One-component water-based conductive coating composition
By using high molecular weight acrylic resin and tackifying resin to replace part of polyolefins in single-component aqueous coatings, the adhesion performance of untreated PP substrates is improved, and the cost and insufficient adhesion performance caused by high polyolefin content is solved. The problem is that excellent adhesion and cost reduction under harsh conditions are achieved.
Patent Information
- Application Number
- CN202211338952.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-28
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-10-28
AI Technical Summary
Existing single-component water-based coatings lack adhesion performance on untreated PP substrates, especially under harsh conditions, and high polyolefin content leads to high costs and limited supply.
Develop a single-component water-based conductive coating composition, which comprises a high molecular weight acrylic resin, a tackifying resin and a polyolefin resin, with a polyolefin resin content of no more than 20 wt%. The coordinated cooperation between the high molecular weight acrylic resin and the tackifying resin is used to replace the part Polyolefins improve adhesion properties and reduce costs.
The same excellent adhesion properties as high-polyolefin content coatings are achieved, especially after steam injection, water immersion and oil immersion, and the cost is reduced by 20-25%.
Smart Images

Figure BDA0003915680180000121 
Figure BDA0003915680180000171
Abstract
Description
Technical Field
[0001] The invention relates to the field of coatings, in particular to a one-component water-based conductive coating, in particular to a coating used on an untreated polar substrate and / or non-polar substrate. Background Art
[0002] For one-component waterborne coatings on untreated PP substrates, waterborne polyolefin latexes (PO) are a viable solution for achieving good adhesion. Current commercial formulations have very high polyolefin content, which leads to cost and application drawbacks as well as compromised performance compared to other substrates.
[0003] In the one-component waterborne coating composition, increasing the polyolefin content can obtain better performance on untreated PP substrates, however, polyolefins are not conducive to the adhesion of ABS / PC+ABS, especially under harsh conditions, and are also not conducive to re-coating.
[0004] On the other hand, high polyolefin content will lead to high costs, and the corresponding suppliers are very limited. Currently there are only two Japanese suppliers, and their production capacity is insufficient.
[0005] Based on the above technical background, it is necessary to develop a new technology that can have both excellent performance and low cost. Summary of the invention
[0006] The inventors have conducted extensive research and developed a one-component water-based conductive coating composition that reduces the polyolefin content while having the same excellent adhesion performance as the coating with a high polyolefin content in the prior art, and even achieves better adhesion performance under harsh conditions, such as maintaining excellent adhesion after steam injection, water immersion, and oil immersion. In addition, the coating composition of the present invention reduces the cost by 20-25% compared with the prior art.
[0007] The present invention provides a one-component water-based conductive coating composition, comprising a resin component and a conductive pigment filler, wherein the resin component comprises a high molecular weight acrylic resin, a tackifying resin and a polyolefin resin, the high molecular weight acrylic resin has a weight average molecular weight greater than 75,000, and the content of the polyolefin resin based on the solid amount of the resin component is no more than 20wt%.
[0008] The present invention also provides a coated substrate, comprising a substrate and a coating composition coated on at least a portion of the substrate, wherein the coating composition is a one-component water-based conductive coating composition, which comprises a resin component and a conductive pigment filler, wherein the resin component comprises a high molecular weight acrylic resin, a tackifying resin and a polyolefin resin, the high molecular weight acrylic resin has a weight average molecular weight greater than 75,000, and the content of the polyolefin resin based on the solid amount of the resin component is not more than 20wt%.
[0009] The features and advantages of the present invention will be specifically presented in the following detailed description of the embodiments. DETAILED DESCRIPTION
[0010] As used herein, unless otherwise expressly stated, the numbers used in the specification and claims, such as values, ranges, amounts or percentages, should be considered to vary in all cases according to the term "about", even if the term is not expressly stated. Therefore, unless otherwise stated, the numerical parameters listed in the specification and claims herein are approximate values and may vary according to the properties to be obtained by the present invention.
[0011] Although the numerical ranges and parameters listed for the broad scope of the present invention are approximate, the numerical values listed in the specific examples are recorded as accurately as possible. However, any numerical value inherently has a certain error. The error is the inevitable result of the standard deviation obtained in its corresponding measurement method.
[0012] In addition, it should be understood that any numerical range described herein is intended to include all subranges subsumed therein. For example, a range of "1 to 10" is intended to include all subranges between (and including) the stated minimum value of 1 and the stated maximum value of 10, i.e., having a minimum value equal to or greater than 1 and a maximum value equal to or less than 10.
[0013] In this application, unless otherwise expressly stated, the use of the singular includes the plural and the plural includes the singular. In addition, in this application, unless otherwise expressly stated, the use of "or" means "and / or", even if "and / or" can be explicitly used in some cases. In addition, in this application, unless otherwise expressly stated, the use of "a" or "an" means "at least one". For example, "a" polymer, "a" coating, etc. refers to any one or more of these items. And, as those skilled in the art will recognize, the features of one embodiment can be used with other embodiments, even if not explicitly stated.
[0014] As used herein, the term "coating" refers to a type of fluid substance that is applied to the surface of a substrate and can be cured by natural or artificial methods to form a coating that covers the surface of the substrate and has protective and decorative effects.
