py)2)Cl2]

[0087]

[0088] The above data show that the target product [Ni((CH3)2NPhN(CH2py)2)Cl2] was obtained in this preparation example.

[0089] Preparation Example 4

[0090] This preparation example provides an electrochromic material [Zn((CH3)2NPhN(CH2py)2)Cl2], which is prepared by the following steps:

[0091] (1) Preparation of ligand: the same as the preparation of ligand in Preparation Example 1;

[0092] (2) Preparation of electrochromic material: Under nitrogen atmosphere, ZnCl2 (292.2 mg, 2.14 mmol) and ligand (CH3)2NPhN(CH2py)2 (682.6 mg, 2.14 mmol) were added to 10 ml of acetonitrile. The reaction mixture was heated to 82°C and allowed to react for 4 h before cooling. The reaction mixture was left uncovered in a fume hood and the solvent evaporated naturally to give a pale yellow crystalline product with a yield of 78%.

[0093] Elemental analysis (C 20 H 22 Calculated for Cl2ZnN4: N, 12.32; C, 52.83; H, 4.88. Measured: N, 12.49; C, 53.18; H, 4.92.

[0094] High resolution mass spectrum m / z:417.0798[M-Cl] + .

[0095] The product was characterized by X-ray single crystal diffraction and the specific results are shown in Table 4.

[0096] Table 4 Crystallographic parameters of [Zn((CH3)2NPhN(CH2py)2)Cl2]

[0097]

[0098] The above data show that the target product [Zn((CH3)2NPhN(CH2py)2)Cl2] was obtained in this preparation example.

[0099] Preparation Example 5

[0100] This preparation example provides an electrochromic material [Mn((CH3)2NPhN(CH2py)2)Br2], which is prepared by the following steps:

[0101] (1) Preparation of ligand: the same as the preparation of ligand in Preparation Example 1;

[0102] (2) Preparation of electrochromic material: Under nitrogen atmosphere, MnBr2 (266.3 mg, 1.24 mmol) and ligand (CH3)2NPhN(CH2py)2 (382.0 mg, 1.20 mmol) were added to 20 ml of acetonitrile, and the reaction mixture was heated to 82°C, reacted for 4 hours, and then cooled. The reaction mixture was placed in a fume hood with an open mouth, and light yellow crystals were obtained through natural evaporation of the solvent, with a yield of 81%.

[0103] Elemental analysis (C 20 H 22 Br2MnN4) calculated values: N, 10.51; C, 45.05; H, 4.16. Measured values: N, 10.60; C, 45.31; H, 4.19.

[0104] High resolution mass spectrum m / z: 532.0352 [M+H] + .

[0105] The product was characterized by X-ray single crystal diffraction and the specific results are shown in Table 5.

[0106] Table 5 Crystallographic parameters of [Mn((CH3)2NPhN(CH2py)2)Br2]

[0107]

[0108] The above data show that the target product [Mn((CH3)2NPhN(CH2py)2)Br2] was obtained in this preparation example.

[0109] Preparation Example 6

[0110] This preparation example provides an electrochromic material [Mn((Ph)2NPhN(CH2py)2)Cl2], which is prepared by the following steps:

[0111] (1) Ligand preparation;

[0112] (2) Preparation of electrochromic material: Under nitrogen atmosphere, MnCl2 (157.2 mg, 1.25 mmol) and ligand (Ph)2NPhN(CH2py)2 (558.7 mg, 1.26 mmol) were added to 20 ml of acetonitrile, and the reaction mixture was heated to 82°C, reacted for 4 hours, and then cooled. The reaction mixture was placed in a fume hood with an open mouth, and light yellow crystals were obtained through natural evaporation of the solvent, with a yield of 73%.

[0113] Elemental analysis (C 30 H 26 Calculated for Cl2MnN4: N, 9.86; C, 55.07; H, 5.14. Measured: N, 9.95; C, 55.31; H, 5.10.

