A creep-resistant insulating engineering plastic and a preparation method thereof

By combining modified polyamide and phenolic resin, the ultraviolet light-resistant and impact-resistant materials generated by the reaction are solved, and the problems of insufficient impact resistance and high temperature resistance in the prior art are realized. The ultraviolet light resistance of high-performance composite materials is achieved and impact resistance enhances the overall performance of the plastic.

CN115584102BActive Publication Date: 2024-11-15NINGBO TIANMAO PLASTIC PRODUCTS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211124076.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-15
Publication Date
2024-11-15
Estimated Expiration
2042-09-15

AI Technical Summary

Technical Problem

The existing creep-resistant insulating engineering plastics have poor impact resistance, insufficient high-temperature resistance in high-performance composite materials such as bulletproof, rocket, and aircraft, and are not resistant to ultraviolet light, which limits its use range.

Method used

Modified polyamide and modified phenolic resin are used to produce UV-resistant ortho-hydroxybenzophenone through the reaction of polyamide prepolymer and modified microspheres, and phenolic prepolymer and 4-amino-3 nitrogen The reaction of phenylboric acid forms boron-oxyester bonds, which combines the styrene butadiene rubber core and hard shell layer, forming a partial interpenetrating network structure to improve impact resistance and heat resistance.

Benefits of technology

It significantly improves the UV resistance, impact resistance and heat resistance of creep-resistant insulating engineering plastics, enhances its tensile strength, and meets the needs of high-performance composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003847599750000071
    Figure BDA0003847599750000071
  • Figure BDA0003847599750000081
    Figure BDA0003847599750000081
Patent Text Reader

Abstract

The invention discloses a creep-resistant insulating engineering plastic and a preparation method thereof, and relates to the technical field of engineering plastics. The invention first prepares a polyamide prepolymer with 4-hydroxyphthalic acid and ethylenediamine, then prepares modified microspheres with p-hydroxystyrene, butadiene and methyl methacrylate, and then prepares a modified polyamide with the polyamide prepolymer and the modified microspheres; then prepares a phenolic prepolymer with p-methylphenol and formaldehyde, and then prepares a modified phenolic resin with the phenolic prepolymer and 4-amino-3-nitrobenzene boric acid; finally, the modified polyamide and the modified phenolic resin are blended and extruded to prepare creep-resistant insulating engineering plastics. The creep-resistant insulating engineering plastics prepared by the invention have good ultraviolet light resistance, impact resistance, heat resistance and tensile strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of engineering plastics, in particular to a creep-resistant insulating engineering plastic and a preparation method thereof. Background Art

[0002] Engineering plastics are a type of plastic used as engineering structural materials. They often have some unique and excellent properties, such as higher heat resistance, fatigue resistance or wear resistance than general plastics.

[0003] Phenolic resin is the earliest synthesized thermosetting resin. It has the advantages of good electrical insulation and creep resistance. It is a commonly used creep-resistant insulating engineering plastic and can replace metal as an engineering structural material. However, phenolic resin has poor impact resistance and insufficient high temperature resistance, and cannot meet the requirements of high-performance composite materials such as bulletproof, rockets, and aircraft. In addition, since phenolic resin is not resistant to ultraviolet light, it is prone to light aging and cannot be used on some equipment exposed to the field for a long time, which greatly limits the scope of use of phenolic resin creep-resistant insulating engineering plastics. Therefore, a creep-resistant insulating engineering plastic with good ultraviolet light resistance, impact resistance, heat resistance and tensile strength was designed and developed. Summary of the invention

[0004] The object of the present invention is to provide a creep-resistant insulating engineering plastic and a preparation method thereof, so as to solve the problems existing in the prior art.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] The invention discloses a creep-resistant insulating engineering plastic, which comprises modified polyamide and modified phenolic resin.

[0007] Furthermore, the modified polyamide is prepared from polyamide prepolymer and modified microspheres.