[0015] As used herein, the term "aqueous" means that the solvent of the coating composition contains at least 50 wt % of water.
[0016] As used herein, the term "single component" means that all film-forming substances, pigments, fillers, solvents, additives, etc. of the coating composition are packaged in one container, thus having the advantages of convenient storage and use.
[0017] As used herein, the term "conductive" means that when the coating composition is applied to the surface of a substrate, the surface resistance of the substrate can be greatly reduced, which facilitates the subsequent electrostatic spraying of the coating. The coating formed by the one-component water-based conductive coating composition according to the present invention can have a resistance of less than 500KΩ after dehydration at 80°C*5min. The resistance can be measured by a Ransburg resistance tester.
[0018] The one-component waterborne conductive coating composition according to the present invention is a heat-curable coating composition, that is, the coating composition needs to be cured by heating to form a film after being applied to the surface of the substrate. In this article, the term "curing" refers to the process of a material becoming fixed and no longer flowing. Suitably, the one-component waterborne conductive coating composition according to the present invention can be cured at 40-80°C*5-10min.
[0019] The one-component water-based conductive coating composition according to the present invention is a thermoplastic composition. In this article, the term "thermoplastic" means that the components in the coating composition are not covalently bonded after curing, and the formed coating film softens after heating. In this article, thermoplastic compositions and non-crosslinked compositions can be used interchangeably.
[0020] The one-component water-based conductive coating composition according to the present invention has a solid content of 30% to 35%. As used herein, the term "solid content" refers to the ratio of the remaining mass of the coating composition after drying and baking to the mass of the coating composition, which can be measured according to GB / T 1725-79 "Determination of Solid Content of Coatings".
[0021] The present invention provides a one-component water-based conductive coating composition, comprising a resin component and a conductive pigment filler, wherein the resin component comprises a high molecular weight acrylic resin, a tackifying resin and a polyolefin resin, the high molecular weight acrylic resin has a weight average molecular weight greater than 75,000, and the content of the polyolefin resin based on the solid amount of the resin component is no more than 20wt%.
[0022] In this article, the "resin component" may also be referred to as "film-forming resin", which refers to a resin in a coating composition that can form a self-supporting, continuous coating film at least on a horizontal surface. In this article, the "resin component solid amount" refers to the sum of the solid weights of the film-forming resin.
[0023] In this article, the "acrylic resin" refers to a polymer with (meth) acrylic monomer as the basic component. The "basic component" means that the (meth) acrylic monomer accounts for at least about 70wt% of all polymerized monomers in the polymer, such as at least about 80wt%, such as at least about 90wt%.
[0024] The acrylic resin used in the present invention has a high molecular weight. The high molecular weight acrylic resin imparts enhanced cohesion to the coating composition. Suitably, the acrylic resin has a weight average molecular weight (Mw) greater than 75,000, such as a Mw greater than 100,000. The weight average molecular weight (Mw) can be measured by gel permeation chromatography using appropriate standards such as polystyrene standards.
[0025] In order to meet the overall performance requirements of the coating, the selection of acrylic resin also needs to consider the impact on other mechanical properties.
[0026] The acrylic resin used in the present invention may have a glass transition temperature (Tg) of less than 0°C, such as less than -10°C, not more than -20°C, for example -20 to -40°C. The glass transition temperature can be measured by conventional methods in the art, for example, by differential scanning calorimetry (DSC), and the test conditions can be tested using conventional test conditions in the art, for example, heating from 0°C to 150°C at a heating rate of 10K / min, cooling from 150°C to 0°C, and then heating from 0°C to 150°C, with a nitrogen rate of 50ml / min. A specific range of glass transition temperatures can provide the coating with good flexibility and low-temperature bendability.
[0027] The acrylic resin used in the present invention may have an acid value of no more than 10 mgKOH / g, such as an acid value of 5 to 8 mgKOH / g. The "acid value" refers to the number of milligrams of potassium hydroxide required to neutralize the free acid in 1 gram of resin. A suitable acid value avoids the adverse enhancement of the hydrophilicity of the coating, which in turn leads to a decrease in water resistance.
[0028] The acrylic resin suitable for use in the present invention may be in the form of a dispersion or emulsion, with a solid content of 30 to 70 wt%, such as 40 to 60 wt%. The "solid content" refers to the percentage of the mass remaining after evaporation to the mass of the original dispersion / emulsion.
[0029] The one-component aqueous conductive coating composition according to the present invention may include about 10 wt % or more, such as about 15 wt % or more, for example, about 20 wt % or more of acrylic resin, based on the solid amount of the resin component of the one-component aqueous conductive coating composition, and / or may include about 40 wt % or less, such as about 35 wt % or less, for example, about 30 wt % or less of acrylic resin. The acrylic resin may be present in the composition in a range of about 10 to 40 wt %, such as about 15 to 35 wt %, for example, about 20 to 30 wt %, or any other combination of these end values, based on the solid amount of the resin component of the one-component aqueous conductive coating composition.
