Oxygen-enriched asphalt-based activated carbon fiber and preparation method and application thereof

Through tetrahydrofuran extraction and heat condensation of medium-temperature coal asphalt, combined with air stabilization, oxygen-rich asphalt-based activated carbon fibers with low softening points were prepared, which resolved the contradiction between softening points and spinning properties, achieved high specific capacitance and stability, and improved the Its application performance in supercapacitor electrode materials.

CN115584572BActive Publication Date: 2024-11-05JIANGSU UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211285653.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-20
Publication Date
2024-11-05
Estimated Expiration
2042-10-20

AI Technical Summary

Technical Problem

During the preparation process of existing activated carbon fibers, the increase in softening point leads to a deterioration of spinning properties, making it difficult to ensure high softening point and good spinning properties at the same time, limiting its application as a supercapacitor electrode material.

Method used

The asphaltene was obtained through tetrahydrofuran extraction by medium-temperature coal asphalt, heat condensation and single-hole melt spinning were carried out, combined with the three-stage air stabilization method, low-temperature carbonization and activation, and oxygen-rich asphalt-based activated carbon fibers were prepared with low softening point.

Benefits of technology

The prepared oxygen-rich asphalt-based activated carbon fiber has a large specific surface area, moderate oxygen content, excellent electrochemical performance, with a specific capacitance of up to 315F/g, and the capacitance retention rate is still as high as 91.4% after 10,000 charge and discharge cycles, which significantly improves the application of materials. potential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115584572B_ABST
    Figure CN115584572B_ABST
Patent Text Reader

Abstract

The present invention provides an oxygen-enriched asphalt-based activated carbon fiber and a preparation method and application thereof, belonging to the technical field of supercapacitor electrode material preparation; in the present invention, medium-temperature coal tar asphalt as a raw material is extracted with tetrahydrofuran to obtain asphaltene, and then subjected to thermal polycondensation and single-hole melt spinning to obtain low-softening-point asphalt precursor; the asphalt precursor is subjected to a three-stage air stabilization method to obtain stabilized fibers, and then subjected to low-temperature carbonization and low-temperature activation to obtain asphalt-based activated carbon fibers; the oxygen-enriched asphalt-based activated carbon fibers have a large specific surface area, a moderate oxygen content, and excellent electrochemical properties, and have broad application prospects in carbon-based electrode materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of supercapacitor electrode material preparation, and specifically relates to an oxygen-enriched asphalt-based activated carbon fiber and a preparation method and application thereof. Background Art

[0002] With the increasing utilization and demand for new energy, it is urgent to develop low-cost, long-life, and environmentally friendly energy storage technologies. Supercapacitors have attracted much attention due to their short charging time, high power density, and long cycle life. Activated carbon fibers have the advantages of large relative area, uniform pore size distribution, and good conductivity, and can be directly used as electrode materials for supercapacitors. However, existing activated carbon fibers still have many defects, such as the high cost of polyacrylonitrile-based activated carbon fibers, which are difficult to apply on a large scale. Although the raw materials for preparing asphalt-based activated carbon fibers are cheap and widely available coal tar or petroleum asphalt, the raw asphalt must be thermally condensed during its preparation process to increase its softening point. In order to achieve successful stabilization of asphalt precursor, the softening point of spinning asphalt is usually required to be above 240°C. However, as the softening point increases, the spinnability of asphalt deteriorates, so it is difficult to simultaneously ensure high softening point and good spinnability, and it is difficult to use as an electrode material in supercapacitors. Therefore, it is necessary to explore a method for preparing asphalt-based activated carbon fibers from low-softening point asphalt fibers. Summary of the invention

[0003] In view of some deficiencies in the prior art, the present invention provides an oxygen-enriched asphalt-based activated carbon fiber and its preparation method and application. In the present invention, the raw material medium-temperature coal tar is extracted with tetrahydrofuran to obtain asphaltene, and then subjected to thermal polycondensation and single-hole melt spinning to obtain low-softening point asphalt precursor; the asphalt precursor is subjected to a three-stage air stabilization method to obtain stabilized fibers, and then subjected to low-temperature carbonization and low-temperature activation to obtain asphalt-based activated carbon fibers; the oxygen-enriched asphalt-based activated carbon fibers have a large specific surface area, moderate oxygen content, and excellent electrochemical properties, and have broad application prospects in carbon-based electrode materials.

