Laser high temperature flash formation method for oxide film on the surface of steel material

The Fe3O4 oxide film is generated on the surface of steel material by laser high-temperature flash formation method, which solves the problems of long generation time, high energy consumption and serious pollution in the traditional method, and improves the high-temperature wear resistance and extends the life of the roll.

CN115612973BActive Publication Date: 2024-11-22SHANGHAI ZHIBO LASER TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211363366.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-02
Publication Date
2024-11-22
Estimated Expiration
2042-11-02

AI Technical Summary

Technical Problem

The prior art is difficult to quickly and effectively form a closely-bonded Fe3O4 oxide film on the surface of steel materials at high temperatures, resulting in the roll being easily damaged in a high temperature environment, and the traditional methods have problems such as high energy consumption, long time and serious pollution.

Method used

Using the laser high-temperature flash formation method, the activation film is formed by coating the activation liquid on the surface of the steel material, and the laser beam scanning is used to heat it to 1450-1500°C, and the Fe3O4 oxide film is generated in a very short time (0.01-10 milliseconds), which solves the problem of The drawbacks of traditional methods.

Benefits of technology

The formation of a stable Fe3O4 oxide film in a very short time is achieved, which improves the high-temperature wear resistance of the roll, extends the roll life, reduces production costs and energy consumption, and avoids pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115612973B_ABST
    Figure CN115612973B_ABST
Patent Text Reader

Abstract

The present application discloses a laser high-temperature flash forming method for an oxide film on the surface of a steel material, the laser high-temperature flash forming method comprising: applying an activation liquid to a surface of a steel material to be formed. 3 O 4 The surface of the steel material is oxidized to form a layer of Fe 2+ , Fe 3+ ion activation film; heating by a laser beam for heating is required to generate the Fe 3 O 4 The surface of the iron and steel material with an oxide film is heated to 1450-1500°C, and the Fe 3 O 4 The surface of the steel material is irradiated with a laser beam for heating and oxygen is sprayed toward the surface of the steel material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of preparation of oxide films on the surface of steel materials, and in particular to a laser high-temperature flash forming method for oxide films on the surface of steel materials. Background Art

[0002] Most industrial components are made of steel materials, such as rollers. Rollers are important components of hot rolling production line mills. Steel strips are rolled under vertical pressure through a pair of rolling rollers. The direct material consumption is about 5-15% of the steel rolling production cost.

[0003] During the production of hot-rolled steel strips, the working conditions of the rollers are very harsh. They are in contact with the rolled material at a temperature of up to 900-1200℃. In addition to the strong high-temperature friction and wear of the rolled material, the roller surface is also subjected to high-temperature oxidation, which forms an oxide film on the roller surface. The peeling of the oxide film aggravates the failure of the roller. In addition, the rollers are repeatedly heated by the rolled material and cooled by cooling water during operation, and are subjected to high-frequency rapid cooling and heating. The fatigue thermal stress generated by rapid cooling and heating will induce microcracks. The fatigue microcracks continue to expand under the action of rolling force, eventually causing the roller surface to crack or even peel off, causing the roller to fail. Therefore, in addition to high wear resistance and toughness, hot-rolled rollers should also have excellent anti-oxidation and thermal fatigue resistance.

[0004] High-speed steel has the characteristics of high toughness and high hardness in physical properties, especially high hardness at high temperature, high wear resistance, good red hardness, good roughness, and good oxide film generation ability. The amount of steel rolled in a single grinding can reach 2 to 4 times that of high-chromium iron material. Therefore, high-speed steel rolls have been widely used in the front section of the finishing rolling stand (F1~4), and new high-speed steel rolls have been gradually developed and promoted for application in the roughing rolling stand and the back section of the finishing rolling stand.

[0005] However, the price of high-speed steel is relatively high. In practical applications, composite high-speed steel rolls are often used to reduce costs. Composite high-speed steel rolls are formed by a core roll with a high-speed steel roll sleeve, where the core roll can be a ductile iron roll. In the process of hot finishing rolling of steel plates, 6 to 8 stands are required for rolling in sequence. The first four stands have a high rolling temperature of about 900 to 1200°C, a large reduction, and a large rolling force, and generally use high-speed steel rolls.

[0006] During the hot rolling process of steel plates, a layer of oxide scale is generated on the surface of the roller due to the contact between the roller surface and the red-hot high-temperature steel billet. This layer of oxide scale has both positive and negative effects.

[0007] Its beneficial effects are: first, it can reduce friction and reduce roll wear; second, it can prevent the red-hot steel billet from sticking to the roll surface; third, the oxide scale has a low thermal conductivity, which can isolate the roll base and the red-hot steel billet, reduce the roll base temperature, reduce thermal shock, and inhibit thermal fatigue cracks on the roll surface.