[0008] Furthermore, the polyamide prepolymer is prepared from 4-hydroxyphthalic acid and ethylenediamine.

[0009] Furthermore, the modified microspheres are prepared from p-hydroxystyrene, butadiene and methyl methacrylate.

[0010] Furthermore, the modified phenolic resin is prepared from phenolic prepolymer and 4-amino-3-nitrobenzeneboric acid; the phenolic prepolymer is prepared from p-methylphenol and formaldehyde.

[0011] Furthermore, a method for preparing creep-resistant insulating engineering plastics is provided, wherein the method for preparing creep-resistant insulating engineering plastics comprises the following preparation steps:

[0012] (1) at 120-125° C., a polyamide prepolymer and modified microspheres are mixed in a mass ratio of 1:0.1-1:0.3, placed in cyclohexane 4-8 times the mass of the polyamide prepolymer, stirred at 500-600 r / min for 4-5 minutes, and then a boron trifluoride ether solution 0.4-0.5 times the mass of the polyamide prepolymer and having a mass fraction of 60-80% is added dropwise at 5-8 ml / min to obtain a modified polyamide;

[0013] (2) At -2 to 2°C, add 4-amino-3-nitrobenzeneboric acid to a 75-80% hydrochloric acid solution having a mass fraction of 2 to 3 times the mass of 4-amino-3-nitrobenzeneboric acid, stir at 80 to 100 r / min for 0.4 to 0.6 h, add a 35-45% sodium nitrite solution having a mass fraction of 0.4 to 0.6 times the mass of 4-amino-3-nitrobenzeneboric acid at 8 to 12 ml / min, continue stirring for 0.9 to 1.1 h, add 1 to 2 times the mass of 4-amino-3-nitrobenzeneboric acid, and add 4-amino-3-nitrobenzeneboric acid to the solution. .5 to 1.8 times of aminosulfonic acid, continue stirring for 0.1 to 0.3 hours to obtain solution A; mix phenolic prepolymer, sodium hydroxide and anhydrous sodium carbonate in a mass ratio of 1:0.1:0.5 to 1:0.3:0.8, stir at a speed of 60 to 65 r / min for 4 to 6 minutes, add solution A with a mass of 1.6 to 2.1 times of the mass of phenolic prepolymer dropwise at a rate of 35 to 40 ml / min, after the dropwise addition, add a catalyst with a mass of 0.1 to 0.12 times of the mass of the phenolic prepolymer, continue stirring for 3 to 5 hours to obtain a modified phenolic resin;

[0014] (3) Modified polyamide and modified phenolic resin are mixed in a mass ratio of 1:1.8 to 1:2, stirred at 700 to 900 r / min for 12 to 18 minutes, placed on a twin-screw extruder, and extruded to obtain creep-resistant insulating engineering plastics at an extrusion temperature of 155 to 175°C, a screw speed of 200 to 300 r / min, and a vacuum degree of -0.02 to 0.02 MPa.

[0015] Furthermore, the preparation method of the polyamide prepolymer in step (1) is as follows: 4-hydroxyphthalic acid and ethylenediamine are mixed in a mass ratio of 1:2 to 1:3, placed in a mass fraction of 90-95% ethylene glycol ether solution which is 1 to 2 times the mass of 4-hydroxyphthalic acid, stirred at 50 to 60 r / min for 2 to 3 minutes, and stirred at 2500 to 2800 r / min for 8 to 10 hours under nitrogen protection conditions to obtain a polyamide prepolymer.

