A kind of low oxygen silicon carbide fiber and preparation method thereof

By using cyano-containing polycarbosilane as raw material, avoiding air non-melting treatment, drying and high-temperature sintering with an inert atmosphere, successfully reducing the oxygen content of silicon carbide fibers, solving the problem of excessive oxygen content, simplifying the process and reducing costs , and also give fiber functional properties.

CN115573056BActive Publication Date: 2024-11-26QIANWAN INST OF CNITECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211181090.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-27
Publication Date
2024-11-26
Estimated Expiration
2042-09-27

AI Technical Summary

Technical Problem

During the preparation process of existing silicon carbide fibers, the non-melting treatment of air leads to excessive oxygen content, resulting in damage to the fiber structure and degradation of mechanical properties. The existing methods to reduce oxygen content are complex and costly.

Method used

Use cyano-containing polycarbosilane as raw material to prepare low-oxygen silicon carbide fibers through spinning, drying and heat curing and high-temperature sintering processes to avoid air non-melting treatment. Use an inert atmosphere to dry and high-temperature sintering. When heterogeneous elements are contained, Further reduce the oxygen content.

Benefits of technology

The oxygen content of silicon carbide fibers is successfully reduced to <3%, simplifying the process, reducing costs, and giving fibers functional properties such as wave absorption and electromagnetic shielding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115573056B_ABST
    Figure CN115573056B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of silicon carbide fiber preparation, and relates to a low-oxygen silicon carbide fiber and a preparation method thereof. The low-oxygen silicon carbide fiber is prepared from cyano-containing polycarbosilane as a raw material through spinning, drying, heat curing and high-temperature sintering. The cyano-containing polycarbosilane is a molecular main chain containing CH 3 HS 2 The compound whose structural unit and molecular branch chain contain ‑C≡N. The present invention uses cyano-containing polycarbosilane as raw material through spinning, drying, heat curing and high-temperature sintering processes to prepare low-oxygen silicon carbide fiber, which has the advantages of simple process and low cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of silicon carbide fiber preparation, and relates to low-oxygen silicon carbide fiber and a preparation method thereof. Background Art

[0002] Silicon carbide (SiC) fibers are widely used in high-tech fields such as aerospace, nuclear energy, etc. due to their high temperature resistance, oxidation resistance, corrosion resistance and excellent mechanical properties. The precursor conversion method is currently the main method for preparing SiC fibers. Its basic process is roughly divided into the following four steps: precursor synthesis, spinning, infusibility, high-temperature firing and sintering. Air infusibility is a common infusibility method. In this process, a large amount of oxygen is introduced into the fiber (usually more than 10%) to form a SiOxCy phase. Above 1200°C, the SiOxCy phase decomposes under heat, releasing CO and SiO gases, resulting in damage to the fiber structure and a sharp drop in mechanical properties.

[0003] In order to reduce the oxygen content in SiC fibers, Okamura et al. (J.Am.Ceram.Soc., 1995, 78: 1013-1017) of Japan used electron beam irradiation in an inert atmosphere to treat polycarbosilane (PCS) fibrils to make them infusible, and obtained SiC fibers with an oxygen content of less than 0.5%. The fibers can still maintain a tensile strength of 2.0 GPa after being treated in argon at 1500°C for 1 hour. Japan Carbon Company has industrialized the development of this technology and produced a new type of low-oxygen SiC fiber in 1995, with the trade name Hi-Nicalon. However, this method greatly increases the preparation cost of SiC fibers. The dry spinning method is to dissolve the high molecular weight part of PCS after graded treatment in an appropriate solvent, add spinning aids, and dry-spin into fibers. Without infusible treatment, heat treatment is directly performed at high temperature to obtain SiC fibers with an oxygen content of about 2% (Compos. Sci. Technol., 1994, 51: 145-159). However, the graded precipitation method involved in this technology is relatively complicated and not easy to prepare on a large scale. In addition, methods for reducing the oxygen content of SiC fibers also include gamma ray irradiation, chemical vapor crosslinking, etc., which undoubtedly increase costs. The Chinese invention patent with application number CN201711193380.5 discloses a submicron / nano oxygen-free silicon carbide fiber felt and a preparation method thereof: a polycarbosilane with a weight average molecular weight greater than 4000 is subjected to a non-good solvent to remove small molecules to obtain a high molecular weight polycarbosilane with a weight average molecular weight greater than 8000, and then the spinning solution of the high molecular weight polycarbosilane, a spinning aid polymer and an organic solvent is subjected to electrostatic spinning, and then subjected to a temperature-increasing heat treatment and high-temperature pyrolysis to obtain a submicron / nano oxygen-free silicon carbide fiber felt. The Chinese invention patent with application number CN201810035177.3 synthesizes a vinyl-containing polycarbosilane with thermosetting properties by a silane-hydrogen addition reaction of polycarbosilane and a vinyl-containing silane, and then dry-spins to obtain a polycarbosilane fiber, which is then subjected to a heat treatment and high-temperature pyrolysis to obtain a low-oxygen silicon carbide fiber. The preparation process of the precursors used in these technologies is relatively complex. Summary of the invention