[0004] The present invention first provides an oxygen-enriched asphalt-based activated carbon fiber, which is in the shape of a fiber similar to a hair and has a diameter of 18 to 20 μm; the surface of the oxygen-enriched asphalt-based activated carbon fiber is rough, and the surface of the oxygen-enriched asphalt-based activated carbon fiber has developed micropores and a small amount of mesopores; the oxygen content of the oxygen-enriched asphalt-based activated carbon fiber exceeds 12wt.%; when the current density is 1A / g, the specific capacitance of the oxygen-enriched asphalt-based activated carbon fiber reaches 315F / g, and its capacitance retention rate is still as high as 91.4% after 10,000 charge and discharge cycles at 1A / g.

[0005] The present invention also provides a method for preparing the above oxygen-enriched asphalt-based activated carbon fiber, comprising the following steps:

[0006] Step 1: crushing the medium temperature coal tar pitch, and then extracting it with tetrahydrofuran (THF) to obtain asphaltene;

[0007] Step 2: crushing the asphaltene, putting it into a reactor, introducing air for blowing, then heating it to 320-330° C. and keeping it for a certain period of time, and cooling it to room temperature after the end of the insulation to obtain a spinning pitch;

[0008] The spinning pitch is subjected to a single-hole melt spinning method to obtain a low-softening-point asphalt raw fiber;

[0009] Step 3: subjecting the asphalt raw silk to a stabilization reaction through a three-stage air stabilization method, and obtaining stabilized asphalt fibers after the reaction is completed;

[0010] Then, the stabilized asphalt fiber is heated to 500-600° C. under the protection of high-purity nitrogen for calcination, and after the calcination, asphalt-based carbon fiber is obtained;

[0011] Then the asphalt-based carbon fiber is mixed with KOH solid powder for activation reaction, and after the reaction is completed, it is washed, filtered and dried to obtain oxygen-enriched asphalt-based activated carbon fiber.

[0012] Wherein, in step 1, the medium temperature coal tar pitch is crushed to less than 20 mesh;

[0013] The weight ratio of the medium temperature coal tar pitch to tetrahydrofuran is 1:4-1:6;

[0014] The medium temperature coal tar has an ash content of ≤0.2wt.%, and a softening point of 80-100°C;

[0015] The asphaltene has an ash content of ≤0.03wt.%, and a softening point of 70-90°C.

[0016] In step 2 of the preparation method, the asphaltene is crushed to less than 20 mesh;

[0017] The air purge flow rate is 300-500 mL / min;

[0018] The heating rate is 5-10°C / min, and the heat preservation time is 2-3h;

[0019] The softening point of the spinning pitch is about 190-200° C.; the diameter of the asphalt raw fibers is 18-20 μm.

[0020] In the preparation method, in step 2, the operation method of the single-hole melt spinning method is: take 20-30g of spinning asphalt, the spinning temperature is 240-250°C, the nitrogen pressure is 1-1.2MPa, the spinneret diameter is 0.2mm, the spinning speed of the spinning drum is 300-500m / min, and the spinning asphalt forms asphalt filaments under the action of nitrogen extrusion and stretching of the spinning drum.

[0021] In the preparation method, in step three, the three-stage air stabilization method is operated as follows: heating from room temperature to 160-170°C at a heating rate of 10-20°C / min, heating to 260-270°C at a heating rate of 0.1-0.3°C / min, and keeping the temperature at this temperature for 2-4 hours.

[0022] In the preparation method, in step 3, the calcination conditions are: heating to 500-600° C. at a heating rate of 5° C. / min and calcining for 30-60 min.

[0023] In the preparation method, in step 3, the mass ratio of the asphalt-based carbon fiber to KOH is 1:1 to 1:2;

[0024] The conditions of the activation reaction are: heating to 600-700° C. at a heating rate of 5-10° C. / min, and maintaining at this temperature for 0.5-1.5 h.

[0025] The washing is performed by washing with 1 mol / L HCl solution and washing with deionized water until neutral;

[0026] The drying step is: placing the mixture in a 100-110° C. forced air drying oven for drying.