[0008] The disadvantage of the oxide scale on the surface of the roller is that the oxide scale formed in the prior art is mainly composed of loose ferrous oxide (FeO). Therefore, in the subsequent rolling process, the oxide scale is easy to peel off. The peeled iron oxide scale is pressed into the surface of the slab, and further stretched into a chain shape as the rolling progresses, which damages the surface quality of the steel slab and causes the rolled steel plate to be downgraded or scrapped.

[0009] According to statistics, the scrap rate of hot-rolled high-strength steel plates caused by the peeling of iron oxide scale is about 20%. Taking a production line with an annual output of 6 million tons as an example, 1.2 million tons of steel are scrapped or downgraded in one year. The sales price difference of downgrading one level is 500 yuan / ton. Therefore, only a 6 million ton hot rolling production line will lose 30 million yuan a year. Because the loose ferrous oxide scale peels off during the rolling process, the rollers are severely worn. When rolling high-quality steel plates, in order to improve the quality of the plate surface, the rollers are often rolled less than 3 times on average before they have to be taken off the machine for re-grinding, resulting in great roller losses. Frequent grinding of rollers will lead to frequent shutdowns for roller replacement, resulting in downtime losses, and will also cause unstable quality of rolled slabs.

[0010] There are three types of iron oxides. One is ferrous oxide (FeO). FeO is a metal-deficient p-type semiconductor with about 5% to 16% cation defects. Therefore, there is a higher concentration of cation vacancies in the FeO layer, which makes the mobility of cations and electrons in the FeO layer very high, so the growth rate of the FeO layer is very fast. However, FeO is black, has a loose structure, and is easy to fall off.

[0011] The second is iron oxide (Fe2O3). Fe2O3 is an oxygen-deficient n-type semiconductor with a relatively high oxygen content. There are many oxygen ion defects inside, forming anion vacancies, which is conducive to the diffusion of oxygen from the outside to the inside. Fe2O3 has two crystal structures. At low temperatures, it is a metastable γ-Fe2O3 cubic crystal, and above 400°C, it is an oblique hexahedral α-Fe2O3. Fe2O3 is red. The main component of reddish-brown rust is iron oxide with n crystal water (Fe2O3·nH2O).

[0012] The third type is ferroferric oxide (Fe3O4). Fe3O4 is a p-type semiconductor and its stoichiometry is higher than that of FeO, so it is not conducive to Fe 2+ Diffusion, Fe3O4 consists of a Fe 2+ and two Fe 2+ , Fe 3+ Composition, belongs to spinel structure, Fe 2+ and Fe 2+ , Fe 3+They are located in the gaps between the tetrahedron and the octahedron. Fe3O4 is black, dense, and hard. It can be used as an abrasive and polishing agent, and it can also play a protective role. Therefore, in industry, a layer of Fe3O4 film is often formed on the surface of steel parts through blackening or bluing treatment to play an anti-corrosion role. Therefore, if a layer of Fe3O4 film that is closely combined with the substrate can be formed on the surface of the roller, it will greatly improve the high-temperature wear resistance of the roller, extend the life of the roller, and improve the surface quality of the rolled plate and strip.

[0013] like Figure 1 As shown, according to the iron-oxygen reaction phase diagram, there are two situations in which Fe3O4 can be stably generated. One is the low-temperature generation of Fe3O4. When the temperature is below 570°C and the oxygen content is less than 57at%, iron and oxygen can generate ferroferric oxide. Further, according to the relationship between Gibbs free energy and temperature in the oxidation reaction, Fe3O4 is the most stable among the oxidation products of pure iron below 567°C, and the thermodynamic tendency of generation is the greatest. Another situation is the high-temperature generation of Fe3O4, that is, at 1450-1582°C and the oxygen content is greater than 58at%, iron and oxygen can generate ferroferric oxide. In other cases, a mixture of ferrous oxide, trimerite and ferric oxide is generally generated.

[0014] For example, the prior art CN114622154A discloses a hot rolling roller surface laser forming prefabricated oxide film equipment and process, which produces the oxide film at 800°C to 900°C. However, according to the iron-oxygen reaction phase diagram, a large amount of fusate will be produced at this temperature, and no matter how long the temperature is kept, a high proportion of Fe3O4 cannot be obtained.

[0015] In fact, in the prior art, most of the methods for generating Fe3O4 oxide film at a temperature below 570°C are generally two ways.