[0004] The object of the present invention is to provide a low-oxygen silicon carbide fiber and a preparation method thereof in view of the deficiencies in the prior art.

[0005] The aforementioned object of the present invention is achieved by the following technical solutions:

[0006] A low-oxygen silicon carbide fiber is prepared from cyano-containing polycarbosilane through spinning, drying, heat curing and high-temperature sintering processes.

[0007] Preferably, the cyano-containing polycarbosilane is a compound having a main molecular chain containing CH3SiHCH2 structural units and a molecular side chain containing -C≡N.

[0008] Preferably, the cyano-containing polycarbosilane has a softening point greater than 250° C. and a weight average molecular weight greater than 4000 g / mol.

[0009] Preferably, the cyano-containing polycarbosilane contains heterogeneous elements, and the heterogeneous elements include one or more of aluminum, iron, titanium, zirconium, cobalt, nickel, boron, lanthanum, yttrium, and niobium. When the cyano-containing polycarbosilane contains heterogeneous elements, using it as a raw material to prepare silicon carbide fibers can more effectively reduce the oxygen content in the silicon carbide fibers. The content of heterogeneous elements in the cyano-containing polycarbosilane is not limited, and any content of heterogeneous elements is within the protection scope of this application.

[0010] The raw material used in the present invention contains cyanopolycarbosilane, which can be prepared by referring to the method of patent CN109354691.

[0011] Preferably, the low-oxygen silicon carbide fibers are not subjected to an air infusibility treatment process.

[0012] Air infusibility treatment is a heating treatment in an air atmosphere. Air infusibility treatment is a common process in the preparation of silicon carbide fibers. However, a large amount of oxygen will be introduced during the air infusibility treatment, which will cause the performance of silicon carbide fibers to drop sharply at high temperatures. The present invention uses cyano-containing polycarbosilane as a raw material, and does not need to go through the air infusibility treatment process. Silicon carbide fibers can be prepared directly through spinning, drying, heat curing and high-temperature sintering processes, and the prepared silicon carbide fibers have a low oxygen content, which is less than 3%.

[0013] Another object of the present invention is achieved by the following technical solution:

[0014] A method for preparing low-oxygen silicon carbide fiber, the method comprising the following steps: dissolving cyano-containing polycarbosilane in an organic solvent to prepare a spinning solution; spinning the spinning solution to obtain cyano-containing polycarbosilane fiber; heating the cyano-containing polycarbosilane fiber in an inert atmosphere to dry and heat-cure it; and calcining the dried and heat-cured fiber at a high temperature in an inert atmosphere to obtain the low-oxygen silicon carbide fiber.

[0015] Preferably, the organic solvent consists of a good solvent and a poor solvent.

[0016] Preferably, the good solvent is one or more of toluene, xylene, tetrahydrofuran, n-hexane, and chloroform, and the poor solvent is one or more of ethanol, n-propanol, isopropanol, acetone, dimethylformamide, and ethyl formate.

[0017] Preferably, the mass ratio of cyano-containing polycarbosilane, good solvent, and poor solvent is 40-65:30-55:5-25.

[0018] Preferably, the spinning is electrospinning or dry spinning.

[0019] Preferably, when the spinning is electrospinning, the process conditions of the electrospinning include: the inner diameter of the spinneret is 0.3-2 mm, the spinning voltage is 10-25 kV, the distance between the spinneret and the collector is 10-25 cm, and the feed rate is 10-35 μL / min.