[0016] Furthermore, the preparation method of the modified microspheres in step (1) is as follows: at 75 to 80° C. and under nitrogen protection, p-hydroxystyrene, butadiene, and deionized water are mixed in a mass ratio of 1:0.2:2 to 1:0.5:4, stirred at 185 to 195 r / min for 4 to 5 min, and then 0.1 to 0.2 times the mass of p-hydroxystyrene sodium dodecyl sulfonate is added, and stirring is continued for 10 to 12 min, and 0.14 to 0.05 times the mass of p-hydroxystyrene is added. .24 times of potassium persulfate, continue stirring for 1 to 1.5 hours, add methyl methacrylate 1 to 2 times of the mass of hydroxystyrene at a rate of 20 to 30 ml / min, continue stirring for 1 to 2 hours after the addition, and cool to room temperature to obtain an emulsion; the emulsion is filtered through a 58-mesh nylon mesh, frozen at -8 to -5°C for 5 to 6 hours, thawed at room temperature, filtered, washed with deionized water for 6 to 8 times, and vacuum dried at 40 to 45°С for 24 to 26 hours to obtain modified microspheres.

[0017] Furthermore, the preparation method of the phenolic prepolymer in step (2) is as follows: at 55-65° C., p-methylphenol and formaldehyde are mixed in a mass ratio of 1:1-1:2.5, added into a 40-50% sodium hydroxide solution with a mass fraction of 8-10 times the mass of p-methylphenol, stirred at 30-50 r / min for 1-3 h, heated to 88-90° C., and continued to stir for 8-12 h to obtain a phenolic prepolymer.

[0018] Furthermore, the catalyst in step (2) is Pd / γ-Al2O3-KNO3.

[0019] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0020] The creep-resistant insulating engineering plastic of the present invention is prepared from modified polyamide and modified phenolic resin; the modified polyamide is prepared from polyamide prepolymer and modified microspheres; the polyamide prepolymer is prepared from 4-hydroxyphthalic acid and ethylenediamine, and the modified microspheres are prepared from p-hydroxystyrene, butadiene and methyl methacrylate; the modified phenolic resin is prepared from phenolic prepolymer and 4-amino-3-nitrobenzene boric acid, and the phenolic prepolymer is prepared from p-methylphenol and formaldehyde;

[0021] First, the carboxyl groups on the polyamide prepolymer react with the phenol groups on the modified microspheres to generate o-hydroxybenzophenone, and at the same time, the modified microspheres are connected to the polyamide prepolymer. After being excited by ultraviolet light, the intramolecular hydrogen bonds of the o-hydroxybenzophenone interconvert with keto-enol, and the absorbed ultraviolet light is released in the form of heat energy or other lower energy, so that the modified polyamide has the effect of ultraviolet light resistance; the interior of the modified microspheres is a styrene-butadiene rubber core generated by the reaction of butadiene and styrene, and the outer layer is a polymethyl methacrylate-polystyrene hard shell layer. The modified microspheres connected to the polyamide prepolymer can, on the one hand, utilize the characteristics of styrene-butadiene rubber to make the modified polyamide have impact resistance. On the other hand, when impacted, the styrene-butadiene rubber debonds at the core-shell interface to generate voids, so that the three-dimensional stress is transformed into a plane stress, thereby absorbing more energy, and further enhancing the impact resistance of the modified polyamide.

[0022] Secondly, p-methylphenol on the phenolic prepolymer reacts with o-nitroaniline on 4-amino-3-nitrobenzene boronic acid to generate 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, which can absorb ultraviolet rays and make the modified phenolic resin have the effect of ultraviolet light resistance; the hydroxyl group on the phenolic prepolymer reacts with the phenylboric acid on the 4-amino-3-nitrobenzene boronic acid to obtain a borane ester bond, and at the same time, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole is coated in the modified phenolic resin, thereby improving the heat resistance of the modified phenolic resin and further enhancing the ultraviolet light resistance effect; the hydrogen bond between the amide group of the modified polyamide and the phenolic hydroxyl group of the modified phenolic resin can promote the mutual miscibility of the modified polyamide and the modified phenolic resin, forming a partial interpenetrating network structure, and improving the tensile strength of the creep-resistant insulating engineering plastic. DETAILED DESCRIPTION

[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0024] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the creep-resistant insulating engineering plastics prepared in the following examples are as follows:

[0025] UV resistance: Take the creep-resistant insulating engineering plastics prepared in the embodiment and the comparative example with the same mass and surface area, and test the UV aging resistance according to GB / T16422.1 standard method, using a UV test box, UV-340 fluorescent UV lamp, blackboard temperature: 60-80°C in light, 40-60°C in darkness, radiation intensity: 0.25-1.55W / m 2 / nm, irradiation time is 12h, and the degree of plastic peeling is evaluated after light aging test.