[0027] The present invention also provides the use of the oxygen-enriched asphalt-based activated carbon fiber in supercapacitor electrode materials.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] The reaction parameters and reaction steps in the present invention allow as much oxygen as possible to be introduced into the final oxygen-enriched asphalt-based activated carbon fiber, and the introduced oxygen element is relatively stable after carbonization treatment, greatly increasing the hydrophilicity, stability and pseudocapacitance of the material. In addition, the present invention combines the thermal reactivity of low-softening-point asphalt precursor to formulate a programmed temperature increase scheme that conforms to its thermal reactivity, prevents the asphalt precursor from melting during the stabilization process, and realizes the preparation of oxygen-enriched asphalt-based activated carbon fiber from low-softening-point asphalt precursor, greatly reducing its preparation difficulty.

[0030] Compared with the existing asphalt-based activated carbon fibers, the oxygen-enriched asphalt-based activated carbon fibers prepared in the present invention have a higher specific surface area, a high oxygen content, stable properties, and greatly reduced preparation cost and difficulty; these gain effects greatly improve the specific capacitance of the oxygen-enriched asphalt-based activated carbon fibers and give them high application potential in the field of supercapacitor electrode materials.

[0031] The oxygen-enriched asphalt-based activated carbon fiber prepared by the present invention has a specific capacitance of up to 315F / g at 1A / g, which greatly exceeds the specific capacitance of existing commercial asphalt-based activated carbon fibers (less than 200F / g); after 10,000 charge and discharge cycles at 1A / g, its capacitance retention rate is as high as 91.4%, and its cycle stability is also better than that of most similar materials whose capacitance after cycles is less than 90%. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is a field emission scanning electron microscope image of asphalt-based activated carbon fiber.

[0033] Figure 2 This is the thermogravimetric curve of asphalt raw fiber during air stabilization.

[0034] Figure 3 This is the nitrogen adsorption and desorption isotherm of oxygen-enriched asphalt-based activated carbon fiber.

[0035] Figure 4 This is the pore size distribution diagram of oxygen-enriched asphalt-based activated carbon fiber.

[0036] Figure 5 is the mass specific capacitance of oxygen-enriched asphalt-based activated carbon fibers at different current densities.

[0037] Figure 6 This is a diagram showing the cycle stability performance test of a button-shaped supercapacitor assembled with oxygen-rich asphalt-based activated carbon fibers as electrode materials. DETAILED DESCRIPTION

[0038] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments, but the protection scope of the present invention is not limited thereto. The following embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, within the scope of the technical concept of the present invention, various changes or modifications can be made to the present invention, and these simple modifications also belong to the protection scope of the present invention.

[0039] Example 1: Preparation method and performance testing of oxygen-enriched asphalt-based activated carbon fibers

[0040] Step 1: crush the medium-temperature coal tar pitch into a powder of ≤20 mesh, mix it with tetrahydrofuran in a mass ratio of 1:4, extract the tetrahydrofuran-soluble component, and vacuum dry to obtain asphaltene with zero quinoline insoluble matter and an ash content of less than 0.03wt.%.

[0041] Step 2: Crush the asphaltene to less than 20 mesh, then put it into a reactor, blow it with an air flow of 300mL / min, heat it to 320℃ at a heating rate of 10℃ / min and keep it at this temperature for 2h, then cool it naturally to room temperature and take it out to obtain a spinning asphalt with a softening point of 190℃; take 20g of spinning asphalt, and spin the obtained spinning asphalt into low softening point asphalt raw fibers with an average diameter of about 18μm through a single-hole melt spinning method under the conditions of a spinning temperature of 240℃, a nitrogen pressure of 1MPa and a winding speed of 500m / min.

[0042] Step 3: Place the asphalt raw fiber in the pre-oxidation furnace and ensure that it is fully dispersed, and heat it from room temperature to 160°C at a heating rate of 10°C / min, and heat it to 260°C at a heating rate of 0.1°C / min. The system is kept at 260°C for 4h, and the stabilized asphalt fiber is obtained after the program is completed. Then the stabilized asphalt fiber is placed in a high-temperature tubular furnace, high-purity nitrogen is introduced as a protective gas, and the temperature is increased to 500°C at a heating rate of 3°C / min and kept at this temperature for 60min to obtain asphalt-based carbon fiber. Finally, the asphalt-based carbon fiber and KOH solid powder are mixed in a mass ratio of 1:1, heated to 600°C at a heating rate of 5°C / min, and kept at this temperature for 1.5h, then washed with 1mol / L HCl solution, and then washed with deionized water until neutral. After washing, it is placed in a 100°C blast drying oven and dried for 12h to obtain oxygen-enriched asphalt-based activated carbon fiber (OPACF-1).