[0020] Preferably, when the spinning is dry spinning, the process conditions of the dry spinning include: under the protection of an inert atmosphere, raising the spinning solution to 50-150° C. in a spinning device, keeping it warm for 0.5-5 hours, and ejecting it through a spinneret hole with an inert gas or a metering pump to form cyano-containing polycarbosilane fibers.

[0021] Preferably, the drying heat curing conditions include: heating to 250-280°C at 0.5-2°C / min in an inert atmosphere, then heating to 280-350°C at 0.2-1.0°C / min, and keeping at this temperature for 0.5-2h. The present invention does not use the air infusibility treatment process, but heats in an inert atmosphere for drying and curing.

[0022] Preferably, the high temperature sintering conditions include: heating to 1000°C-1800°C at 2-10°C / min under an inert atmosphere, and keeping at this temperature for 0.5-2h.

[0023] The inert atmosphere herein includes, but is not limited to, argon atmosphere and nitrogen atmosphere.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] (1) The present invention uses cyano-containing polycarbosilane as a raw material, and through spinning, drying, heat curing and high-temperature sintering processes, low-oxygen silicon carbide fibers with an oxygen content of less than 3% can be prepared;

[0026] (2) In the preparation process of the silicon carbide fiber of the present invention, the air infusibility treatment process is not used, but dry heat curing is carried out in an inert atmosphere. The dry heat curing conditions are to increase the temperature to 250°C-280°C at 0.5-2°C / min in an inert atmosphere, and then increase the temperature to 280°C-350°C at 0.2-1.0°C / min, and keep the temperature at this temperature for 0.5-2h, thereby avoiding the introduction of a large amount of oxygen;

[0027] (3) When cyano-containing polycarbosilane contains heterogeneous elements, using it as a raw material to prepare silicon carbide fibers can more effectively reduce the oxygen content in the silicon carbide fibers and give the silicon carbide fibers certain functional properties, such as wave absorption and electromagnetic shielding;

[0028] (4) Compared with the prior art, the method for preparing low-oxygen silicon carbide fiber of the present invention has simpler process and lower cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 (a) and (b) are SEM photos of SiC fiber 1 in Example 1 of the present invention. Figure 1 (c) is a SEM photo of SiC fiber 1 in Example 1 of the present invention after being kept at 1400°C for 1 hour. Figure 1 (d) is a SEM photograph of SiC fiber 1 in Example 1 of the present invention after being kept at a constant temperature of 1600° C. for 1 hour. DETAILED DESCRIPTION

[0030] The technical scheme of the present invention is further described below by specific examples and accompanying drawings. It should be understood that the specific examples described herein are only used to help understand the present invention and are not intended for specific limitations of the present invention. The accompanying drawings used herein are only for better illustrating the disclosure of the present invention and do not have a limiting effect on the scope of protection. If not otherwise specified, the raw materials used in the embodiments of the present invention are all commonly used raw materials in the art, and the methods used in the embodiments are all conventional methods in the art.

[0031] 1. Preparation of cyano-containing polycarbosilane PCS-CN01

[0032] Take 50g of polycarbosilane (PCS) (softening point 250℃, weight average molecular weight 3820g / mol) and dissolve it in 60g of tetrahydrofuran (THF). After complete dissolution, add it to a 250ml flask, add 10g of acrylonitrile, add 0.003g of Wilkinson catalyst under nitrogen protection, and then heat the reaction system to 60℃ for 8h. Finally, remove THF by vacuum distillation to obtain cyano-containing polycarbosilane PCS-CN01.

[0033] After testing, the softening point of PCS-CN01 is 255°C and the weight average molecular weight is 4120 g / mol.

[0034] Example 1

[0035] The method for preparing the silicon carbide fiber of this embodiment is as follows:

[0036] Take 5.5g of PCS-CN01 precursor, add 3.6g of xylene and 0.9g of acetone respectively to prepare a spinning solution;

[0037] Then, electrospinning was performed to obtain PCS-CN01 fibers. The spinning conditions were as follows: the inner diameter of the spinneret was 0.8 mm, the spinning voltage was 16 kV, the distance between the spinneret and the collector was 15 cm, and the feed rate was 30 μL / min.

