Preparation method and application of polyurethane sealing material for shield main drive

By introducing fluoropolyether and fluoroelastomer into the main drive polyurethane sealing material of the shield machine and carrying out molding vulcanization of polytetrafluoroethylene, the problem of performance attenuation of polyurethane sealing materials at high temperatures is solved, and the material resistance is significantly improved High temperature performance and equipment construction efficiency.

CN115572360BActive Publication Date: 2024-11-08CHINA RAILWAY ENGINEERING EQUIPMENT GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211216972.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-30
Publication Date
2024-11-08
Estimated Expiration
2042-09-30

AI Technical Summary

Technical Problem

The existing shield machine main drive polyurethane sealing materials have severely attenuated wear resistance, tensile strength, hardness, tear strength and other properties under high temperature conditions, affecting the material's performance and equipment construction efficiency.

Method used

The fluoropolyether glycol and diisocyanate are used for polypolymerization, and the isocyanate-capped fluoropolyurethane prepolymer is obtained, and the isocyanate-capped fluoropolyurethane-fluororubber is added to the polypolymerization reaction with the terminal hydroxyl liquid fluororubber to form the isocyanate-capped fluoropolyurethane-fluororubber copolymer. The molding vulcanization is then performed under the condition of adding or not adding hydroxyl surface-modified polytetrafluoroethylene, using diamines and/or diols as curing agents.

Benefits of technology

It improves the wear resistance, tensile strength, hardness and tear strength of polyurethane sealing materials at high temperatures, extends the service life of the material and the construction efficiency of the equipment, and broadens the upper limit of the use temperature of the sealing materials and the equipment speed.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115572360B_ABST
    Figure CN115572360B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of polyurethane sealing materials, and specifically relates to a preparation method and application of a polyurethane sealing material for a shield main drive. The preparation method comprises the following steps: (1) a fluorine-containing polyether diol and a diisocyanate are subjected to an addition polymerization reaction to obtain an isocyanate-terminated fluorine-containing polyurethane prepolymer; (2) a fluorine-containing polyurethane prepolymer and a terminal hydroxyl liquid fluororubber are subjected to an addition polymerization reaction to obtain an isocyanate-terminated fluorine-containing polyurethane-fluororubber copolymer; (3) the fluorine-containing polyurethane-fluororubber copolymer and a curing agent are subjected to mold vulcanization under the condition of adding or not adding hydroxyl surface-modified polytetrafluoroethylene; the curing agent is a diamine and / or a diol. The polyurethane sealing material obtained by the method of the present invention avoids the attenuation of properties such as wear resistance, tensile strength, hardness, and tear strength under high temperature conditions, broadens the upper limit of the use temperature of the sealing material and the upper limit of the equipment speed, and realizes the improvement of the polyurethane sealing performance of the shield main drive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polyurethane sealing materials, and in particular relates to a preparation method and application of a shield main drive polyurethane sealing material. Background Art

[0002] The main drive seal of the shield machine is known as the "immune system" of the shield machine. Its main function is to prevent materials in the excavation chamber, such as sand, gravel, mud, and water, from entering the main bearing, so as to avoid damage to the main bearing and the inability of the shield machine to advance. At present, the main drive seal of the shield machine mainly adopts the structure of labyrinth + polyurethane finger seal + VD seal. The polyurethane finger seal has excellent oil resistance and high pressure bearing capacity, but when used under complex working conditions of high linear speed and high pressure, the friction heat generated by the lip is large, causing the seal temperature to rise quickly, and it is very easy to reach the limit use temperature of polyurethane, resulting in a significant attenuation of the material's wear resistance and mechanical properties, and an accelerated thermal aging rate, which seriously affects the material's performance and equipment construction efficiency.

[0003] The Chinese invention patent application with application publication number CN109593178A discloses a low-hardness, high-temperature resistant polyurethane elastomer material, which improves the high-temperature performance of polyurethane materials by using a large amount of raw materials containing rigid cyclohexyl structures. The high-temperature resistance of existing polyurethane sealing materials has been limited. The tensile strength, tear strength and pressure-dependent energy of the material at 90°C are seriously attenuated compared to 70°C. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a shield main drive polyurethane sealing material to solve the problem that the existing shield main drive polyurethane sealing has serious performance degradation such as wear resistance, tensile strength, hardness, tear strength, etc. under high temperature conditions.