[0026] Impact resistance: The creep-resistant insulating engineering plastics prepared in the examples and comparative examples with the same mass and surface area were tested for impact strength according to the GB / T1043 standard method.

[0027] Heat resistance: The creep-resistant insulating engineering plastics prepared in the embodiment and the comparative example with the same mass and surface area were tested for Martin heat resistance temperature according to the GB1035 standard method.

[0028] Tensile strength: The creep-resistant insulating engineering plastics prepared in the examples and comparative examples with the same mass and surface area were tested for tensile strength according to the GB / T1040 standard method.

[0029] Example 1

[0030] (1) 4-Hydroxyphthalic acid and ethylenediamine were mixed in a mass ratio of 1:2, placed in a 90% ethylene glycol ether solution with a mass fraction of 1 times the mass of 4-hydroxyphthalic acid, stirred at 50 r / min for 2 minutes, and stirred at 2500 r / min for 8 hours under nitrogen protection to obtain a polyamide prepolymer; p-hydroxystyrene, butadiene, and deionized water were mixed in a mass ratio of 1:0.2:2 at 75°C and nitrogen protection, stirred at 185 r / min for 4 minutes, and then sodium dodecyl sulfonate with a mass fraction of 0.1 times the mass of p-hydroxystyrene was added, and the stirring was continued for 10 minutes, and potassium persulfate with a mass fraction of 0.14 times the mass of p-hydroxystyrene was added, and the stirring was continued for 1 hour. Add methyl methacrylate in an amount of 1 times the mass of p-hydroxystyrene at a rate of 20 ml / min, continue stirring for 1 hour after the addition is completed, and cool to room temperature to obtain an emulsion; filter the emulsion through a 58-mesh nylon mesh, freeze it at -8°C for 5 hours, thaw it at room temperature, filter it, wash it with deionized water for 6 times, and vacuum dry it at 40°С for 24 hours to obtain modified microspheres; mix the polyamide prepolymer and the modified microspheres at a mass ratio of 1:0.1 at 120°C, place them in cyclohexane in an amount of 4 times the mass of the polyamide prepolymer, stir them at 500 r / min for 4 minutes, and then add a 60% boron trifluoride ether solution in an amount of 0.4 times the mass of the polyamide prepolymer at a rate of 5 ml / min to obtain a modified polyamide;

[0031] (2) at 55°C, p-methylphenol and formaldehyde were mixed in a mass ratio of 1:1, added to a 40% sodium hydroxide solution with a mass fraction of 8 times the mass of p-methylphenol, stirred at 30 r / min for 1 hour, heated to 88°C, and stirred for 8 hours to obtain a phenolic prepolymer; at -2°C, 4-amino-3-nitrobenzeneboric acid was added to a 75% hydrochloric acid solution with a mass fraction of 2 times the mass of 4-amino-3-nitrobenzeneboric acid, stirred at a speed of 80 r / min for 0.4 hours, and 0.4 times the mass of 4-amino-3-nitrobenzeneboric acid was added dropwise at a speed of 8 ml / min. A 35% sodium nitrite solution was added, and after the addition, stirring was continued for 0.9h, and aminosulfonic acid (1.5 times the mass of 4-amino-3-nitrobenzeneboric acid) was added, and stirring was continued for 0.1h to obtain solution A; phenolic prepolymer, sodium hydroxide, and anhydrous sodium carbonate were mixed in a mass ratio of 1:0.1:0.5, and stirred at a speed of 60r / min for 4min, and solution A (1.6 times the mass of phenolic prepolymer) was added dropwise at a speed of 35ml / min, and after the addition, Pd / γ-Al2O3-KNO3 (0.1 times the mass of phenolic prepolymer) was added, and stirring was continued for 3h to obtain a modified phenolic resin;

[0032] (3) Modified polyamide and modified phenolic resin were mixed in a mass ratio of 1:1.8, stirred at 700 r / min for 12 min, placed on a twin-screw extruder, and extruded to obtain creep-resistant insulating engineering plastics at an extrusion temperature of 155°C, a screw speed of 200 r / min, and a vacuum degree of -0.02 MPa.