[0016] One is high-temperature steam treatment. The specific method is to place the steel part in high-temperature steam at 540-570℃, so that a blue iron oxide (Fe3O4) film with a thickness of 4-6μm is formed on its surface. The structure of this oxide film is fine and can be firmly attached to the surface of the metal. The principle is that water vapor decomposes and releases active oxygen atoms when it contacts hot iron, and then the active oxygen atoms react with metal iron to form Fe3O4 cores, which grow and precipitate on the surface of the workpiece. High-temperature steam treatment requires the workpiece to be heated to about 550℃, and the high-temperature steam treatment time takes about 1 hour. In addition, the process time of heating the roller from room temperature to 550℃ and slowly cooling to room temperature after the blueing treatment is completed, for small workpieces, the whole process takes about 3 hours. This method itself has the problems of high energy consumption and long time. If this method is used to blue the surface of the high-speed steel roller, the high-speed steel roller is 5.5 meters long, the maximum diameter can reach 1 meter, and the weight can reach 30 tons. If the high-temperature steam method is used for treatment, there are many practical difficulties. For example, it is difficult to find such a huge heating furnace, and the heating cost is too high. Second, it takes more than 10 hours to heat a 30-ton roll to 550°C. Third, once heated to 550°C, the high-speed steel roll will soften due to tempering, reducing the roll hardness and causing the roll to be scrapped. Fourth, during the air cooling process, the high-speed steel roll is very brittle and the roll surface may crack. Therefore, it is not feasible to use the high-temperature bluing method to treat the high-speed steel roll.

[0017] The second method to generate Fe3O4 oxide film is alkali boiling oxidation. The specific method is to put the steel parts into a mixed solution of NaOH and NaNO2 at a certain concentration at about 140°C, and generate Fe3O4 oxide film through chemical reaction. The thickness and density of the film are related to the concentration of NaOH and NaNO2, temperature and treatment time during oxidation. If the temperature is too low, the nucleation rate and growth rate of Fe3O4 are low, and the oxide film is difficult to form. If the temperature is too high, the oxide film is easily dissolved, so the treatment temperature needs to be strictly controlled between 130 and 150°C. This method itself has serious pollution, and the strong alkali solution will lead to a bad working environment after evaporation. For high-speed steel with high alloy content, the cooking time in alkali solution is much higher than that of ordinary carbon steel, which takes about 80 minutes. If the alkali boiling oxidation method is used to generate Fe3O4 oxide film on the surface of high-speed steel rolls, there are the following problems: first, the processing time is long, and the alkali boiling alone requires 80 minutes. In addition, the 30-ton roll must be heated to 130°C before it can be placed in the high-temperature alkali solution pool, otherwise the alkali solution temperature in the entire alkali boiling pool will be reduced. It takes at least 3 hours to heat the 5.5-meter-long, 1-meter-diameter, and 30-ton roll to about 140°C. In addition to the surface cleaning process after being lifted out of the alkali boiling pool, it takes at least 6 hours to process a roll; second, there is serious pollution, the alkali solution volatilizes and pollutes the working environment, and the residual alkali solution on the surface of the roll needs special treatment; third, the processing cost is high, and a huge high-temperature alkali solution pool is required; fourth, the quality of the oxide scale is difficult to guarantee, and the thickness and uniformity of the oxide film are greatly affected by the concentration and temperature of the alkali solution. Such a huge alkali solution pool has large fluctuations in the concentration and temperature of the alkali solution, and it is difficult to guarantee the consistency of the quality of the oxide film generated on the surfaces of different rolls. Even for the same roll, the quality of the oxide film will be uneven and inconsistent due to differences in concentration, temperature, and alkali solution flow rate.

[0018] The reason why the prior art does not use high temperature (1450-1582°C) to form the Fe3O4 oxide film is that, firstly, the prior art heats the workpiece as a whole, which consumes too much energy. When the workpiece is heated to such a high temperature, the workpiece will soften. During the cooling process, it will crack due to uneven internal and external temperatures, and the material will also undergo phase change. In addition, the processing time is long, the required site is large, the equipment is complex, and a high-concentration oxygen atmosphere (oxygen content greater than 58at%) needs to be formed, which is difficult to implement in terms of performance, cost, and efficiency.

[0019] Second, from Figure 1 It can be seen from the iron-oxygen reaction phase diagram that the area where the Fe3O4 oxide film is formed under high temperature conditions is very narrow, and the conditions are harsh. If the temperature is lower than 1450°C, the Fe3O4 oxide film cannot be formed, and once it is higher than 1500°C, it will cause the steel material to melt, so the processing temperature needs to be precisely controlled. On the other hand, if only air or oxygen is provided, since the oxygen provided in air and oxygen is oxygen molecules, not active oxygen atoms, it cannot react quickly with steel to form an oxide film. Summary of the invention

[0020] One advantage of the present invention is that it provides a laser high-temperature flash formation method for an oxide film on the surface of a steel material. This method is the first to propose a method for flash generating an Fe3O4 oxide film at a high temperature (1450-1500°C), thereby solving the problem that the traditional generation of an Fe3O4 oxide film can only be carried out slowly at a low temperature.