[0030] The tackifying resin used in the present invention may include rosin resin and / or terpene resin. Examples of the rosin resin include, but are not limited to, natural rosin, polymerized rosin, modified rosin modified with maleic acid, fumaric acid, (meth) acrylic acid, etc., and rosin derivatives, such as esters, phenolic modifications, and hydrogenated products of the above rosins. Examples of the terpene resin include, but are not limited to, resins composed of α-pinene, β-pinene, limonene, dipentene, terpene phenols, terpene alcohols, and / or terpene aldehydes, and derivatives of the above resins, such as hydrogenated products.
[0031] Tackifying resins can provide enhanced initial adhesion to coatings, but they also affect the coating's coating properties, substrate wetting properties, and water resistance, which can adversely reduce adhesion. For this reason, the selection of tackifying resins requires a comprehensive consideration of various properties.
[0032] The tackifying resin used in the present invention has a Mw of less than 1,000, suitably less than 800, such as less than 600. The Mw may be determined by gel permeation chromatography using appropriate standards such as polystyrene standards.
[0033] Suitably, the tackifying resin used in the present invention has a softening point below 100° C., for example, a softening point below 90° C., or a softening point below 80° C., or a softening point below 70° C. The softening point can be determined with reference to GB 8146. The softening point within this range will not deteriorate the coating performance and substrate wetting performance of the coating while ensuring the favorable properties of the tackifying resin.
[0034] Suitably, the tackifying resin used in the present invention has an acid value of no more than 10 mgKOH / g, such as an acid value of 5 to 8 mgKOH / g. The "acid value" refers to the milligrams of potassium hydroxide required to neutralize the free acid in 1 gram of resin. The acid value is beneficial to the water resistance of the coating.
[0035] The tackifying resin suitable for use in the present invention may be in the form of a dispersion or emulsion, with a solid content of 30 to 70 wt%, such as 40 to 60 wt%. The "solid content" refers to the percentage of the mass remaining after evaporation to the mass of the original dispersion / emulsion.
[0036] The one-component aqueous conductive coating composition according to the present invention may include about 10 wt % or more, such as about 15 wt % or more, for example, about 20 wt % or more of a tackifying resin, based on the solid amount of the resin component of the one-component aqueous conductive coating composition, and / or may include about 40 wt % or less, such as about 35 wt % or less, for example, about 30 wt % or less of a tackifying resin. The tackifying resin may be present in the composition in a range of about 10 to 40 wt %, such as about 15 to 35 wt %, for example, about 20 to 30 wt %, or any other combination of these end values, based on the solid amount of the resin component of the one-component aqueous conductive coating composition.
[0037] In the one-component water-based conductive coating composition of the present invention, the weight ratio of acrylic resin to tackifying resin may be about 1-4:4-1, such as about 1-3:3-1, such as 4:1, 4:2, 4:3, 1:1, 1:2, 1:3 or 1:4.
[0038] The "polyolefin" resin used in the present invention refers to a polymer with olefin monomers as the basic component. The "basic component" means that the olefin monomers in the polymer account for at least about 50wt%, such as at least about 60wt%, such as at least about 70wt% of all polymerized monomers.
[0039] The polyolefin resin suitable for the present invention in the art can be selected from one or more of polyethylene, ethylene-vinyl acetate copolymer, polypropylene, polystyrene and acrylonitrile-butadiene-styrene copolymer resin.
[0040] The polyolefin resin suitable for the present invention in the art is a non-halogenated polyolefin resin. The non-halogenated polyolefin resin refers to a polyolefin resin that does not contain halogen. For example, the polyolefin resin suitable for the present invention is a non-chlorinated polyolefin resin. The non-chlorinated polyolefin resin refers to a polyolefin resin that does not contain chlorine. The polyolefin resin suitable for the present invention can also be a maleic acid-modified polyolefin resin.
[0041] The polyolefin resin suitable for use in the present invention may be in the form of a dispersion or emulsion, with a solid content of 10 to 50 wt%, such as 20 to 40 wt%. The "solid content" refers to the percentage of the mass remaining after evaporation to the mass of the original dispersion / emulsion.
[0042] In the one-component water-based conductive coating of the present invention, the synergistic combination of the high molecular weight acrylic resin and the tackifying resin produces good substrate adhesion, especially on untreated PP and / or ABS substrates. Therefore, the high molecular weight acrylic resin and the tackifying resin can partially replace polyolefins, so that the one-component water-based conductive coating of the present invention has the same excellent performance effect as the coating with high polyolefin content in the prior art at a low polyolefin content.
[0043] Suitably, the content of the polyolefin resin based on the solid amount of the resin component is no more than 20wt%, such as about 18wt% or less, for example 15wt% or less. For example, based on the solid amount of the resin component of the one-component aqueous conductive coating composition, the one-component aqueous conductive coating composition according to the present invention may include about 5wt% or more, for example about 8wt% or more, such as about 10wt% or more of the polyolefin resin, and may include about 20wt% or less, such as about 18wt% or less, for example about 15wt% or less of the polyolefin resin. Based on the solid amount of the resin component of the one-component aqueous conductive coating composition, the polyolefin resin may be present in the composition in a range of about 5 to 20wt%, such as about 8 to 18wt%, for example about 10 to 15wt%, or any other combination of these end values.