[0114] The product was characterized by X-ray single crystal diffraction and the specific results are shown in Table 6.

[0115] Table 6 Crystallographic parameters of [Mn((Ph)2NPhN(CH2py)2)Cl2]

[0116]

[0117] The above data show that the target product [Mn((Ph)2NPhN(CH2py)2)Cl2] was obtained in this preparation example.

[0118] Preparation Example 7

[0119] This preparation example provides an electrochromic material [Mn((C4H9)2NPhN(CH2py)2)Cl2], which is prepared by the following steps:

[0120] (1) Ligand preparation:

[0121] Under N2 atmosphere, 4-amino-N,N-di-n-butylaniline (1.21 g, 5.52 mmol) was dissolved in 100 ml of redistilled acetonitrile, 2-chloromethylpyridine hydrochloride (2.72 g, 16.58 mmol) was added, followed by ethyl diisopropylamine (10 mL) and catalyst equivalent of KI, and stirred at room temperature overnight. After the reaction was completed, ethyl acetate was used for extraction, and column chromatography was selected for purification, with ethyl acetate as the developing solvent, to obtain the ligand (C4H9)2NPhN(CH2py)2;

[0122] 1H NMR (400MHz, CDCl3): δ = 8.57 (s, 2H), 7.60 (t, 2H), 7.35 (d, 2H), 7.15 (dd, 2H), 6.63 (d ,2H), 6.58(d,2H),4.73(s,4H),3.12(t,4H),1.47(m,4H),1.30(m,4H),0.90(t,6H);

[0123] (2) Preparation of electrochromic material: Under nitrogen atmosphere, MnCl2 (145.6 mg, 1.16 mmol) and ligand (C4H9)2NPhN(CH2py)2 (470.3 mg, 1.17 mmol) were added to 20 ml of acetonitrile, and the reaction mixture was heated to 82°C, reacted for 4 hours, and then cooled. The reaction mixture was placed in a fume hood with an open mouth, and light yellow crystals were obtained through natural evaporation of the solvent, with a yield of 73%.

[0124] Elemental analysis (C 26 H 34 Calculated for Cl2MnN4: N, 10.60; C, 59.10; H, 6.49. Measured: N, 11.02; C, 58.53; H, 6.44.

[0125] The product was characterized by X-ray single crystal diffraction and the specific results are shown in Table 7.

[0126] Table 7 Crystallographic parameters of [Mn((C4H9)2NPhN(CH2py)2)Cl2]

[0127]

[0128] The above data show that the target product [Mn((C4H9)2NPhN(CH2py)2)Cl2] was obtained in this preparation example.

[0129] Preparation Example 8

[0130] This preparation example provides an electrochromic material [Mn((C 13 H 27 )2NPhN(CH2py)2)Cl2], which is prepared by the following steps:

[0131] (1) Ligand preparation;

[0132] (2) Preparation of electrochromic material: Under nitrogen atmosphere, MnCl2 (104.5 mg, 0.83 mmol) and ligand (C 13 H 27)2NPhN(CH2py)2 (560.6 mg, 0.86 mmol) was added to 20 ml of acetonitrile, and the reaction mixture was heated to 82°C and allowed to react for 4 hours before cooling down. The reaction mixture was placed in a fume hood with the solvent evaporated naturally to obtain pale yellow crystals with a yield of 73%.

[0133] Elemental analysis (C 44 H 70 Calculated for Cl2MnN4: N, 7.17; C, 67.67; H, 9.04. Measured: N, 7.06; C, 67.92; H, 9.08.

[0134] The above data show that the target product [Mn((C 13 H 27 )2NPhN(CH2py)2)Cl2].

[0135] Example 1

[0136] The present embodiment provides an electrochromic device, which comprises a transparent substrate layer, a conductive layer, an electrochromic functional layer, a conductive layer, and a transparent substrate layer stacked in sequence, wherein the electrochromic material in the electrochromic functional layer is the electrochromic material prepared in Preparation Example 7 ([Mn((C4H9)2NPhN(CH2py)2)Cl2]), the ion conductor is a gel formed by a solution of a polyacrylate polymer and lithium bistrifluoromethanesulfonyl imide, and the counter electrode material is N,N'-diethyl-4,4'-bipyridyl salt.