[0021] One advantage of the present invention is that it provides a laser high-temperature flash method for forming an oxide film on the surface of a steel material, wherein the Fe3O4 oxide film generated in situ on the surface of the steel material by the laser high-temperature flash method is tightly bonded to the steel material matrix, thereby solving the problem that traditional oxidation methods are prone to generate FeO and have low bonding strength.

[0022] One advantage of the present invention is that it provides a laser high-temperature flash method for forming an oxide film on the surface of a steel material, wherein the laser high-temperature flash method for forming an oxide film on the surface of a steel material can form a stable Fe3O4 oxide film on the surface of the steel material, and the operating conditions are simple and the production cost is low, thereby solving the problems of long oxidation time, high temperature and high energy consumption of traditional oxidation methods.

[0023] Another advantage of the present invention is to provide a laser high-temperature flash method for forming an oxide film on the surface of a steel material, wherein an activation liquid is coated on the surface of the steel material to form an activation film, wherein the activation film can absorb light and increase the laser light absorption rate, and can also form active Fe in the activation film in advance or at the same time as the laser forms a high temperature. 2 + , Fe 3+ ions, at the same time, the activated membrane can release active oxygen atoms and active Fe 2+ , Fe 3+ Ions and active oxygen atoms can combine quickly to flash generate Fe3O4 oxide film, thus solving the problem of high laser reflectivity and low light absorbance on the steel surface, and also solving the problem of long oxidation reaction time of traditional steel, making millisecond-level flash oxidation possible.

[0024] Another advantage of the present invention is that it provides a laser high-temperature flash method for forming an oxide film on the surface of a steel material, wherein the laser high-temperature flash method for forming an oxide film on the surface of a steel material can form an Fe3O4 oxide film in an extremely short time (such as 0.01 to 10 milliseconds).

[0025] Another advantage of the present invention is that it provides a laser high-temperature flash formation method for an oxide film on the surface of a steel material. By rapidly scanning the surface of the steel material with a high-energy laser beam used for heating, local high temperature is formed only at a micron-level depth at the laser spot on the surface of the steel material, thereby solving the problems of the traditional method requiring overall heating, complex equipment, large site, high energy consumption, and low efficiency.

[0026] In order to achieve at least one of the above advantages, the present invention provides a laser high-temperature flash forming method for an oxide film on the surface of a steel material, the laser high-temperature flash forming method for an oxide film on the surface of a steel material comprising:

[0027] Applying an activation liquid on the surface of the steel material where the Fe3O4 oxide film needs to be formed, so as to form an activation film on the surface of the steel material; and

[0028] The surface of the steel material on which the Fe3O4 oxide film is to be formed is scanned with a laser beam for heating, so that the laser scanning spot on the surface of the steel material is heated to 1450-1500° C., thereby generating the Fe3O4 oxide film at a flash speed.

[0029] According to one embodiment of the present invention, the activation film contains Fe 2+ , Fe 3+ ion.

[0030] According to one embodiment of the present invention, pre-treating the surface of the steel material comprises:

[0031] Grinding the surface of steel materials to remove the surface fatigue layer; and / or

[0032] Clean the emulsion or oil on the surface of the steel material by alkali, and remove the emulsion or oil on the surface of the steel material by water washing; and / or

[0033] Wipe the steel surface with alcohol.

[0034] According to an embodiment of the present invention, the activation solution is an activation solution containing oxygen acid ions.

[0035] According to an embodiment of the present invention, the activation solution containing oxygen acid radical ions is an activation solution containing phosphate ions and / or sulfate ions and / or nitrate ions and / or hypochlorite ions.

[0036] According to an embodiment of the present invention, the laser high-temperature flash method for forming an oxide film on the surface of a steel material comprises the following steps:

[0037] Before or simultaneously with the laser beam scanning, a light absorber is coated on the surface of the activation film.

[0038] According to an embodiment of the present invention, the light absorber is a carbon-based light absorber.

[0039] According to an embodiment of the present invention, the steel material is a rolling mill roll.

[0040] According to an embodiment of the present invention, while the surface of the steel material is irradiated with a laser beam for heating, oxygen is sprayed toward the laser spot on the surface of the steel material.

[0041] According to an embodiment of the present invention, the flow rate of the oxygen is 0.1-15 L / min.

[0042] According to an embodiment of the present invention, the time for generating the oxide film is 0.01 to 10 milliseconds.