[0044] The resin component in the aqueous one-component conductive coating composition according to the present invention may also include a polyurethane resin. The polyurethane resin refers to a polymer whose repeating units include a carbamate functional group. The polyurethane may include a polymer of at least 50wt% of organic units, such as at least 70wt%, such as at least 90wt% of organic units connected by carbamate bonds. In this context, the organic unit includes one or more residues selected from the following: simple diols, such as butanediol, polyester diols, polyether diols, polycarbonate diols, etc.
[0045] The polyurethane resin suitable for use in the present invention may be in the form of a dispersion or emulsion, with a solid content of 20 to 60 wt%, such as 30 to 50 wt%. The "solid content" refers to the percentage of the mass remaining after evaporation to the mass of the original dispersion / emulsion.
[0046] In the water-based one-component conductive coating composition of the present invention, acrylic resin, polyurethane resin, rosin resin and polyolefin resin are compounded to achieve excellent adhesion effect. Specifically, in the water-based one-component conductive coating composition of the present invention, the usage ratio of acrylic resin, polyurethane resin and rosin resin is 1-10:10-30:1-20, suitably 1-10:10-20:1-10, such as 5-10:10-15:5-10.
[0047] The aqueous conductive coating composition according to the present invention may include about 20 wt % or more, such as about 25 wt % or more, for example, about 30 wt % or more of a polyurethane resin, based on the solid amount of the resin component of the aqueous one-component conductive coating composition, or may include about 50 wt % or less, such as about 45 wt % or less, for example, about 40 wt % or less of a polyurethane resin. The polyurethane resin may be present in the composition in a range of about 20 to 50 wt %, such as about 25 to 45 wt %, for example, about 30 to 40 wt %, or any other combination of these end values, based on the solid amount of the resin component of the aqueous one-component conductive coating composition.
[0048] The water-based one-component conductive coating composition according to the present invention may include conductive pigments and fillers. The conductive pigments and fillers refer to pigments and / or fillers whose surfaces are treated to form a conductive oxide layer. Common conductive pigments and fillers in the art may be used in the present invention. Conductive pigments and fillers suitable for use in the present invention may include one or more of conductive titanium dioxide, conductive carbon black, graphene, conductive nanotubes, and conductive mica.
[0049] Based on the total weight of the one-component waterborne conductive coating composition, the one-component waterborne conductive coating composition according to the present invention may include about 0.1 wt% or more, 1 wt% or more, 5 wt% or more, such as about 10 wt% or more, for example, about 15 wt% or more of conductive pigments, and / or may include about 35 wt% or less, such as about 30 wt% or less, for example, about 25 wt% or less of conductive pigments. Based on the total weight of the one-component waterborne conductive coating composition, the conductive pigment may be present in the composition in a range of about 0.1 to 35 wt%, such as about 1 to 30 wt%, for example, about 5 to 25 wt%, or any other combination of these end values.
[0050] In the water-based one-component conductive coating composition of the present invention, the weight ratio of the resin component to the conductive pigment and filler may be about 7:1 to 10:1, for example, 7:1, 8:1, 9:1 or 10:1.
[0051] Based on the requirements of performance and appearance, the aqueous one-component conductive coating composition according to the present invention may also include non-conductive pigments and fillers, that is, non-conductive pigments and / or non-conductive fillers. Non-conductive pigments suitable for use in the present invention may include organic pigments and / or inorganic pigments, such as titanium dioxide, perylene-perylene red, etc.; and / or, effect pigments, such as aluminum powder, pearlescent powder, etc. Non-conductive fillers suitable for use in the present invention may include one or more of matting powder, barium sulfate and calcium carbonate. Generally, the aqueous one-component conductive coating composition according to the present invention may include 0 to 40 wt% of non-conductive pigments and fillers based on the total weight of the coating composition.
[0052] The one-component water-based conductive coating composition according to the present invention may further include 0 to 10 wt% of an organic solvent (also referred to as a "cosolvent") based on the total weight of the coating composition. The organic solvent may help the components in the composition to be compatible, thereby affecting the properties of the paint film. The organic solvent suitable for the present invention may include one or more of hydrocarbon solvents, ester solvents, ether solvents, alcohol solvents, and alcohol ether solvents, such as alcohol solvents and / or alcohol ether solvents.
[0053] The one-component aqueous conductive coating composition according to the present invention may further include 20 to 40 wt % of water based on the total weight of the coating composition.
[0054] Based on the requirements of performance and appearance, the water-based one-component conductive coating composition according to the present invention may also include a substrate wetting agent, a dispersant and / or a crosslinking aid. The substrate wetting agent suitable for the present invention may include a polyether-modified polysiloxane substrate wetting agent, and its amount may be 0 to 2 wt% based on the total weight of the coating composition, such as 0.1 to 2 wt%. The dispersant suitable for the present invention may include a polyurethane wetting dispersant, and its amount may be 0 to 5 wt%, such as 0.1 to 5 wt%. The crosslinking aid suitable for the present invention may include an amino resin, a blocked isocyanate or a carbodiimide, and its amount may be 0 to 8 wt% based on the total weight of the coating composition.