[0038] The PCS-CN01 fiber was placed in a tube furnace and heated to 250°C at 2°C / min under argon atmosphere, then heated to 300°C at 0.5°C / min and kept at this temperature for 1h for drying and thermal curing.

[0039] The dried and heat-cured fiber was placed in a high-temperature furnace, and under the protection of an argon atmosphere, the temperature was raised to 1200° C. at a rate of 2° C. / min, and kept at this temperature for 2 h, thereby obtaining SiC fiber 1.

[0040] According to the test, the oxygen content of SiC fiber 1 is 2.2%.

[0041] Figure 1 (a) and (b) are SEM photos of SiC fiber 1 in Example 1 of the present invention; Figure 1 (c) is the SEM image of SiC fiber 1 kept at 1400℃ for 1h; Figure 1 (d) is a SEM photo of SiC fiber 1 kept at 1600°C for 1 h. It can be seen that due to the low oxygen content of SiC fiber 1, the fiber structure can still remain intact without pores when kept at 1600°C for 1 h.

[0042] Example 2

[0043] The method for preparing the silicon carbide fiber of this embodiment is as follows:

[0044] Take 20g of PCS-CN01 precursor, add 10g of xylene and 3g of acetone respectively to prepare a spinning solution;

[0045] Then, dry spinning was performed to obtain PCS-CN02 fibers. The dry spinning conditions were as follows: under the protection of argon atmosphere, the spinning solution was heated to 80°C in the spinning device, kept warm for 0.5h, and argon gas was used to spray it through the spinneret hole. The argon gas pressure was 0.3MPa.

[0046] The PCS-CN02 fiber was placed in a tubular furnace and heated to 250°C at 2°C / min under argon atmosphere, then heated to 300°C at 0.5°C / min and kept at this temperature for 1h for drying and thermal curing.

[0047] The dried and heat-cured fiber was placed in a high-temperature furnace, and under the protection of an argon atmosphere, the temperature was raised to 1200° C. at a rate of 2° C. / min, and kept at this temperature for 2 h, thereby obtaining SiC fiber 2.

[0048] According to the test, the oxygen content of the SiC fiber 2 is 2.3%.

[0049] 2. Preparation of cyano-containing polyaluminocarbosilane PACS-CN01

[0050] Take 50g of aluminum-containing polycarbosilane (PACS) (softening point 260℃, weight average molecular weight 4130g / mol, aluminum content 1wt%) and dissolve it in 60g of tetrahydrofuran (THF). After complete dissolution, add it to a 250ml flask, add 10g of acrylonitrile, add 0.5g of azobisisobutyronitrile catalyst under nitrogen protection, and then heat the reaction system to 60℃ for 15h. Finally, remove THF by vacuum distillation to obtain cyano-containing polyaluminocarbosilane PACS-CN01.

[0051] After testing, the softening point of PACS-CN01 is 267°C and the weight average molecular weight is 4250 g / mol.

[0052] Embodiment 3:

[0053] The method for preparing the silicon carbide fiber of this embodiment is as follows:

[0054] Take 5.5g of PACS-CN01 precursor, add 4g of tetrahydrofuran and 1g of n-propanol respectively to prepare a spinning solution;

[0055] Then, electrospinning was performed to obtain PACS-CN01 fibers. The spinning conditions were as follows: the inner diameter of the spinneret was 0.8 mm, the spinning voltage was 18 kV, the distance between the spinneret and the collector was 15 cm, and the feed rate was 25 μL / min.

[0056] The PACS-CN01 fiber was placed in a tube furnace and heated to 260°C at 2°C / min under argon atmosphere, then heated to 290°C at 0.5°C / min and kept at this temperature for 1h for drying and heat curing.

[0057] The dried and heat-cured fiber was placed in a high-temperature furnace, and under the protection of an argon atmosphere, the temperature was raised to 1800° C. at a rate of 2° C. / min, and kept at this temperature for 1 hour, thereby obtaining SiC fiber 3.

[0058] According to the test, the oxygen content of SiC fiber 3 is 0.5%.

[0059] Example 4

[0060] The method for preparing the silicon carbide fiber of this embodiment is as follows:

[0061] Take 20g of PACS-CN01 precursor, add 12g of tetrahydrofuran and 3g of ethanol respectively to prepare a spinning solution;

[0062] Then, dry spinning was performed to obtain PACS-CN02 fibers. The dry spinning conditions were as follows: under the protection of argon atmosphere, the spinning solution was heated to 75°C in the spinning device, kept warm for 0.5h, and argon gas was used to spray it through the spinneret hole. The argon gas pressure was 0.2MPa.