[0043] According to an embodiment of the present invention, the color of the activation film is dark.

[0044] According to an embodiment of the present invention, the activation solution is an activation solution containing oxygen-free acid radical ions, wherein the laser high-temperature flash method for forming an oxide film on the surface of a steel material comprises:

[0045] While irradiating the surface of the steel material with a laser beam for heating, oxygen is sprayed toward the laser spot on the surface of the steel material.

[0046] According to an embodiment of the present invention, the activation solution is an activation solution containing halogen ions. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 The iron-oxygen reaction phase diagram is shown.

[0048] Figure 2 A flow chart of a method for laser high-temperature flash formation of an oxide film on the surface of a steel material in one embodiment is shown. DETAILED DESCRIPTION

[0049] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art can think of other obvious variations. The basic principles of the present invention defined in the following description can be applied to other embodiments, variations, improvements, equivalents, and other technical solutions that do not deviate from the spirit and scope of the present invention.

[0050] Those skilled in the art should understand that, in the disclosure of the present invention, the terms "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicating the orientation or position relationship are based on the orientation or position relationship shown in the drawings, which are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation. Therefore, the above terms should not be understood as limiting the present invention.

[0051] It is to be understood that the term "one" should be understood as "at least one" or "one or more", that is, in one embodiment, the number of an element may be one, while in another embodiment, the number of the element may be multiple, and the term "one" should not be understood as a limitation on the quantity.

[0052] refer to Figure 2 According to a preferred embodiment of the present invention, a laser high-temperature flash method for forming an oxide film on the surface of a steel material will be described in detail below. The laser high-temperature flash method for forming an oxide film on the surface of a steel material comprises the steps of:

[0053] S1001, the activation liquid is applied to the surface of the steel material where the Fe3O4 oxide film is to be formed, such as the surface of the roll, to form a layer containing Fe3O4 on the surface of the steel material. 2+ , Fe 3+ Activated membrane of ions.

[0054] In one embodiment, the activation solution is implemented as an activation solution containing oxygen acid ions.

[0055] As an example, the activation liquid is implemented as sulfuric acid or / and sulfate, and sulfuric acid or / and sulfate is applied to the surface of a steel material such as a roller to pre-activate the roller surface, so that the iron element on the surface of the steel material reacts with sulfate ions, and a layer of FeSO4 or Fe2(SO4)3 activation film is generated according to different sulfate ion concentrations and reaction temperatures. Compared with Fe atoms, Fe 2+ , Fe 3+ The ions are more active, which in turn increases the activity of the oxidation reaction, so that a layer of Fe3O4 oxide film can be flash-formed on the steel material at high temperatures.

[0056] In addition, SO4 2— It decomposes at high temperatures to produce active [O] elements, which are more likely to promote the formation of Fe3O4 oxide film than oxygen.

[0057] By forming a layer containing Fe on the surface of the steel material 2+ , Fe 3+ Ion-activated membrane, due to the Fe 2+ , Fe 3+ The ions are highly active and can rapidly form Fe3O4 oxide films in high temperature environments.

[0058] For example, in one example, a layer containing Fe is formed on the surface of the steel material by coating sulfuric acid or / and sulfate. 2+ , Fe 3+Ion activation film. Sulfuric acid or sulfate reacts with iron and steel materials such as iron on the surface of the roller to form FeSO4, Fe2(SO4)3 film. The color of FeSO4, Fe2(SO4)3 film is yellow, yellow-brown, brown or brown-black. The specific color is determined by the length of time of action. The longer the time, the darker the color.

[0059] Without this dark activation film, the surface color of the roller after grinding is bright silver, and the reflectivity of the laser is extremely high. On the one hand, it will lead to low laser efficiency. On the other hand, since the surface of the roller is a circular arc surface, the reflectivity of the laser on the roller surface is different, that is, the absorbance of the same spot at different positions is different. The different absorbance will lead to different temperatures, which will lead to uneven oxide film, thus causing uneven Fe3O4 oxide film generated later. Therefore, the activation treatment of the roller surface with the activation solution has three effects at the same time. On the one hand, it forms active Fe 2+ , Fe 3+ ions and active [O] elements, which promote the rapid formation of Fe3O4 oxide film. Secondly, the dark iron nitrate film can greatly improve the absorbance. Thirdly, it ensures the uniformity and consistency of the quality of the generated Fe3O4.

[0060] More importantly, since the activated film can release active [O] elements after decomposition at high temperature, there is no need for additional oxygen to be introduced, and the Fe3O4 oxide film can be quickly formed on the surface of the steel material at high temperature (1450-1500°C).