[0005] The second object of the present invention is to provide the application of the material obtained by the above method as the main drive seal of the shield machine, so as to further improve the sealing performance of the equipment at high temperatures, and improve the service life of the material and the efficiency of the equipment.

[0006] In order to achieve the above purpose, the technical solution adopted by the present invention is:

[0007] A method for preparing a shield main drive polyurethane sealing material comprises the following steps:

[0008] (1) performing a polyaddition reaction between a fluorinated polyether diol and a diisocyanate to obtain an isocyanate-terminated fluorinated polyurethane prepolymer;

[0009] (2) a fluorinated polyurethane prepolymer and a hydroxyl-terminated liquid fluororubber are subjected to a polyaddition reaction to obtain an isocyanate-terminated fluorinated polyurethane-fluororubber copolymer;

[0010] (3) The fluorine-containing polyurethane-fluororubber copolymer and a curing agent are subjected to compression vulcanization with or without the addition of hydroxyl-surface-modified polytetrafluoroethylene; the curing agent is a diamine and / or a diol.

[0011] The preparation method of the shield main drive polyurethane sealing material provided by the present invention introduces fluorine-containing polyol and hydroxyl-containing fluororubber into polyurethane molecules, so that the use temperature of the polyurethane sealing composite material maintaining high performance is increased from 70°C to 90°C; the limit of the equipment speed on the use temperature of the seal is reduced, and the speed is increased from 0.7m / s to 1.5m / s, and the material has excellent water resistance, oil resistance, chemical medium resistance and mechanical strength. The polyurethane sealing material obtained by the method of the present invention avoids the attenuation of properties such as wear resistance, tensile strength, hardness, and tear strength under high temperature conditions, broadens the upper limit of the use temperature of the sealing material and the upper limit of the equipment speed, and realizes the improvement of the polyurethane sealing performance of the shield main drive.

[0012] To further improve the temperature resistance of the polyurethane seal, preferably, in step (1), the fluorinated polyether diol is a fluorinated polyether polyol ZDOL; the diisocyanate is an aromatic diisocyanate; the aromatic diisocyanate is selected from one or a combination of two or more of toluene diisocyanate T-80, toluene diisocyanate T-100, diphenylmethane diisocyanate, and 1,5-naphthalene diisocyanate; in step (2), the hydroxyl-terminated liquid fluororubber is a vinylidene fluoride-hexafluoropropylene copolymer elastomer or a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer elastomer.

[0013] Further preferably, in step (1), the number average molecular weight of the fluorinated polyether polyol ZDOL is 1000-4000 g / mol; the mass ratio of the fluorinated polyether polyol ZDOL and the aromatic diisocyanate is (1000-1200):(540-560); in step (2), the number average molecular weight of the hydroxyl-terminated liquid fluororubber is 4000-10000 g / mol; the mass ratio of the hydroxyl-terminated liquid fluororubber to the fluorinated polyether polyol ZDOL is (130-150):(1000-1200).

[0014] To further promote the efficient progress of the addition polymerization reaction, preferably, in step (1), the addition polymerization reaction uses dibutyltin dilaurate as a catalyst, and the addition polymerization reaction is carried out at 70-80°C for 2-3 hours; for every 1000-1200g of fluorinated polyether polyol ZDOL, the corresponding amount of dibutyltin dilaurate is 0.1-0.2mg; in step (2), the addition polymerization reaction uses dibutyltin dilaurate as a catalyst, and the addition polymerization reaction is carried out at 30-70°C for 2-3 hours; for every 130-150g of hydroxyl-terminated liquid fluororubber, the corresponding amount of dibutyltin dilaurate is 0.1-0.2mg.

[0015] To further improve the vulcanization rate and the temperature resistance of the material, preferably, in step (3), the diamine is 3,3'-dichloro-4,4'-diaminodiphenylmethane; the diol is 1,4-butanediol; and the mass ratio of 3,3'-dichloro-4,4'-diaminodiphenylmethane to 1,4-butanediol is 1:(1-1.5).