[0137] The color-changing behavior of the electrochromic device was investigated at a voltage of 1.1 V. Figure 3 The electrochromic device can adjust the visible light transmittance. The transmittance color (Lab value) of the electrochromic device before and after the color change changes significantly. The specific results are shown in Table 8.

[0138] Table 8

[0139] L a b Before color change 88.75 -2.92 28.26 After color change 8.99 15.39 -32.69

[0140] The electrochromic device prepared in Example 1 includes the electrochromic material of the present invention and has good electrochromic performance.

Claims

1. An electrochromic functional layer, comprising an electrochromic material, wherein the electrochromic material is a mononuclear metal complex; The general structural formula of the mononuclear metal complex is: 1 )(X 2 )]; in, M is selected from manganese, cobalt, nickel, zinc, copper, iron or ruthenium; X 1 , X 2 Each independently selected from F, Cl, Br, I, or PF 6 ; A is a bipyridine ligand, and its structure is shown in Formula I: Formula I; R 1 , R 2 Each is independently selected from a saturated hydrocarbon group, an unsaturated hydrocarbon group, an aromatic group or a heteroatom-containing group.

2. The electrochromic functional layer according to claim 1, in, The structure of the mononuclear metal complex is shown in Formula II: Formula II.

3. The electrochromic functional layer according to claim 1, in, The electrochromic material is a crystal of the mononuclear metal complex.

4. The electrochromic functional layer according to any one of claims 1 to 3, in, The R 1 , R 2 Each is independently selected from a saturated hydrocarbon group or an aryl group.

5. The electrochromic functional layer according to any one of claims 1 to 3, in, The saturated hydrocarbon group is a straight-chain alkyl group or a branched-chain alkyl group having 1 to 20 carbon atoms.

6. The electrochromic functional layer according to claim 5, in, The saturated hydrocarbon group is methyl, ethyl, n-butyl, tert-butyl, n-heptyl, tert-octyl or n-tridecyl.

7. The electrochromic functional layer according to any one of claims 1 to 3, in, The aryl group is a monocyclic or polycyclic aromatic group having 6 to 20 carbon atoms.

8. The electrochromic functional layer according to claim 7, in, The aryl group is phenyl or naphthyl.

9. The electrochromic functional layer according to any one of claims 1 to 3, in, The unsaturated hydrocarbon group is a straight chain unsaturated hydrocarbon group or a branched chain unsaturated hydrocarbon group having 1 to 20 carbon atoms.

10. The electrochromic functional layer according to claim 9, in, The unsaturated hydrocarbon group is an allyl group.

11. The electrochromic functional layer according to any one of claims 1 to 3, in, The heteroatom-containing group is a functional group containing N, O, S, Si or P.

12. The electrochromic functional layer according to claim 11, in, The heteroatom-containing group is an ester group, an ether bond, an amide group or a conjugated group containing a heteroatom.

13. The electrochromic functional layer according to any one of claims 1 to 3, in, The R 1 , R 2 Each is independently selected from methyl, n-butyl, n-tridecyl or phenyl.

14. The electrochromic functional layer according to any one of claims 1 to 3, in, The M is selected from manganese, cobalt, nickel or zinc; the X 1 , X 2 Each is independently selected from Cl or Br.

15. The electrochromic functional layer according to any one of claims 1 to 3, in, The electrochromic material is selected from one of the following structures: ; 。 16. The electrochromic functional layer according to any one of claims 1 to 3, in, The electrochromic functional layer also contains an ion conductor and a counter electrode material.

17. An electrochromic device, comprising a transparent substrate layer, a conductive layer, and an electrochromic functional layer; in, The electrochromic functional layer is the electrochromic functional layer according to any one of claims 1 to 16.