[0063] The PACS-CN02 fiber was placed in a tube furnace and heated to 262°C at 2°C / min under argon atmosphere, then heated to 290°C at 0.5°C / min and kept at this temperature for 1h for drying and heat curing.

[0064] The dried and heat-cured fiber was placed in a high-temperature furnace, and under the protection of an argon atmosphere, the temperature was raised to 1800° C. at a rate of 2° C. / min, and kept at this temperature for 1 hour to obtain SiC fiber 4.

[0065] According to the test, the oxygen content of the SiC fiber 4 is 0.4%.

[0066] 3. Preparation of cyano-containing polyferrocarbosilane PFCS-CN01

[0067] Take 50g of iron-containing polycarbosilane (PFCS) (softening point 265℃, weight average molecular weight 4190g / mol, iron content 0.5wt%) and dissolve it in 60g of tetrahydrofuran (THF). After complete dissolution, add it to a 250ml flask, add 10g of acrylonitrile, add 0.5g of azobisisobutyronitrile catalyst under nitrogen protection, and then heat the reaction system to 60℃ for 20h. Finally, remove THF by vacuum distillation to obtain cyano-containing polyferrocarbosilane PFCS-CN01.

[0068] After testing, the softening point of PFCS-CN01 is 272°C and the weight average molecular weight is 4330 g / mol.

[0069] Example 5

[0070] The method for preparing the silicon carbide fiber of this embodiment is as follows:

[0071] Take 5.5g of PFCS-CN01 precursor, add 4.5g of n-hexane and 1.5g of dimethylformamide respectively to prepare a spinning solution;

[0072] Then, PFCS-CN01 fibers were obtained by electrospinning. The spinning conditions were as follows: the inner diameter of the spinneret was 0.8 mm, the spinning voltage was 20 kV, the distance between the spinneret and the collector was 15 cm, and the feed rate was 20 μL / min.

[0073] The PFCS-CN01 fiber was placed in a tube furnace and heated to 265°C at 2°C / min under argon atmosphere, then heated to 295°C at 0.5°C / min and kept at this temperature for 1h for drying and thermal curing.

[0074] The dried and heat-cured fiber was placed in a high-temperature furnace, and under the protection of an argon atmosphere, the temperature was raised to 1600° C. at a rate of 2° C. / min, and kept at this temperature for 1.5 h, thereby obtaining SiC fiber 5.

[0075] According to the test, the oxygen content of the SiC fiber 5 is 1.8%.

[0076] Example 6

[0077] The method for preparing the silicon carbide fiber of this embodiment is as follows:

[0078] Take 20g of PFCS-CN01 precursor, add 14g of n-hexane and 4g of dimethylformamide respectively to prepare a spinning solution;

[0079] Then, dry spinning was performed to obtain PFCS-CN02 fibers. The dry spinning conditions were as follows: under the protection of argon atmosphere, the spinning solution was heated to 70°C in the spinning device, kept warm for 0.5h, and argon gas was used to spray it through the spinneret hole. The argon gas pressure was 0.3MPa.

[0080] The PFCS-CN02 fiber was placed in a tubular furnace and heated to 265°C at 2°C / min under argon atmosphere, then heated to 295°C at 0.5°C / min and kept at this temperature for 1h for drying and thermal curing.

[0081] The dried and heat-cured fiber was placed in a high-temperature furnace, and under the protection of an argon atmosphere, the temperature was raised to 1700°C at a rate of 2°C / min, and kept at this temperature for 1.5 hours to obtain SiC fiber 6.

[0082] According to the test, the oxygen content of the SiC fiber 6 is 1.1%.

[0083] Comparative Example 1

[0084] The preparation method of silicon carbide fiber of Comparative Example 1 is as follows:

[0085] Take 5.5 g of polycarbosilane (PCS) (softening point 250°C, weight average molecular weight 3820 g / mol), add 3.6 g of xylene and 0.9 g of acetone respectively to prepare a spinning solution;

[0086] Then, electrospinning was performed to obtain PCS01 fibers. The spinning conditions were as follows: the inner diameter of the spinneret was 0.8 mm, the spinning voltage was 16 kV, the distance between the spinneret and the collector was 15 cm, and the feed rate was 30 μL / min.