[0016] Preferably, in step (3), the temperature of the compression vulcanization is 120-130° C., the pressure is 12-15 MPa, and the time is 45 min to 50 min.

[0017] Preferably, the content of polytetrafluoroethylene in the shield main drive polyurethane sealing material changes gradually, and the shield main drive polyurethane sealing material has a friction contact end that contacts and moves relative to the contact object. The polytetrafluoroethylene content is high near the friction contact end, and the polytetrafluoroethylene content is low away from the friction contact end. Further preferably, the shield main drive polyurethane sealing material has a lip, and the lip forms the friction contact end; the shield main drive polyurethane sealing material is a finger-type seal or a lip-shaped seal structure. When used under complex working conditions of high linear speed and high pressure, the seal temperature rises rapidly due to the large amount of heat generated by friction at the lip. The above design can reduce the friction coefficient of the lip material and the amount of heat generated by friction at the lip, while the elasticity of the waist part is not affected, so it can effectively slow down the aging rate of the material, improve the service life of the material and the efficiency of equipment use.

[0018] In order to better achieve accurate and automatic addition of polytetrafluoroethylene and produce a composite material with gradual changes in self-lubricating and resilience properties, preferably, the fluorine-containing polyurethane-fluororubber copolymer component is pumped by injection pump A, the curing agent component is pumped by injection pump B, and the hydroxyl surface-modified polytetrafluoroethylene component is pumped by a powder delivery pump. After the three-component pumped materials are mixed, they are poured into a sealed mold for the compression vulcanization.

[0019] The material obtained by the above method is used as the main drive seal of the shield machine.

[0020] The polyurethane sealing material produced by the above method significantly improves the high temperature resistance of polyurethane sealing, effectively delays the aging rate of the material at high temperature, and improves the operational adaptability of the main drive seal of the shield machine. Through the gradual content design of polytetrafluoroethylene, a composite material with gradual self-lubricity and resilience can be prepared, which further improves the operational adaptability and is beneficial to improving the service life of the material and the equipment construction efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 is a distribution diagram of polytetrafluoroethylene content in the lip seal structure of the present invention;

[0022] Figure 2 This is a distribution diagram of the polytetrafluoroethylene content in the finger-shaped sealing structure of the present invention. DETAILED DESCRIPTION

[0023] In order to prepare a polyurethane sealing system with excellent properties such as high temperature resistance, oil resistance, self-lubrication, chemical medium resistance and mechanical strength, the present invention introduces three substances, namely, fluorine-containing polyol, hydroxyl-containing fluororubber and hydroxyl-containing polytetrafluoroethylene powder, into the polyurethane system, which not only realizes the copolymerization reaction of polyurethane and fluororubber, but also accurately adapts the addition amount of polytetrafluoroethylene according to the different positions of the sealing lip, thereby obtaining a shield main drive polyurethane sealing performance gradient composite material.

[0024] The idea of ​​preparing the shield main drive polyurethane sealing performance gradient composite material of the present invention is as follows:

[0025] Firstly, fluorinated polyol and isocyanate are used to prepare isocyanate-terminated fluorinated polyurethane prepolymer, which has excellent water resistance, oil resistance, chemical resistance and mechanical strength. Since fluororubber has excellent heat resistance and its long-term use temperature can reach 250°C, hydroxyl-containing fluororubber and polyurethane prepolymer are copolymerized to obtain fluorinated polyurethane-fluororubber copolymer, which improves the high temperature resistance of the material.

[0026] Secondly, in the polyurethane pouring control process, three quantitative feeding injection pumps A, injection pump B and powder conveying pumps are controlled by computer to control the addition amount of polyurethane prepolymer, curing agent and hydroxyl-containing polytetrafluoroethylene powder respectively. The three components are transported to the machine head for high-speed stirring and poured into the sealing mold. According to the different material finger types and lip-shaped sealing lip positions, the addition amount of polytetrafluoroethylene is accurately adapted to achieve precise adjustment of the friction coefficient between the sealing lip and the contact surface, and the friction coefficient between the sealing lip and the contact object is reduced while the elasticity of the waist part is not affected, the friction heat generated by the lip is reduced, and the aging rate of the material is effectively delayed. The use temperature of the composite material with gradual self-lubricity and resilience properties of the shield main drive polyurethane seal is increased from 70°C to 90°C, and the speed of the equipment equipped with the seal is increased from 0.7m / s to 1.5m / s, which effectively improves the service life of the material and the equipment construction efficiency, and reduces the procurement cost of the sealing strip.