[0033] Example 2

[0034] (1) 4-Hydroxyphthalic acid and ethylenediamine were mixed in a mass ratio of 1:2.5, placed in a 92.5% ethylene glycol ether solution with a mass fraction of 1.5 times the mass of 4-hydroxyphthalic acid, stirred at 55 r / min for 2.5 minutes, and stirred at 2650 r / min for 9 hours under nitrogen protection to obtain a polyamide prepolymer; p-hydroxystyrene, butadiene, and deionized water were mixed in a mass ratio of 1:0.35:3 at 77.5°C and nitrogen protection, stirred at 190 r / min for 4.5 minutes, and then sodium dodecyl sulfonate with a mass fraction of 0.15 times the mass of p-hydroxystyrene was added, and the stirring was continued for 11 minutes, and potassium persulfate with a mass fraction of 0.19 times the mass of p-hydroxystyrene was added, and the stirring was continued for 1.25 hours. Add methyl methacrylate in an amount 1.5 times the mass of p-hydroxystyrene dropwise at a rate of 25 ml / min, continue stirring for 1.5 hours after the addition is complete, and cool to room temperature to obtain an emulsion; filter the emulsion through a 58-mesh nylon mesh, freeze it at -1.5°C for 5.5 hours, thaw it at room temperature, filter it with suction, wash it with deionized water for 7 times, and vacuum dry it at 42.5°С for 25 hours to obtain modified microspheres; mix the polyamide prepolymer and the modified microspheres at a mass ratio of 1:0.2 at 122.5°C, place them in cyclohexane in an amount 6 times the mass of the polyamide prepolymer, stir them at 550 r / min for 4.5 minutes, and then add a 70% boron trifluoride ether solution in an amount 0.45 times the mass of the polyamide prepolymer dropwise at 6.5 ml / min to obtain a modified polyamide;

[0035] (2) At 60°C, p-methylphenol and formaldehyde were mixed in a mass ratio of 1:1.75, added to a 45% sodium hydroxide solution with a mass fraction of 9 times the mass of p-methylphenol, stirred at 40 r / min for 2 hours, heated to 89°C, and stirred for 10 hours to obtain a phenolic prepolymer; at 0°C, 4-amino-3-nitrobenzeneboric acid was added to a 77.5% hydrochloric acid solution with a mass fraction of 2.5 times the mass of 4-amino-3-nitrobenzeneboric acid, stirred at a speed of 90 r / min for 0.5 hours, and 0.5 times the mass of 4-amino-3-nitrobenzeneboric acid was added dropwise at a speed of 10 ml / min. A 40% sodium nitrite solution was added, and after the dripping was completed, stirring was continued for 1 hour, and 1.65 times the mass of 4-amino-3-nitrobenzeneboric acid aminosulfonic acid was added, and stirring was continued for 0.2 hours to obtain solution A; phenolic prepolymer, sodium hydroxide, and anhydrous sodium carbonate were mixed in a mass ratio of 1:0.2:0.65, and stirred at a speed of 62.5r / min for 5 minutes, and 1.85 times the mass of solution A of phenolic prepolymer was dripped at 37.5ml / min, and after the dripping was completed, 0.11 times the mass of Pd / γ-Al2O3-KNO3 of phenolic prepolymer was added, and stirring was continued for 4 hours to obtain modified phenolic resin;

[0036] (3) Modified polyamide and modified phenolic resin were mixed in a mass ratio of 1:1.9, stirred at 800 r / min for 15 min, placed on a twin-screw extruder, and extruded to obtain creep-resistant insulating engineering plastics at an extrusion temperature of 165°C, a screw speed of 250 r / min, and a vacuum degree of 0 MPa.