[0055] The one-component waterborne conductive coating composition according to the present invention may further include one or more of the following other auxiliary ingredients, including but not limited to, rheological additives for adjusting the rheological properties of the coating, improving the anti-settling property during storage and the anti-sagging property during application; anti-foaming agents and defoaming agents for inhibiting the formation of bubbles and making the generated bubbles escape or burst during the production process; anti-pinhole agents for increasing the surface tension of the coating and eliminating pinholes; fragrances for providing a pleasant smell to the coating; preservatives for protecting the coating from mold; pH regulators for controlling pH and stabilizing the coating; waxes for improving scratch resistance and improving touch; thickeners for increasing the viscosity of the coating and improving the wet film thickness and protecting the coating from sedimentation and delamination, etc. When these auxiliary ingredients are present, each auxiliary ingredient is present in an amount of up to about 2 wt% based on the total weight of the coating composition.
[0056] The water-based one-component conductive coating composition according to the present invention can be obtained by the following preparation method, comprising:
[0057] (1) mixing a resin component, a solvent and optional additives;
[0058] (2) adding matting powder and non-conductive pigment to the mixture obtained in (1), and dispersing at a high speed of more than 1000 rpm for more than 60 minutes, so that the fineness of the mixture is ≥7.0 HGM;
[0059] (3) Add conductive pigment to the mixture obtained in (2).
[0060] Suitably, the method for preparing the waterborne one-component conductive coating composition according to the present invention is carried out at 10-35°C.
[0061] Suitably, in the method for preparing the water-based one-component conductive coating composition according to the present invention, step (1) is carried out at a rotation speed of 500 to 1000 rpm.
[0062] Suitably, according to the method for preparing the water-based one-component conductive coating composition of the present invention, the acrylic resin, polyurethane resin, rosin resin and polyolefin resin in step (1) are added to the reactor in sequence.
[0063] Suitably, according to the method for preparing the water-based one-component conductive coating composition of the present invention, the solvent in step (1) comprises water and / or an organic solvent.
[0064] Suitably, according to the method for preparing the water-based one-component conductive coating composition of the present invention, the pH value of the mixture obtained in step (1) is 8.2-8.8.
[0065] Suitably, according to the method for preparing the water-based one-component conductive coating composition of the present invention, the non-conductive pigment and filler in step (2) is added in the form of grinding slurry.
[0066] Suitably, according to the method for preparing the water-based one-component conductive coating composition of the present invention, the conductive pigment in step (3) is added in the form of grinding slurry.
[0067] Suitably, according to the method for preparing the water-based one-component conductive coating composition of the present invention, the pH value of the composition system after step (3) is adjusted to 8.2-8.8.
[0068] The grinding slurry of the conductive pigment and the non-conductive pigment can be prepared by conventional methods in the art. The grinding slurry of the conductive pigment and the non-conductive pigment suitable for the water-based one-component conductive coating composition of the present invention can be obtained by the following preparation method, including:
[0069] (1) adding water and optional additives into a container;
[0070] (2) Adding conductive pigments or non-conductive pigments during stirring, and adding defoaming agent after dispersion;
[0071] In step (1), the optional auxiliary agent is preferably a dispersant and / or a rheological auxiliary agent;
[0072] In step (2), a pH adjuster is optionally further added.
[0073] The present invention also provides a coated substrate, comprising a substrate and a coating composition coated on the substrate, wherein the coating composition is a one-component water-based conductive coating composition, which comprises a resin component and a conductive pigment filler, wherein the resin component comprises a high molecular weight acrylic resin, a tackifying resin and a polyolefin resin, the high molecular weight acrylic resin has a weight average molecular weight greater than 75,000, and the content of the polyolefin resin based on the solid amount of the resin component is not more than 20wt%.
[0074] Suitably, the substrate may be a non-metallic substrate, including a PP and / or ABS substrate. Suitably, the substrate may be a polar substrate, or a non-polar substrate.
[0075] According to the coated substrate of the present invention, the substrate may not have been subjected to surfactant treatment, chemical treatment, flame treatment, UV treatment and / or plasma treatment.
[0076] The one-component water-based conductive coating composition of the present invention can be applied by any standard method known in the art, such as spraying, dipping, roller coating, brushing, etc., and then cured under heating conditions to form a coating. Generally, the one-component water-based conductive coating composition according to the present invention is cured at 40 to 80° C. * 5 to 10 minutes. The coating formed by the coating composition of the present invention can be applied to a thickness of 1-20 μm, preferably 5-20 μm, 1-15 μm or 5-10 μm.
[0077] Example
[0078] The following examples are provided to further illustrate the present invention but should not be construed as limiting the invention to the details described in the examples. Unless otherwise indicated, all parts and percentages in the following examples are by weight.