[0027] Further, the preparation process of the material is as follows:

[0028] The first step is to synthesize the fluorinated polyurethane prepolymer: add fluorinated polyether diol to a reaction kettle equipped with a stirring rod, a thermometer, and a reflux condenser, and dehydrate under reduced pressure at a temperature of 110°C and a vacuum degree of -0.1MPa for 3 hours; add aromatic diisocyanate and a catalyst, dibutyltin dilaurate, to carry out an addition polymerization reaction to obtain an isocyanate-terminated fluorinated polyurethane prepolymer;

[0029] The second step is the synthesis of fluorinated polyurethane-fluororubber copolymer: add hydroxyl-terminated liquid fluororubber to the prepolymer obtained in the first step, then add catalyst dibutyltin dilaurate and mix evenly, obtain isocyanate-terminated fluorinated polyurethane-fluororubber copolymer after polyaddition reaction, adjust the equipment reaction vacuum degree to -0.1MPa, remove bubbles and set aside;

[0030] The third step: three quantitative feeding injection pumps A, B and powder delivery pumps are controlled by computer, fluorinated polyurethane prepolymer is added to injection pump A, 3,3'-dichloro-4,4'-diaminodiphenylmethane (MOCA) and 1,4-butanediol are loaded into injection pump B, and hydroxyl-containing polytetrafluoroethylene powder is loaded into the powder delivery pump (the injection amount of hydroxyl-containing polytetrafluoroethylene is intelligently adjusted according to the injection amount of injection pumps A and B). The three components are transported to the machine head for high-speed stirring and poured into the sealing mold, and the shield main drive polyurethane seal self-lubricating and resilience performance gradient composite material is obtained by compression vulcanization.

[0031] The first step is the polyaddition reaction process of fluorinated polyether diol and aromatic diisocyanate. The viscosity of the reaction system is not high, which is conducive to the synthesis of isocyanate-terminated polyurethane prepolymer. In this step, the aromatic diisocyanate is selected from one or more combinations of toluene diisocyanate T-80, toluene diisocyanate T-100, diphenylmethane diisocyanate, and 1,5-naphthalene diisocyanate. The fluorinated polyether diol is preferably a fluorinated polyether polyol ZDOL. More preferably, the Mn of the fluorinated polyether polyol ZDOL is 1000-4000 g / moL. The fluorinated polyether polyol ZDOL can be prepared according to the prior art (Research Progress of Fluorinated Polyether Polyols, Zhang Yingqiang, Polymer Bulletin, Issue 7, 2012, Section 1.1.1) to obtain a fluorinated polyether silicon-free oligomer with Mn=1000-4000 g / moL.

[0032] Preferably, the mass ratio of fluorinated polyether polyol ZDOL to aromatic diisocyanate is (1000-1200):(540-560). The mass ratio of fluorinated polyether polyol ZDOL to dibutyltin dilaurate is (1000-1200) g:(0.1-0.2) mg.

[0033] Preferably, the isocyanate content of the obtained isocyanate-terminated fluorinated polyurethane prepolymer is 3-8%.

[0034] The second step is the preparation process of isocyanate-terminated fluorinated polyurethane-fluororubber copolymer. In this step, the hydroxyl-terminated liquid fluororubber is a low relative molecular mass vinylidene fluoride (VDF)-hexafluoropropylene (HFP) or VDF-HFP-tetrafluoroethylene (TFE) copolymer elastomer. The low relative molecular mass is preferably 4000-10000. Liquid fluororubbers with different hydroxyl termini can be prepared with reference to the prior art (Preparation of liquid hydroxyl-terminated fluororubber by NaBH4 / LaCl3 reduction system, Li Donghan, Journal of Shenyang University of Chemical Technology, Vol. 35, No. 1, 2021.).