[0043] Figure 1 This is a field emission scanning electron microscope image of asphalt-based activated carbon fiber. Figure 1 It can be seen that the surface of oxygen-enriched asphalt-based activated carbon fiber is rough and has a small amount of pores.

[0044] Figure 2 is the thermogravimetric curve of asphalt raw fiber during air stabilization. Figure 2 It can be seen that the weight of the asphalt precursor shows a slow downward trend before 160°C, and the weight and heat release of the asphalt precursor both increase significantly after 160°C, reaching a peak at around 225°C. This indicates that before 160°C, the asphalt precursor is mainly dehydrated and the light components volatilize, and its stabilization reaction is slow. Therefore, the heating rate can be appropriately increased. After 160°C, the stabilization reaction of the asphalt precursor accelerates, so the heating rate needs to be greatly reduced to make the stabilization reaction of the asphalt precursor more complete.

[0045] Figure 3 This is the nitrogen adsorption-desorption isotherm of oxygen-enriched asphalt-based activated carbon fiber. It can be seen from the figure that the prepared oxygen-enriched asphalt-based activated carbon fiber has strong adsorption capacity and well-developed micropores, which provides a large number of adsorption sites for electrons and electrolyte ions, thereby enhancing its capacitive performance.

[0046] Figure 4 This is the pore size distribution diagram of oxygen-enriched asphalt-based activated carbon fiber. It can be seen from the figure that the obtained oxygen-enriched asphalt-based activated carbon fiber has a small amount of mesopores in addition to micropores. The existence of these mesopores provides channels for the diffusion and transmission of ions in the electrolyte, thereby increasing the specific capacitance and rate performance of the material.

[0047] In this example, the prepared oxygen-enriched pitch-based activated carbon fiber was used as a supercapacitor electrode material. A 6 mol / L KOH solution was used as an electrolyte in a three-electrode system. The prepared oxygen-enriched pitch-based activated carbon fiber electrode was used as a working electrode, a platinum sheet was used as a counter electrode, and a Hg / HgO calomel electrode was used as a reference electrode to test its electrochemical properties. The test results are shown in FIG. Figure 5 As shown, from Figure 5 It can be seen that when the current density is 1A / g, the specific capacitance measured is 286F / g, and when the current density is 50A / g, the specific capacitance measured is 219F / g. The capacitance retention rate is as high as 76.6%, and its rate performance exceeds that of most existing similar materials.

[0048] Example 2: Preparation method and performance testing of oxygen-enriched asphalt-based activated carbon fibers

[0049] Step 1: crush the medium-temperature coal tar pitch into a powder of ≤20 mesh, mix it with tetrahydrofuran at a mass ratio of 1:5, extract the tetrahydrofuran-soluble component, and vacuum dry to obtain asphaltene with zero quinoline insoluble matter and ash content less than 0.03wt.%.

[0050] Step 2: Crush the asphaltene to less than 20 mesh, then put it into a reactor, blow it with an air flow of 400mL / min, heat it to 325℃ at a heating rate of 8℃ / min and keep it at this temperature for 2.5h, then cool it naturally to room temperature and take it out to obtain a spinning asphalt with a softening point of 195℃; take 25g of spinning asphalt, and spin the obtained spinning asphalt into low softening point asphalt raw fibers with an average diameter of about 19μm through a single-hole melt spinning method under the conditions of a spinning temperature of 245℃, a nitrogen pressure of 1.1MPa and a winding speed of 400m / min.

[0051] Step 3: Place the asphalt raw fiber in a pre-oxidation furnace and ensure that it is fully dispersed, and heat it from room temperature to 165°C at a heating rate of 15°C / min, and heat it to 265°C at a heating rate of 0.2°C / min. The system is kept at 265°C for 3 hours. After the program is completed, stabilized asphalt fiber is obtained. Then the stabilized asphalt fiber is placed in a high-temperature tubular furnace, high-purity nitrogen is introduced as a protective gas, and the temperature is increased to 550°C at a heating rate of 4°C / min and kept at this temperature for 40 minutes to obtain asphalt-based carbon fiber. Finally, the asphalt-based carbon fiber and KOH solid powder are mixed in a mass ratio of 1:1.5, heated to 650°C at a heating rate of 8°C / min, and kept at this temperature for 1 hour, then washed with 1mol / L HCl solution, and then washed with deionized water until neutral. After washing, it is placed in a 105°C blast drying oven and dried for 11 hours to obtain oxygen-enriched asphalt-based activated carbon fiber (OPACF-1.5);