[0087] Put the PCS01 fiber into a tube furnace, and heat it to 210℃ at 0.5℃ / min under air atmosphere protection, and keep it at this temperature for 8h to dry and infusible in air;

[0088] The air-infusible fiber was placed in a high-temperature furnace, and under the protection of an argon atmosphere, the temperature was raised to 1200°C at a rate of 2°C / min, and kept at this temperature for 2 hours to obtain SiC fiber 7.

[0089] According to the test, the oxygen content of the SiC fiber 7 is 12.5%.

[0090] The various aspects, embodiments, and features of the present invention should be considered to be illustrative in all aspects and not limiting of the present invention, the scope of which is defined solely by the claims. Other embodiments, modifications, and uses will be apparent to those skilled in the art without departing from the spirit and scope of the claimed invention.

[0091] The use of headings and sections in this disclosure is not meant to limit the disclosure; each section may apply to any aspect, embodiment, or feature of the disclosure.

[0092] Finally, it should be noted that the specific embodiments described herein are merely examples of the present invention, and are not intended to limit the implementation methods of the present invention. A person skilled in the art of the present invention may make various modifications or supplements to the specific embodiments described, or replace them in a similar manner. It is not necessary and impossible to provide all examples of all implementation methods here. However, these obvious changes or modifications derived from the essential spirit of the present invention still fall within the scope of protection of the present invention, and interpreting them as any additional limitation is contrary to the spirit of the present invention.

Claims

1. A method for preparing low-oxygen silicon carbide fiber, It is characterized in that The preparation method comprises the following steps: dissolving cyano-containing polycarbosilane in an organic solvent to prepare a spinning solution; spinning the spinning solution to obtain cyano-containing polycarbosilane fibers; heating the cyano-containing polycarbosilane fibers in an inert atmosphere to perform drying and thermal curing; and calcining the dried and thermally cured fibers at a high temperature in an inert atmosphere to obtain low-oxygen silicon carbide fibers; The cyano-containing polycarbosilane has a molecular main chain containing CH 3 HS 2 Compounds whose structural units and molecular branches contain -C≡N; The organic solvent consists of a good solvent and a poor solvent; the good solvent is one or more of toluene, xylene, tetrahydrofuran, n-hexane, and chloroform, and the poor solvent is one or more of ethanol, n-propanol, isopropanol, acetone, dimethylformamide, and ethyl formate.

2. The preparation method according to claim 1, It is characterized in that The cyano-containing polycarbosilane has a softening point greater than 250° C. and a weight average molecular weight greater than 4000 g / mol.

3. The preparation method according to claim 1, It is characterized in that The cyano-containing polycarbosilane contains heterogeneous elements, and the heterogeneous elements include one or more of aluminum, iron, titanium, zirconium, cobalt, nickel, boron, lanthanum, yttrium, and niobium.

4. The preparation method according to claim 1, It is characterized in that The mass ratio of cyano-containing polycarbosilane, good solvent and poor solvent is 40-65:30-55:5-25.

5. The preparation method according to claim 1, It is characterized in that The spinning is electrospinning, and the process conditions of electrospinning include: the inner diameter of the spinneret is 0.3-2 mm, the spinning voltage is 10-25 kV, the distance between the spinneret and the collector is 10-25 cm, and the feed rate is 10-35 μL / min; Alternatively, the spinning is dry spinning, and the process conditions of dry spinning include: under the protection of an inert atmosphere, raising the spinning solution to 50-150° C. in a spinning device, keeping the temperature for 0.5-5 hours, and ejecting it through a spinneret hole with an inert gas or a metering pump to form cyano-containing polycarbosilane fibers.

6. The preparation method according to claim 1, It is characterized in that Dry heat curing conditions include: heating to 250°C-280°C at 0.5-2°C / min in an inert atmosphere, then heating to 280°C-350°C at 0.2~1.0°C / min, and keeping at this temperature for 0.5-2h.

7. The preparation method according to claim 1, It is characterized in that The high temperature sintering conditions include: heating to 1000°C-1800°C at 2-10°C / min in an inert atmosphere, and keeping at this temperature for 0.5-2h.