[0035] Preferably, the mass ratio of the hydroxyl-terminated liquid fluororubber to the fluorinated polyether polyol ZDOL is (130-150): (1000-1200). The mass ratio of the hydroxyl-terminated liquid fluororubber to dibutyltin dilaurate is (130-150) g: (0.1-0.2) mg.

[0036] The fluorine content of the isocyanate-terminated fluorinated polyurethane-fluororubber copolymer is 4.0-12%.

[0037] The third step is the preparation process of the polyurethane sealing material. This method can be used to achieve accurate and automatic addition of polytetrafluoroethylene powder. Among them, the hydroxyl group in the hydroxyl surface-modified polytetrafluoroethylene is a reactive group that can react with an isocyanate group. The hydroxyl surface-modified polytetrafluoroethylene can be prepared using commercial products or according to existing technologies (such as chemical methods represented by sodium-naphthalene treatment liquid, radiation grafting modification methods, etc.) to make the surface of the polytetrafluoroethylene contain hydroxyl groups. The particle size of the hydroxyl surface-modified polytetrafluoroethylene powder is 1 to 5 μm.

[0038] The content of polytetrafluoroethylene powder is the highest at the lip, which can reach 18%, and the content is the lowest at the position far from the lip, which can be as low as 0%. The compression vulcanization temperature is 110-130°C, the pressure is 12-15MPa, and the time is 45min-75min. More preferably, the temperature is 120-130°C, the pressure is 12-15MPa, and the time is 45min-50min.

[0039] The implementation process of the present invention is further described below in conjunction with specific embodiments.

[0040] 1. Specific embodiment of the method for preparing the shield main drive polyurethane sealing material of the present invention

[0041] Example 1

[0042] The method for preparing the shield main drive polyurethane sealing material of this embodiment comprises the following steps:

[0043] (1) Add fluorinated polyether diol to a reaction kettle equipped with a stirring rod, a thermometer, and a reflux condenser, and dehydrate under reduced pressure at a temperature of 110° C. and a vacuum degree of −0.1 MPa for 3 h; after the temperature drops to 70° C., add aromatic diisocyanate and a catalyst, dibutyltin dilaurate, and react for 2.5 h to obtain an isocyanate-terminated fluorinated polyurethane prepolymer.

[0044] The fluorinated polyether diol is specifically a fluorinated polyether polyol ZDOL, and the number average molecular weight is 4000 g / mol.

[0045] The aromatic diisocyanate is specifically T-80.

[0046] The amount of fluorinated polyether diol added was 1000 g, the amount of aromatic diisocyanate added was 540 g, the amount of dibutyltin dilaurate added was 0.2 mg, and the content of isocyanate in the obtained fluorinated polyurethane prepolymer was 5.5%.

[0047] (2) Add hydroxyl-terminated liquid fluororubber to the prepolymer, then add catalyst dibutyltin dilaurate and mix well. After reacting at 70°C for 3 hours, an isocyanate-terminated fluorinated polyurethane-fluororubber copolymer is obtained. The equipment reaction vacuum is adjusted to -0.1 MPa, and bubbles are removed for standby use.

[0048] In this step, the hydroxyl-terminated liquid fluororubber is a VDF-HFP copolymer elastomer with a number average molecular weight of 4000 g / mol. The amount of the hydroxyl-terminated liquid fluororubber added is 130 g. The amount of dibutyltin dilaurate added is 0.2 mg.

[0049] The fluorine content of the isocyanate terminated fluorinated polyurethane-fluororubber copolymer is 4.0%.

[0050] (3) Three quantitative feeding injection pumps A, B and powder delivery pumps are controlled by computer, fluorinated polyurethane prepolymer is added to injection pump A, 3,3'-dichloro-4,4'-diaminodiphenylmethane (MOCA) and 1,4-butanediol are loaded into injection pump B, and hydroxyl-containing polytetrafluoroethylene powder is loaded into the powder delivery pump (the injection amount of hydroxyl-containing polytetrafluoroethylene is intelligently adjusted according to the injection amount of injection pumps A and B). The three components are transported to the machine head for high-speed stirring and poured into the sealing mold, and the shield main drive polyurethane seal self-lubricating and rebound elasticity gradient composite material is obtained by compression vulcanization. The compression vulcanization temperature is 120℃, the pressure is 12MPa, and the time is 45min.