[0052] The oxygen-enriched pitch-based activated carbon fiber prepared above was used as the electrode material of the supercapacitor. In a three-electrode system, 6 mol / L KOH solution was used as the electrolyte, the prepared oxygen-enriched pitch-based activated carbon fiber electrode was used as the working electrode, the platinum sheet was used as the counter electrode, and the Hg / HgO calomel electrode was used as the reference electrode. The electrochemical performance was tested. The test results are shown in FIG. Figure 5 As shown, from Figure 5 It can be seen that when the current density is 1A / g, the specific capacitance measured is 306F / g, and when the current density is 50A / g, the specific capacitance measured is 235F / g. The capacitance retention rate is as high as 76.8%, and its rate performance exceeds that of most existing similar materials.

[0053] Example 3: Preparation method and performance testing of oxygen-enriched asphalt-based activated carbon fibers

[0054] Step 1: crush the medium-temperature coal tar pitch into a powder of ≤20 mesh, mix it with tetrahydrofuran in a mass ratio of 1:6, extract the tetrahydrofuran-soluble component, and vacuum dry to obtain asphaltene with zero quinoline insoluble matter and ash content less than 0.03wt.%.

[0055] Step 2: Crush the asphaltene to less than 20 mesh, then put it into a reactor, blow it with an air flow of 500mL / min, heat it to 330℃ at a heating rate of 5℃ / min and keep it at this temperature for 3h, then cool it naturally to room temperature and take it out to obtain a spinning asphalt with a softening point of 200℃; take 30g of spinning asphalt, and spin the obtained spinning asphalt into low softening point asphalt raw fibers with an average diameter of about 20μm through a single-hole melt spinning method under the conditions of a spinning temperature of 250℃, a nitrogen pressure of 1.2MPa and a winding speed of 300m / min.

[0056] Step 3: Place the asphalt raw fiber in a pre-oxidation furnace and ensure that it is fully dispersed. First, heat it from room temperature to 170°C at a heating rate of 20°C / min, then heat it to 270°C at a heating rate of 0.3°C / min. The system is kept at 270°C for 2h. After the program is completed, stabilized asphalt fiber is obtained. Then put the stabilized asphalt fiber into a high-temperature tubular furnace, introduce high-purity nitrogen as a protective gas, heat it to 600°C at a heating rate of 5°C / min and keep it at this temperature for 30min to obtain asphalt-based carbon fiber. Finally, mix the asphalt-based carbon fiber with KOH solid powder in a mass ratio of 1:2, heat it to 700°C at a heating rate of 10°C / min, keep it at this temperature for 0.5h, then wash it with 1mol / L HCl solution, and then wash it with deionized water until neutral. After washing, put it in a 110°C blast drying oven and dry it for 10h to obtain oxygen-enriched asphalt-based activated carbon fiber (OPACF-2);

[0057] The oxygen-enriched pitch-based activated carbon fiber prepared above was used as the electrode material of the supercapacitor. In a three-electrode system, 6 mol / L KOH solution was used as the electrolyte, the prepared oxygen-enriched pitch-based activated carbon fiber electrode was used as the working electrode, the platinum sheet was used as the counter electrode, and the Hg / HgO calomel electrode was used as the reference electrode. The electrochemical performance was tested. The test results are shown in FIG. Figure 5 As shown, when the current density is 1A / g, the measured specific capacitance is 315F / g, which is better than most similar materials. When the current density is 50A / g, the measured specific capacitance is 256F / g, and the capacitance retention rate is as high as 81.3%. Its rate performance exceeds that of most existing similar materials.

[0058] In this example, the prepared oxygen-enriched pitch-based activated carbon fiber (OPACF-2) was used as an electrode material to assemble a button-shaped supercapacitor to investigate its cycle stability. The results are shown in FIG. Figure 6 As shown, Figure 6 This is a test diagram of the cycle stability performance of button-shaped supercapacitors assembled with pitch-based activated carbon fibers as electrode materials. Figure 6 It can be seen that after 10,000 charge-discharge cycles at 1 A / g, the capacitance retention rate of OPACF-2 is 91.4%, while the capacitance retention rate of similar materials in the prior art does not exceed 90% after 10,000 charge-discharge cycles. It can be seen that the cycle stability performance of the oxygen-enriched asphalt-based activated carbon fiber prepared in the present invention is better than that of most similar materials.