[0079] Embodiment 1:
[0080] The one-component water-based conductive coating A1 provided by the present invention is prepared using the components and contents listed in Table 1 below, and the specific steps are: (1) adding acrylic resin, polyurethane resin, rosin resin, and polyolefin resin to a reactor in sequence under stirring; (2) adjusting the pH value of the mixture in step (1) to 8.2-8.8, and adding appropriate deionized water to adjust the viscosity of the system; (3) stirring and adding a defoamer and an organic solvent to the mixture in step (2); (4) stirring and adding white slurry and matting powder to the mixture in step (3), and dispersing the matting powder at a high speed of more than 1000 rpm for more than 60 minutes, and detecting a fineness of ≥7.0 HGM; (5) stirring and adding a conductive black slurry, a substrate wetting agent, a defoamer, and a rheological additive to the mixture in step (4); and (6) adjusting the pH of the system to 8.2-8.8.
[0081] The preparation method of the white slurry is as follows: 1) adding water, a dispersant, and a rheological additive into a container in sequence under stirring; 2) slowly adding titanium dioxide and a defoaming agent under stirring, and grinding after high-speed dispersion for 60 minutes.
[0082] The preparation method of the conductive black slurry is as follows: 1) adding water and a dispersant into a container in sequence while stirring, 2) slowly adding conductive carbon black while stirring, 3) after high-speed dispersion for 60 minutes, adding a defoamer and a pH adjuster while stirring, and continuing high-speed dispersion for 20 minutes before grinding.
[0083] Table 1. One-component water-based conductive coatings A1-A6 and C1-C4
[0084]
[0085]
[0086] “\” indicates that the component is not added; each resin component (wt %) represents the solid content.
[0087] a. Amino resin;
[0088] b. Blocked isocyanate;
[0089] c. Carbodiimide;
[0090] Embodiment 2:
[0091] Prepare a one-component water-based conductive coating A2 according to the steps of Example 1
[0092] Embodiment 3:
[0093] Prepare a one-component water-based conductive coating A3 according to the steps of Example 1
[0094] Embodiment 4:
[0095] The one-component water-based conductive coating A4 provided by the present invention is prepared using the components and contents listed in Table 1, and the specific steps are: (1) adding acrylic resin, polyurethane resin, rosin resin, and polyolefin resin to a reactor in sequence under stirring; (2) adjusting the pH value of the mixture in step (1) to 8.2-8.8, and adding appropriate deionized water to adjust the viscosity of the system; (3) stirring and adding a defoamer and an organic solvent to the mixture in step (2); (4) stirring and adding white slurry and matting powder to the mixture in step (3), and high-speed dispersing the matting powder at a speed greater than 1000 rpm for more than 60 minutes, and detecting a fineness of ≥7.0 HGM; (5) stirring and adding a conductive black slurry, an amino resin, a substrate wetting agent, a defoamer, and a rheological additive to the mixture in step (4); and (6) adjusting the pH of the system to 8.2-8.8.
[0096] Embodiment 5:
[0097] The one-component water-based conductive coating A5 provided by the present invention is prepared using the components and contents listed in Table 1, and the specific steps are: (1) adding acrylic resin, polyurethane resin, rosin resin, and polyolefin resin to a reactor in sequence under stirring; (2) adjusting the pH value of the mixture in step (1) to 8.2-8.8, and adding appropriate deionized water to adjust the viscosity of the system; (3) stirring and adding a defoamer and an organic solvent to the mixture in step (2); (4) stirring and adding white slurry and matting powder to the mixture in step (3), and dispersing the matting powder at a high speed of more than 1000 rpm for more than 60 minutes, and detecting a fineness of ≥7.0 HGM; (5) stirring and adding a conductive black slurry, a blocked isocyanate, a substrate wetting agent, a defoamer, and a rheological additive to the mixture in step (4); and (6) adjusting the pH of the system to 8.2-8.8.
[0098] Example 6
[0099] The one-component water-based conductive coating A6 provided by the present invention is prepared using the components and contents listed in Table 1, and the specific steps are: (1) adding acrylic resin, polyurethane resin, rosin resin, and polyolefin resin to a reactor in sequence under stirring; (2) adjusting the pH value of the mixture in step (1) to 8.2-8.8, and adding appropriate deionized water to adjust the viscosity of the system; (3) stirring and adding a defoamer and an organic solvent to the mixture in step (2); (4) stirring and adding white slurry and matting powder to the mixture in step (3), and dispersing the matting powder at a high speed of more than 1000 rpm for more than 60 minutes, and detecting a fineness of ≥7.0 HGM; (5) stirring and adding a conductive black slurry, carbodiimide, a substrate wetting agent, a defoamer, and a rheological additive to the mixture in step (4); (6) adjusting the pH of the system to 8.2-8.8.
[0100] Comparative Example C1
[0101] The components and contents listed in Table 1 were used to prepare a single-component water-based conductive coating C1 used as a comparative example. The specific steps were as follows: (1) adding a polyolefin resin into a reactor, and adding appropriate deionized water to adjust the viscosity of the system; (2) adding a defoamer, an organic solvent and a white slurry to the mixture in step (1) with stirring, and adjusting the pH value of the mixture in step (2) to 8.2-8.8; (3) adding a matting powder with stirring, and dispersing the matting powder at a high speed of more than 1000 rpm for more than 60 minutes, and detecting a fineness of ≥7.0 HGM; (4) adding a conductive black slurry, a substrate wetting agent, a defoamer and a rheological additive to the mixture in step (3) with stirring; and (5) adjusting the pH value of the system to 8.2-8.8.