[0051] In this step, the mass ratio of MOCA to 1,4-butanediol is 1:1. The reason for adopting this ratio is that MOCA can improve the rigidity of the material, and 1,4-butanediol can improve the flexibility of the material, thus taking into account both the rigidity and flexibility of the material.

[0052] This step produces a lip seal, and the sealing structure diagram is shown in Figure 1 As shown, the content of polytetrafluoroethylene gradually decreases in the front-to-back direction from the lip end to the mounting end. Figure 1 The color depth shows the change of PTFE content. The closer to the lip, the darker the color of the area, indicating that the content of PTFE in the polyurethane composite material is higher. Specifically, the PTFE content at the lip on the front side is the highest, reaching 16%, while the PTFE content of the sealing material on the rear side is 0%.

[0053] In other implementation situations of this embodiment, the following can be obtained: Figure 2 The finger seal structure shown in the figure shows the trend of the change of PTFE content. Figure 1 same.

[0054] Example 2

[0055] The method for preparing the shield main drive polyurethane sealing material of this embodiment is different from the method of Example 1 in that:

[0056] In step (1), the fluorinated polyether diol is fluorinated polyether polyol ZDOL, and the number average molecular weight is 4000 g / mol. The aromatic diisocyanate is T-100, and the reaction conditions are 70° C. and 2.5 h.

[0057] In step (3), the mass ratio of MOCA to 1,4-butanediol is 1:1.5. In the sealing structure, the content of polytetrafluoroethylene changes gradually, with a maximum of 16% and a minimum of 0%. The temperature of the compression vulcanization is 120°C, the pressure is 13 MPa, and the time is 50 minutes.

[0058] Example 3

[0059] The method for preparing the shield main drive polyurethane sealing material of this embodiment is different from the method of Example 1 in that:

[0060] In step (1), the fluorinated polyether diol is fluorinated polyether polyol ZDOL, and the number average molecular weight is 4000 g / mol. The aromatic diisocyanate is T-100. The reaction conditions are 70° C. and 2.5 h.

[0061] In step (3), the mass ratio of MOCA to 1,4-butanediol is 1:1. In the sealing structure, the content of polytetrafluoroethylene changes gradually, with a maximum of 18% and a minimum of 0%. The temperature of the compression vulcanization is 130°C, the pressure is 14 MPa, and the time is 50 minutes.

[0062] Example 4

[0063] The method for preparing the shield main drive polyurethane sealing material of this embodiment is different from the method of Example 1 in that:

[0064] In step (1), the fluorinated polyether diol is fluorinated polyether polyol ZDOL, and the number average molecular weight is 4000 g / mol. The aromatic diisocyanate is T-100. The reaction conditions are 70° C. and 2.5 h.

[0065] In step (3), the mass ratio of MOCA to 1,4-butanediol is 1:1.5. In the sealing structure, the content of polytetrafluoroethylene changes gradually, with a maximum of 18% and a minimum of 0%. The temperature of the compression vulcanization is 130°C, the pressure is 14 MPa, and the time is 50 minutes.

[0066] 2. Application of composite materials with gradual changes in self-lubricity and resilience of polyurethane seals for main drive of shield machines

[0067] This experimental example tests various properties of the obtained polyurethane sealing material, and the test standards and results of each property are listed in Table 1. In the following examples, the samples represented by Examples 1 to 4 are polyurethane sealing materials with a constant tetrafluoroethylene content of 16% prepared in the manner of Examples 1 to 4. The comparative example is P1038 of Beijing Jianke Huifeng Technology Co., Ltd.

[0068] Table 1 Performance indicators of polyurethane sealing materials

[0069]

[0070] Based on the above experimental contents, it can be known that the operating temperature of the polyurethane sealing composite material prepared by the above technical scheme to maintain high performance is increased from 70°C to 90°C; on this basis, the limit of the equipment speed on the sealing operating temperature can be reduced, and the speed is increased from 0.7m / s to 1.5m / s, which improves the service life of the material and the equipment construction efficiency, and is conducive to reducing the replacement frequency of sealing materials and reducing the procurement cost of sealing materials.