[0037] Example 3

[0038] (1) 4-Hydroxyphthalic acid and ethylenediamine were mixed in a mass ratio of 1:3, placed in a 95% ethylene glycol ether solution with a mass fraction of twice that of 4-hydroxyphthalic acid, stirred at 60 r / min for 3 min, and stirred at 2800 r / min for 10 h under nitrogen protection to obtain a polyamide prepolymer; p-hydroxystyrene, butadiene, and deionized water were mixed in a mass ratio of 1:0.5:4 at 80°C and nitrogen protection, stirred at 195 r / min for 5 min, and then sodium dodecyl sulfonate with a mass fraction of 0.2 times that of p-hydroxystyrene was added, and the stirring was continued for 12 min, and potassium persulfate with a mass fraction of 0.24 times that of p-hydroxystyrene was added, and the stirring was continued for 1.5 h, dripping methyl methacrylate twice the mass of p-hydroxystyrene at a speed of 30 ml / min, stirring continued for 2 h after dripping, cooling to room temperature to obtain an emulsion; filtering the emulsion through a 58-mesh nylon mesh, freezing at -5°C for 6 h, thawing at room temperature, suction filtering, washing with deionized water for 8 times, and vacuum drying at 45°С for 26 h to obtain modified microspheres; mixing the polyamide prepolymer and the modified microspheres at a mass ratio of 1:0.3 at 125°C, placing them in cyclohexane 8 times the mass of the polyamide prepolymer, stirring at 600 r / min for 5 min, and then dripping 0.5 times the mass of the polyamide prepolymer with a mass fraction of 80% boron trifluoride ether solution at 8 ml / min to obtain a modified polyamide;

[0039] (2) At 65°C, p-methylphenol and formaldehyde were mixed in a mass ratio of 1:2.5, added to a 50% sodium hydroxide solution with a mass fraction of 10 times the mass of p-methylphenol, stirred at 50 r / min for 3 hours, heated to 90°C, and stirred for 12 hours to obtain a phenolic prepolymer; at 2°C, 4-amino-3-nitrobenzeneboric acid was added to an 80% hydrochloric acid solution with a mass fraction of 3 times the mass of 4-amino-3-nitrobenzeneboric acid, stirred at a speed of 100 r / min for 0.6 hours, and 0.6 times the mass of 4-amino-3-nitrobenzeneboric acid was added dropwise at a speed of 12 ml / min. A sodium nitrite solution with a molar fraction of 45% was added, and stirring was continued for 1.1 hours after the addition, and aminosulfonic acid with a mass of 1.8 times that of 4-amino-3-nitrobenzeneboric acid was added, and stirring was continued for 0.3 hours to obtain solution A; phenolic prepolymer, sodium hydroxide, and anhydrous sodium carbonate were mixed in a mass ratio of 1:0.3:0.8, and stirred at a speed of 65r / min for 6 minutes, and solution A with a mass of 2.1 times that of the phenolic prepolymer was added dropwise at a speed of 40ml / min, and after the addition, Pd / γ-Al2O3-KNO3 with a mass of 0.12 times that of the phenolic prepolymer was added, and stirring was continued for 5 hours to obtain a modified phenolic resin;

[0040] (3) Modified polyamide and modified phenolic resin were mixed in a mass ratio of 1:2, stirred at 900 r / min for 18 min, placed on a twin-screw extruder, and extruded to obtain creep-resistant insulating engineering plastics at an extrusion temperature of 175°C, a screw speed of 300 r / min, and a vacuum degree of 0.02 MPa.

[0041] Comparative Example 1

[0042] The difference between Comparative Example 1 and Example 2 is that in step (1), the modified polyamide is prepared by using a polyamide prepolymer prepared from ethylenediamine and oxalic acid and modified microspheres, and the remaining steps are the same as Example 2.