[0102] Comparative Example C2
[0103] The components and contents listed in Table 1 were used to prepare a single-component water-based conductive coating C2 used as a comparative example. The specific steps were as follows: (1) adding a polyolefin resin and a polyurethane resin into a reactor in sequence, and adding appropriate deionized water to adjust the viscosity of the system; (2) adding a defoamer, an organic solvent and a white slurry to the mixture in step (1) with stirring, and adjusting the pH value of the mixture in step (2) to 8.2-8.8; (3) adding a matting powder with stirring, and dispersing the matting powder at a high speed at a speed greater than 1000 rpm for more than 60 minutes, and detecting a fineness of ≥7.0 HGM; (4) adding a conductive black slurry, a substrate wetting agent, a defoamer and a rheological additive to the mixture in step (3) with stirring; and (5) adjusting the pH value of the system to 8.2-8.8.
[0104] Comparative Example C3
[0105] The components and contents listed in Table 1 were used to prepare a single-component water-based conductive coating C3 used as a comparative example. The specific steps were as follows: (1) polyolefin resin, polyurethane resin, and acrylic resin were added to a reactor in sequence, and appropriate deionized water was added to adjust the viscosity of the system; (2) a defoamer, an organic solvent, and a white slurry were added to the mixture in step (1) with stirring, and the pH value of the mixture in step (2) was adjusted to 8.2-8.8; (3) matting powder was added with stirring, and the matting powder was dispersed at a high speed of more than 1000 rpm for more than 60 minutes, and the fineness was detected to be ≥7.0 HGM; (4) conductive black slurry, substrate wetting agent, defoamer, and rheological additive were added to the mixture in step (3) with stirring; and (5) the pH of the system was adjusted to 8.2-8.8.
[0106] Comparative Example C4
[0107] The specific steps of preparing the one-component water-based conductive coating C4 used as a comparative example using the components and contents listed in Table 1 are as follows: (1) adding polyolefin resin, polyurethane resin and rosin resin into a reactor in sequence, and adding appropriate deionized water to adjust the viscosity of the system; (2) adding defoaming agent, organic solvent and white slurry to the mixture in step (1) with stirring, and adjusting the pH value of the mixture in step (2) to 8.2-8.8; (3) adding matting powder with stirring, and dispersing the matting powder at a high speed of more than 1000 rpm for more than 60 minutes, and detecting the fineness ≥7.0 HGM; (4) adding conductive black slurry, substrate wetting agent, defoaming agent and rheological additive to the mixture in step (3) with stirring; (5) adjusting the pH value of the system to 8.2-8.8.
[0108] Performance Test:
[0109] First, the one-component water-based conductive coatings A1, A2, A3, A4, A5, A6 provided by the present invention and the one-component water-based conductive coatings C1, C2, C3, C4 of the comparative example are applied to an untreated PP or ABS substrate and cured at 40-80°C*5-10min; then a water-based color paint is applied and cured at 40-80°C*5-10min, and a solvent-based varnish is cured at 80-90°C*30-50min, and finally placed at room temperature for 7 days.
[0110] The coated substrates were subjected to the following performance tests:
[0111] Adhesion performance: Refer to GMW14829-2017A standard to evaluate the adhesion performance of the coating. Requirements: Adhesion level 0-1.
[0112] Substrate A1 A2 A3 A4 A5 A6 C1 C2 C3 C4 PP OK OK OK OK OK OK OK NG OK NG ABS OK OK OK OK OK OK OK OK NG NG
[0113] Adhesion performance under harsh conditions:
[0114] Steam injection :
[0115] standard PV1503 equipment Walter Line 60° "X" cross line Knives knife Water temperature 70℃ Injection pressure 90±5bar Water flow 10.5L / min Impact Angle 45° Impact distance 150mm Impact time 20s per cut Nozzle requirements EG 2505 Impact method Spray along the line, once per line Require No paint film delamination at the line
[0116] Flooding : Soak in 40 degree water for 240 hours continuously. The test standard is based on GBT1733. The specific method is as follows:
[0117] Add enough deionized water to the water tank, adjust the water temperature to 40±1℃, and maintain this temperature during the whole test process, then start the circulation and ventilation of the water in the tank, place the sample on the test plate rack, immerse 2 / 3 of the sample in the water, keep the samples at least 30mm apart, and at least 50mm apart from the bottom and wall of the tank, constantly change the position of the sample in the tank during the test, and the change time interval shall not exceed 3d. After reaching the specified time of 240h, take the sample out of the tank, use filter paper to absorb the water marks, and check the surface of the sample for loss of gloss, discoloration, blistering and other phenomena after 24 hours of recovery, and test the adhesion to evaluate the water resistance of the paint film. Test results: The appearance should be free of defects such as loss of gloss, discoloration, blistering, wrinkling, etc., and the adhesion is 0-1 level.