Claims

1. A method for preparing a shield main drive polyurethane sealing material, It is characterized in that The following steps are involved: (1) A fluorinated polyether diol and a diisocyanate are subjected to a polycondensation reaction to obtain an isocyanate-terminated fluorinated polyurethane prepolymer; (2) The fluorinated polyurethane prepolymer and the hydroxyl-terminated liquid fluororubber are subjected to polycondensation reaction to obtain an isocyanate-terminated fluorinated polyurethane-fluororubber copolymer; (3) vulcanizing the fluorine-containing polyurethane-fluororubber copolymer and the curing agent under the condition of adding hydroxyl surface-modified polytetrafluoroethylene; the curing agent is a diamine and / or a diol; The fluorine-containing polyurethane-fluororubber copolymer component is pumped by injection pump A, the curing agent component is pumped by injection pump B, and the hydroxyl surface-modified polytetrafluoroethylene component is pumped by a powder delivery pump. The three pumped materials are mixed and poured into a sealed mold for the molding vulcanization; the injection amount of the hydroxyl-containing polytetrafluoroethylene is adjusted according to the injection amount of the injection pumps A and B; The content of polytetrafluoroethylene in the shield main drive polyurethane sealing material gradually changes. The shield main drive polyurethane sealing material has a friction contact end that contacts and moves relative to a contact object. The polytetrafluoroethylene content is high near the friction contact end and low far from the friction contact end.

2. The method for preparing the shield main drive polyurethane sealing material according to claim 1, It is characterized in that In step (1), the fluorinated polyether diol is a fluorinated polyether polyol ZDOL; the diisocyanate is an aromatic diisocyanate; the aromatic diisocyanate is selected from one or a combination of two or more of toluene diisocyanate T-80, toluene diisocyanate T-100, diphenylmethane diisocyanate, and 1,5-naphthalene diisocyanate; in step (2), the hydroxyl-terminated liquid fluororubber is a vinylidene fluoride-hexafluoropropylene copolymer elastomer or a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer elastomer.

3. The method for preparing the shield main drive polyurethane sealing material according to claim 2, It is characterized in that In step (1), the number average molecular weight of the fluorinated polyether polyol ZDOL is 1000-4000 g / mol; the mass ratio of the fluorinated polyether polyol ZDOL and the aromatic diisocyanate is (1000-1200):(540-560); in step (2), the number average molecular weight of the hydroxyl-terminated liquid fluororubber is 4000-10000 g / mol; the mass ratio of the hydroxyl-terminated liquid fluororubber to the fluorinated polyether polyol ZDOL is (130-150):(1000-1200).

4. The method for preparing the shield main drive polyurethane sealing material according to claim 3, It is characterized in that In step (1), the polycondensation reaction uses dibutyltin dilaurate as a catalyst, and the polycondensation reaction is carried out at 70-80°C for 2-3 hours; for every 1000-1200g of fluorinated polyether polyol ZDOL, the corresponding amount of dibutyltin dilaurate is 0.1-0.2mg; in step (2), the polycondensation reaction uses dibutyltin dilaurate as a catalyst, and the polycondensation reaction is carried out at 30-70°C for 2-3 hours; for every 130-150g of hydroxyl-terminated liquid fluororubber, the corresponding amount of dibutyltin dilaurate is 0.1-0.2mg.

5. The method for preparing the shield main drive polyurethane sealing material according to claim 1, It is characterized in that In step (3), the diamine is 3,3'-dichloro-4,4'-diaminodiphenylmethane; the diol is 1,4-butanediol; and the mass ratio of 3,3'-dichloro-4,4'-diaminodiphenylmethane to 1,4-butanediol is 1:(1-1.5).

6. The method for preparing the shield main drive polyurethane sealing material according to claim 1, It is characterized in that In step (3), the temperature of the compression vulcanization is 120-130° C., the pressure is 12-15 MPa, and the time is 45 min-50 min.

7. The method for preparing the shield main drive polyurethane sealing material according to claim 1, It is characterized in that The shield main drive polyurethane sealing material has a lip, and the lip forms the friction contact end; the shield main drive polyurethane sealing material is a finger-type seal or a lip-shaped seal structure.

8. Use of the material obtained by the preparation method according to any one of claims 1 to 7 as a main drive seal for a shield machine.