[0061] Preferably, in step S1001, when sulfuric acid or / and sulfate is used as the activation solution, the sulfate ions [SO4 2- ] The concentration is 0.5~15mol / L.

[0062] In another embodiment, the oxygen-containing acid radical ion activation solution is implemented as a nitrate ion (NO3 - ) to form active Fe 2+ , Fe 3+ It is understood that the nitrate ion (NO3 - ) can also provide active [O] elements when it forms a high temperature under subsequent laser beam irradiation, thereby promoting the rapid formation of Fe3O4 oxide film. In addition, the generation of nitrate ions (NO3 - ) is used, the surface of the steel material gradually changes from silvery white to a dark color, such as yellow, brown, or brown-black, which can increase the laser absorbency and significantly reduce laser reflection.

[0063] In another embodiment, the oxygen-containing acid radical ion activation solution is implemented as a solution containing hypochlorite ions (ClO - ) to form active Fe 2+ , Fe 3+ It is understood that the ferrous hypochlorite and ferric chloride containing hypochlorite ions (ClO - ) activated film can provide active [O] elements by decomposition when the subsequent laser beam forms a high temperature, thereby promoting the rapid formation of Fe3O4 oxide film. In addition, the generation of chlorohypochlorite (ClO - ) after the activation film is formed, the surface of the steel material gradually changes from silvery white to dark colors, such as green, yellow-green, and yellow, which increases the laser absorbency and reduces the laser reflection.

[0064] In another embodiment, the oxygen-containing acid radical ion activation solution is implemented as an iron-based phosphating solution containing phosphate ions.

[0065] Preferably, the main components of the iron-based phosphating solution are phosphoric acid (H3PO4) and sodium dihydrogen phosphate (NaH2PO4), the oxidant is NaNO3, Fe 2+ , Fe 3+ It is generated by the reaction between the iron atoms on the surface of the steel material and the phosphating liquid.

[0066] It is worth mentioning that, in the present embodiment, the iron-based phosphating solution has a phosphate concentration of 10 to 30 g / L and a pH value of 2.0 to 3.0.

[0067] According to the different components of the phosphating solution, phosphating treatment includes zinc-based, manganese-based, zinc-calcium-based and iron-based phosphating. The characteristic of iron-based phosphating is that the phosphating solution contains Fe 2+ , Fe 3+ Ions, iron ions can be provided by dissolving on the surface of steel. Compared with zinc, manganese and zinc-calcium systems, iron phosphating has thin phosphating film thickness (less than 1μm), high porosity and low density (film weight 0.2-1g / m 2 ) characteristics, the color of the phosphating film is mostly blue-purple, and can be rainbow-colored or gray depending on the reaction time, film thickness, and composition of the phosphating solution. Therefore, the dark iron-based phosphating film can be used as a laser light absorber, and its thin thickness and high porosity allow oxygen to pass through the phosphating film and contact the iron element of the steel matrix. Therefore, the present invention selects an iron-based phosphating solution to activate the surface of the steel workpiece.

[0068] During the phosphating process, the surface of the steel substrate reacts with the phosphoric acid or hypophosphite in the phosphating solution, where the atoms on the outer layer of the steel workpiece react with the anions in the solution as a medium, and the soluble phosphate on the surface is continuously converted into insoluble phosphate, and finally a phosphate conversion film is deposited on the surface of the steel workpiece. The main components of the iron phosphating film are FePO4, Fe3(PO4)2 and Fe(OH)3.

[0069] In this embodiment, the phosphate (PO4 3- ) concentration range is different from that of ordinary phosphating solution. The phosphate (PO4 3- ) concentration is 10-30 g / L, while the concentration of phosphate in ordinary phosphating solution is generally greater than 30 g / L. In the present invention, if phosphate (PO4 3- ) concentration is less than 10g / L, the film is too thin and the color is too light, which is not conducive to improving the absorbance. 3- ) concentration is greater than 30g / L, the film thickness is too large, the compactness is increased, and it is not conducive to the subsequent oxygen penetration. For ordinary phosphating solution, the purpose is to obtain a phosphating film with low porosity, high corrosion resistance and large thickness. For the present invention, the purpose is to obtain a phosphating film with blue-purple, rainbow or gray, loose and porous, and thin thickness, so the phosphating process parameter selection ranges of the two are different.

[0070] The phosphate film in this embodiment is characterized by blue-purple, rainbow or gray color, thin thickness and low corrosion resistance to improve laser absorption rate.