[0118] Oil immersion : Soak in E92# gasoline for half an hour. The specific method is as follows:
[0119] Add enough gasoline to the glass tank, insert the sample into the tank, and immerse 2 / 3 of the length of the test plate in 92# gasoline. After the specified time, take out the sample and wipe the surface with filter paper to remove the residual liquid on the surface. The recovery time is 24 hours. Observe the surface loss of gloss, discoloration, bubbling and other phenomena of the paint film and test the adhesion to evaluate the gasoline resistance of the paint film. Test results: The appearance should be free of defects such as loss of gloss, discoloration, bubbling, etc., and the adhesion is 0-1 level.
[0120] Steam injection for harsh conditions
[0121] Substrate A1 A2 A3 A4 A5 A6 C1 C2 C3 C4 PP OK OK OK OK OK OK OK NG NG NG ABS OK OK OK OK OK OK NG OK NG NG
[0122] Water resistant under harsh conditions
[0123] Substrate A1 A2 A3 A4 A5 A6 C1 C2 C3 C4 PP OK OK OK OK OK OK OK NG NG NG ABS OK OK OK OK OK OK OK NG NG NG
[0124] Resistant to E92# gasoline under harsh conditions
[0125] Substrate A1 A2 A3 A4 A5 A6 C1 C2 C3 C4 PP OK OK OK OK OK OK OK NG NG NG
[0126] Other performance tests
[0127]
[0128] *Recoating refers to coating a base material with primer + color paint + clear coat, and then coating a base material with primer + color paint + clear coat again, wherein the primer is the single-component water-based conductive coating according to the present invention.
[0129] From the above performance test results, it can be seen that the one-component water-based conductive coating provided by the present invention has significantly excellent steam jet performance - it can pass the steam jet of PV1503 standard; it has significantly excellent water resistance - after continuous immersion in 40-degree water for 240 hours, the sample surface is checked for no loss of gloss, discoloration, blistering, etc., and the test adhesion is 0-1 level; it has excellent gasoline resistance - after immersion in E92# gasoline for half an hour, the sample surface is checked for no loss of gloss, discoloration, blistering, etc., and the test adhesion is 0-1 level. In addition, the one-component water-based conductive coating provided by the present invention also meets the performance requirements of cold and wet cycle, accelerated aging resistance, impact resistance, recoating, etc. of primer for automotive parts.
[0130] Therefore, it can be seen from the above performance test results that the present invention, by replacing part of the polyolefin resin with acrylic resin, polyurethane polyester and tackifying resin, further reduces the cost while improving the adhesion of the coating to the substrate, especially the adhesion to the ABS substrate. Even under harsh conditions, such as steam injection, water immersion and oil immersion, the one-component water-based conductive coating provided by the present invention still has excellent adhesion, and also has excellent water resistance, oil resistance and adhesion.
[0131] While particular aspects of the invention have been illustrated and described, it will be apparent to those skilled in the art that various other changes and modifications may be made without departing from the spirit and scope of the invention. It is therefore intended that the appended claims cover all such changes and modifications as fall within the scope of the invention.
Claims
1. A one-component water-based conductive coating composition, comprising a resin component and a conductive pigment, wherein the resin component comprises a high molecular weight acrylic resin, a rosin resin, a polyurethane and a polyolefin resin, wherein the high molecular weight acrylic resin has a weight average molecular weight greater than 100,000 and a glass transition temperature of -20 to -40°C, the rosin resin has a softening point lower than 80°C and an acid value of no more than 10 mgKOH / g, the high molecular weight acrylic resin, the polyurethane resin and the rosin resin are used in a ratio of 1-10:10-30:1-20, and the content of the polyolefin resin based on the solid amount of the resin component is no more than 20 wt%.
2. The coating composition of claim 1, wherein the composition is thermoplastic.
3. The coating composition of claim 1, wherein the weight ratio of the high molecular weight acrylic resin to the rosin resin is 4:1 to 1:
4.
4. The coating composition according to claim 1, wherein the high molecular weight acrylic resin has an acid value of not more than 10 mgKOH / g.
5. The coating composition of claim 1, wherein the high molecular weight acrylic resin comprises at least 70 wt% of (meth)acrylic monomers based on the solid weight thereof.
6. The coating composition of claim 1, wherein the rosin resin has a weight average molecular weight of less than 1,000.
7. The coating composition according to claim 1, wherein the weight ratio of the resin component to the conductive pigment is 7:1 to 10:
1.
8. The coating composition of claim 1, wherein the coating composition has a solid content of 30% to 35%.
9. The coating composition according to claim 1, wherein the coating formed by the coating composition has a resistance of less than 500 kΩ after dehydration at 80°C for 5 minutes.
10. The coating composition according to claim 1, wherein the coating formed by the coating composition has an adhesion of at least grade 0 to 1 on untreated PP and / or ABS, with reference to GMW14829-2017 A standard.
11. A coated substrate comprising a substrate and the coating composition according to any one of claims 1 to 10 applied on at least a portion of the substrate.
12. The coated substrate of claim 11, wherein the substrate comprises a non-metallic substrate.
13. The coated substrate of claim 11 or 12, wherein the substrate comprises PP and / or ABS.
14. The coated substrate of claim 11, wherein the substrate comprises a polar substrate and / or a non-polar substrate.