[0043] Comparative Example 2

[0044] The difference between Comparative Example 2 and Example 2 is that in step (1), only polyamide prepolymer is used to prepare modified polyamide, and the remaining steps are the same as Example 2.

[0045] Comparative Example 3

[0046] The difference between Comparative Example 3 and Example 2 is that modified polyamide is not prepared, and only modified phenolic resin is used to prepare creep-resistant insulating engineering plastics, and the remaining steps are the same as Example 2.

[0047] Comparative Example 4

[0048] The difference between Comparative Example 4 and Example 2 is that in step (2), a phenolic prepolymer prepared from phenol and formaldehyde and 4-amino-3-nitrobenzene boric acid are used to prepare a modified phenolic resin, and the remaining steps are the same as in Example 2.

[0049] Comparative Example 5

[0050] The difference between Comparative Example 5 and Example 2 is that in step (2), only phenolic prepolymer is used to prepare the modified phenolic resin, and the remaining steps are the same as Example 2.

[0051] Comparative Example 6

[0052] The difference between Comparative Example 6 and Example 2 is that no modified phenolic resin is prepared, and only modified polyamide is used to prepare creep-resistant insulating engineering plastics, and the remaining steps are the same as Example 2.

[0053] Effect example

[0054] Table 1 below shows the performance analysis results of the ultraviolet light resistance, impact resistance, heat resistance and tensile strength of the creep-resistant insulating engineering plastics prepared by Examples 1 to 3 of the present invention and Comparative Examples 1 to 6.

[0055] Table 1

[0056]

[0057]

[0058] From Table 1, it can be found that the creep-resistant insulating engineering plastics prepared in Examples 1, 2, and 3 have strong UV resistance, impact resistance, heat resistance, and tensile strength; from the comparison of the experimental data of Examples 1, 2, and 3 with Comparative Example 1, it can be found that the use of polyamide prepolymer prepared with 4-hydroxyphthalic acid to prepare modified polyamide can form o-hydroxybenzophenone, and the prepared creep-resistant insulating engineering plastic has strong UV resistance; from the comparison of the experimental data of Examples 1, 2, and 3 with Comparative Example 2, it can be found that the use of modified microspheres to prepare modified polyamide can form o-hydroxybenzophenone, and the prepared creep-resistant insulating engineering plastic has strong UV resistance and impact resistance; from the comparison of the experimental data of Examples 1, 2, and 3 with Comparative Example 3, it can be found that the use of modified polyamide to prepare creep-resistant insulating engineering plastics can form a partial interpenetrating network structure, and the prepared creep-resistant insulating engineering plastic has strong UV resistance and impact resistance. and tensile strength are strong; from the comparison of the experimental data of Examples 1, 2, 3 and Comparative Example 4, it can be found that the use of p-methylphenol to prepare the modified phenolic resin can form 2-(2'-hydroxy-5'-methylphenyl) benzotriazole, and the prepared creep-resistant insulating engineering plastics have strong ultraviolet light resistance; from the comparison of the experimental data of Examples 1, 2, 3 and Comparative Example 5, it can be found that the use of 4-amino-3-nitrobenzene boric acid to prepare the modified phenolic resin can form 2-(2'-hydroxy-5'-methylphenyl) benzotriazole and borooxy ester bonds, and the prepared creep-resistant insulating engineering plastics have strong ultraviolet light resistance and heat resistance; from the comparison of the experimental data of Examples 1, 2, 3 and Comparative Example 6, it can be found that the use of modified phenolic resin to prepare creep-resistant insulating engineering plastics can form a partial interpenetrating network structure, and the prepared creep-resistant insulating engineering plastics have strong ultraviolet light resistance, heat resistance and tensile strength.