[0071] The pH value of the phosphating solution in this embodiment is also different from that of the traditional phosphating solution. The pH value of the phosphating solution in the present invention is 2.0-3.0, while the pH value of the traditional phosphating solution is generally 3.0-4.5. When the pH value is low, the amount of hydrogen evolution is large and the film layer is loose and porous. However, when the pH value is lower than 2.0, local corrosion is too fast, resulting in an uneven phosphating film. When the pH value exceeds 3.0, the film density increases, the film thickness increases, and it is not conducive to the oxygen penetration of the subsequent oxygen injection process. In order to generate a phosphating film with good density, large thickness and corrosion resistance, the pH value of the phosphating solution is relatively high in the traditional phosphating treatment. In another embodiment, the activation solution can also be implemented as an activation solution without oxygen acid ions.

[0072] Preferably, the activation solution of the oxygen-free acid radical ions can be implemented as an activation solution containing halogen ions.

[0073] For example, the oxygen-free acid radical ion activation solution is implemented as a chloride ion (Cl - ) to form active Fe 2+ , Fe 3+ The active Fe contained in the activated film 2+ , Fe3+ Ions are beneficial to the rapid formation of Fe3O4 oxide film. However, compared with the activation solution containing oxygen acid radical ions, the chloride ion (Cl - ) is unable to provide active [O] elements when it forms a high temperature under subsequent laser beam irradiation. Therefore, when the laser is irradiating the surface of the steel material, oxygen must be sprayed onto the laser spot on the surface of the material at the same time.

[0074] In one embodiment, the activation solution of the oxygen-free acid radical ion can be implemented as a solution containing chloride ions (Cl - ) activation solution. Containing chloride ions (Cl - ) is used, the surface of the steel material gradually changes from silvery white to a dark color, such as yellow, brown, or brown-black, which can increase the laser absorbency and significantly reduce laser reflection.

[0075] In another embodiment, the oxygen-free acid radical ion activation solution is implemented as a bromide ion (Br - ) to form active Fe 2+ , Fe 3+ Ion ferrous bromide, ferric bromide activation film. The active Fe contained in the activation film 2+ , Fe 3+ Ions are beneficial to the rapid formation of Fe3O4 oxide film. However, compared with the activation solution containing oxygen acid radical ions, the chloride ion (Cl - ) activated film is unable to provide active [O] elements when it is formed under the subsequent laser beam irradiation and high temperature. Therefore, when the laser irradiates the surface of the steel material, oxygen must be sprayed to the laser spot on the surface of the material at the same time. - ) is used, the surface of the steel material gradually changes from silvery white to a dark color, such as brown, reddish brown, and tan, which can increase the laser absorbency and significantly reduce laser reflection.

[0076] It will be understood by those skilled in the art that the above-mentioned activation solution is used to form the Fe-containing 2+ , Fe 3+ The surface of the ion activation film is dark in color, which is darker and more uniform in color than the steel material without the activation film. This can effectively prevent the reflection of subsequent lasers and maintain the consistency of light absorption, so that the surface of the steel material can be uniformly heated to a high temperature by the laser, thereby ensuring the uniformity of the thickness of the Fe3O4 oxide film formed subsequently.

[0077] The laser high-temperature flash method for forming an oxide film on the surface of a steel material comprises the following steps:

[0078] S1002, heating the surface of the steel material on which the Fe3O4 oxide film is to be formed to 1450-1500°C by using a laser beam for heating, so as to generate the Fe3O4 oxide film at a flash speed.

[0079] Specifically, in step S1002, a laser beam guided by a laser head is irradiated onto the surface of a steel material, such as the surface of a rolling roller.

[0080] The roller rotates at a high speed at a rotation speed ω, which is between 50rpm and 500rpm. At the same time, the laser head and the oxygen injection tube make a linear feed motion along the axial direction of the roller at a speed v. The feed speed v of the roller is 50-500mm / min, the spot area of ​​the laser beam is 0.05-2mm2, the overlap rate is 30-80%, and the laser power is 2000W-6000W.

[0081] While laser scanning the workpiece surface, if the activated film is produced by oxygen-free acid coating on the steel material surface, oxygen needs to be sprayed to the laser irradiation spot on the workpiece surface through the oxygen injection tube. If the activated film is produced by oxygen-containing acid coating on the steel material surface, oxygen can be sprayed to the laser irradiation spot on the workpiece surface through the oxygen injection tube, or oxygen can be not sprayed. The flow rate of the oxygen is 0.1-15L / min. Under the irradiation of the high-energy laser beam, the temperature at the laser spot on the roller surface instantly rises to 1450-1500℃, and the Fe3O4 oxide film is instantly produced in situ on the roller surface. .

[0082] Preferably, the laser high-temperature flash method for forming an oxide film on the surface of a steel material comprises the steps of:

[0083] S1003, pre-treating the surface of the steel material. Those skilled in the art should understand that step S1003 includes:

[0084] S100331, grinding the surface of steel materials to remove the surface fatigue layer.