[0059] The embodiments are preferred implementations of the present invention, but the present invention is not limited to the above-mentioned implementations. Any obvious improvements, substitutions or modifications that can be made by those skilled in the art without departing from the essential content of the present invention belong to the protection scope of the present invention.

Claims

1. A method for preparing oxygen-enriched pitch-based activated carbon fibers, characterized in that: include: Step 1: crushing the medium temperature coal tar pitch, and then extracting it with tetrahydrofuran to obtain asphaltene; Step 2: crushing the asphaltene, putting it into a reactor, blowing it with air, and then heating it to 320-330°C for insulation, cooling it to room temperature after insulation, and obtaining spinning pitch; the heating rate is 5-10°C / min, and the insulation time is 2-3h; the softening point of the spinning pitch is 190-200°C; The spinning pitch is subjected to a single-hole melt spinning method to obtain a low-softening-point asphalt precursor; the single-hole melt spinning method comprises the following steps: taking 20-30 g of the spinning pitch, the spinning temperature is 240-250° C., the nitrogen pressure is 1-1.2 MPa, the spinneret diameter is 0.2 mm, the spinning speed of the spinning drum is 300-500 m / min, and the spinning pitch forms asphalt precursor under the action of nitrogen extrusion and stretching of the spinning drum; the diameter of the asphalt precursor is 18-20 μm; Step 3: Stabilizing the asphalt raw silk through a three-stage air stabilization method, and obtaining stabilized asphalt fibers after the reaction is completed; the three-stage air stabilization method is specifically: heating from room temperature to 160-170°C at a heating rate of 10-20°C / min, heating to 260-270°C at a heating rate of 0.1-0.3°C / min, and keeping the temperature at this final temperature for 2-4 hours; Then, the stabilized asphalt fiber is heated to 500-600°C under the protection of high-purity nitrogen and calcined for 30-60 minutes, and asphalt-based carbon fiber is obtained after the calcination. Then the asphalt-based carbon fiber is mixed with KOH solid powder for activation reaction, and after the reaction is completed, it is washed, filtered, and dried to obtain oxygen-enriched asphalt-based activated carbon fiber; The oxygen-enriched asphalt-based activated carbon fiber is in a fiber shape similar to a hair, with a diameter of 18 to 20 μm.

2. The method for preparing oxygen-enriched asphalt-based activated carbon fiber according to claim 1, characterized in that: Medium temperature coal tar pitch is crushed to less than 20 mesh; The weight ratio of the medium temperature coal tar pitch to tetrahydrofuran is 1:4-1:6; The medium temperature coal tar pitch has an ash content of ≤0.2 wt.% and a softening point of 80-100°C; The asphaltene has an ash content of ≤0.03 wt.% and a softening point of 70-90°C.

3. The method for preparing oxygen-enriched asphalt-based activated carbon fiber according to claim 1, characterized in that: In step 2, asphaltene is crushed to less than 20 mesh; The air purge flow rate was 300-500 mL / min.

4. The method for preparing oxygen-enriched asphalt-based activated carbon fiber according to claim 1, characterized in that: In step 3, the mass ratio of asphalt-based carbon fiber and KOH is 1:1~1:2; The activation reaction conditions are: heating to 600-700° C. at a heating rate of 5-10° C. / min, and maintaining at this temperature for 0.5-1.5 h.

5. The oxygen-enriched asphalt-based activated carbon fiber prepared by the method according to any one of claims 1 to 4, characterized in that: The surface of the oxygen-enriched asphalt-based activated carbon fiber is rough, and the surface of the oxygen-enriched asphalt-based activated carbon fiber has well-developed micropores and a small amount of mesopores.

6. The oxygen-enriched asphalt-based activated carbon fiber according to claim 5, characterized in that: The oxygen content of the oxygen-enriched asphalt-based activated carbon fiber exceeds 12 wt.%; when the current density is 1 A / g, the specific capacitance of the oxygen-enriched asphalt-based activated carbon fiber reaches 315 F / g, and the capacitance retention rate reaches 91.4% after 10,000 charge and discharge cycles at 1 A / g.

7. Use of the oxygen-enriched asphalt-based activated carbon fiber according to claim 5 in supercapacitor electrode materials.

Citation Information

Patent Citations

  • Integrated two-phase pitch-based carbon nanofiber as well as preparation method and application thereof

    CN114808197A

  • Carbon material, dual layer capacitor polarizable electrode

    CN1349234A