[0059] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A method for preparing creep-resistant insulating engineering plastics, characterized in that: The method comprises the following preparation steps: (1) At 75-80°C and nitrogen protection, p-hydroxystyrene, butadiene and deionized water were mixed in a mass ratio of 1:0.2:2-1:0.5:4, stirred at 185-195 r / min for 4-5 min, then sodium dodecyl sulfonate (0.1-0.2 times the mass of p-hydroxystyrene) was added, and stirring was continued for 10-12 min, potassium persulfate (0.14-0.24 times the mass of p-hydroxystyrene) was added, and stirring was continued for 1-1.5 h, methyl methacrylate (1-2 times the mass of p-hydroxystyrene) was added dropwise at a rate of 20-30 ml / min, and stirring was continued for 1-2 h after the addition was completed, and the emulsion was cooled to room temperature to obtain an emulsion; the emulsion was filtered through a 58-mesh nylon mesh, frozen at -8--5°C for 5-6 h, thawed at room temperature, filtered, washed with deionized water for 6-8 times, and vacuum dried at 40-45°C for 24-8 hours. 26h to obtain modified microspheres; 4-hydroxyphthalic acid and ethylenediamine were mixed in a mass ratio of 1:2~1:3, placed in a mass fraction of 90~95% ethylene glycol ether solution of 1~2 times the mass of 4-hydroxyphthalic acid, stirred at 50~60r / min for 2~3min, and stirred at 2500~2800r / min for 8~10h under nitrogen protection to obtain polyamide prepolymer; at 120~125℃, the polyamide prepolymer and the modified microspheres were mixed in a mass ratio of 1:0.1~1:0.3, placed in cyclohexane of 4~8 times the mass of the polyamide prepolymer, stirred at 500~600r / min for 4~5min, and then a mass fraction of 60~80% boron trifluoride ether solution of 0.4~0.5 times the mass of the polyamide prepolymer was added dropwise at 5~8ml / min to obtain modified polyamide; (2) At 55-65°C, p-methylphenol and formaldehyde were mixed in a mass ratio of 1:1-1:2.5, added to a 40-50% sodium hydroxide solution with a mass fraction of 8-10 times the mass of p-methylphenol, stirred at 30-50 r / min for 1-3 h, heated to 88-90°C, and continued to stir for 8-12 h to obtain a phenolic prepolymer; at -2-2°C, 4-amino-3-nitrobenzeneboric acid was added to a 75-80% hydrochloric acid solution with a mass fraction of 2-3 times the mass of 4-amino-3-nitrobenzeneboric acid, stirred at 80-100 r / min for 0.4-0.6 h, and 0.4% of 4-amino-3-nitrobenzeneboric acid was added dropwise at 8-12 ml / min. ~0.6 times the mass fraction of 35~45% sodium nitrite solution, after the dripping is completed, continue stirring for 0.9~1.1h, add 1.5~1.8 times the mass of 4-amino-3-nitrobenzeneboric acid aminosulfonic acid, continue stirring for 0.1~0.3h, and obtain solution A; phenolic prepolymer, sodium hydroxide, and anhydrous sodium carbonate are mixed at a mass ratio of 1:0.1:0.5~1:0.3:0.8, stir at a speed of 60~65r / min for 4~6min, and add 1.6~2.1 times the mass of solution A of phenolic prepolymer at 35~40ml / min, after the dripping is completed, add 0.1~0.12 times the mass of catalyst of phenolic prepolymer, continue stirring for 3~5h, and obtain modified phenolic resin; (3) Modified polyamide and modified phenolic resin are mixed in a mass ratio of 1:1.8~1:2, stirred at 700~900 r / min for 12~18 min, placed on a twin-screw extruder, and extruded to obtain creep-resistant insulating engineering plastics at an extrusion temperature of 155~175°C, a screw speed of 200~300 r / min, and a vacuum degree of -0.02~0.02 MPa.

2. The method for preparing creep-resistant insulating engineering plastics according to claim 1, characterized in that: The catalyst in step (2) is Pd / γ-Al2O3-KNO3.