[0085] More preferably, the step S1003 includes:

[0086] S10032, use alkali to clean the emulsion or oil stains on the surface of the steel material, and then use water to remove the emulsion or oil stains on the surface of the steel material.

[0087] Preferably, after step S10032, pre-treating the surface of the steel material further comprises:

[0088] S10033, wipe the surface of steel materials with alcohol.

[0089] It is particularly worth mentioning that if there is residual emulsion or oil on the surface of the steel material, the uniformity of the activated film in the subsequent pre-activation process cannot be guaranteed.

[0090] In addition, in step S1002, the surface of the steel material is irradiated by a high-energy laser beam, so that sufficient heat can be instantly provided to heat the surface of the roll to the required temperature. In order to quickly heat the surface of the roll to 1450-1500°C, the present invention adopts high-power and small spot to obtain high energy density, and the high power refers to a laser with a power of 2000W-10000W. If the laser power is less than 2000W, the energy is insufficient, and the spot is too small, which will reduce the efficiency of oxide film generation. If the laser power is greater than 10000W, the energy is too large, which may cause overburning, and the steel material needs to move at a too high speed, which is difficult to match the corresponding motion mechanism. Therefore, the laser power is preferably 2000W-10000W.

[0091] The spot shape formed by the laser beam can be a small circular, square or rectangular spot, wherein the small spot refers to a spot with an area of ​​0.05 to 10 mm 2 If the laser spot area is less than 0.05mm 2 , it will seriously reduce production efficiency. And the spot area is greater than 10mm 2 , the energy density is insufficient, and the surface temperature of the steel material is difficult to reach 1450-1500°C, so the spot area is 0.05-10mm 2 The spot overlap rate is 30% to 80%. If the spot overlap rate is less than 30%, the laser energy is insufficient due to the virtual light effect at the edge of the laser spot, resulting in the inability to form a Fe3O4 oxide film. If the overlap rate is greater than 80%, the steel material may be melted and the generation efficiency will be reduced.

[0092] In one embodiment, the steel material is set as a rolling roller. During the preparation process, the speed of the rolling roller is ω and the speed range is 50 to 500 rpm. If the laser power is large, the speed can be appropriately increased. If the speed is lower than 50 rpm, the production efficiency is low. If the speed exceeds 500 rpm, since the weight of the rolling roller can reach 30 tons, excessive speed will cause production safety hazards, so the speed should be 50 to 500 rpm.

[0093] Correspondingly, in the present embodiment, the linear feed speed v of the laser head along the axial direction of the roller is in the range of 50 to 500 mm / min. If the feed speed is lower than 50 mm / min, firstly, the production efficiency is low, and secondly, the roller surface is melted due to overburning caused by excessive power density. If the feed speed is higher than 500 mm / min, the power density on the roller surface is too low and the Fe3O4 oxide film cannot be generated.

[0094] Furthermore, the second condition for forming an oxide film at high temperature is that the oxygen content is greater than 58at%, while the oxygen content in the atmosphere is only 21at%. If the oxygen content is insufficient, Fe3O4 cannot be generated even if the temperature reaches 1450-1500°C. The activation film in the present invention can be generated by coating an oxygen-containing acid or an oxygen-free acid activation liquid on the surface of a steel material. If the activation film is generated by coating an oxygen-containing acid activation liquid on the surface of a steel material, the activation film can provide a large amount of active oxygen atoms when heated by laser irradiation, satisfying the conditions required for forming the Fe3O4 oxide film. If the activation film is generated by coating an oxygen-free acid activation liquid on the surface of a steel material, oxygen needs to be sprayed onto the laser spot on the surface of the steel material.

[0095] Of course, as a preferred embodiment, the laser high temperature flash forming method of the oxide film on the surface of the steel material comprises the steps of:

[0096] S1004, while irradiating the surface of the steel material with a laser beam, spraying oxygen toward the laser spot on the surface of the steel material.

[0097] It is worth mentioning that if the activation film is formed by coating the surface of the steel material with an oxygen-containing acid activation liquid, this step is optional. If the activation film is formed by coating the surface of the steel material with an oxygen-free acid activation liquid, this step is necessary.

[0098] It is worth mentioning that the injected oxygen is directed toward the light spot formed by the laser beam on the surface of the steel material.

[0099] The present invention proposes a method of spraying oxygen onto the surface of the roller. For example, oxygen can be sprayed from the jet pipe onto the laser spot to provide sufficient oxygen elements for the oxidation of the roller surface. The oxygen flow rate is 0.1 to 15 L / min. If the oxygen flow rate is less than 0.1 L / min, the oxygen supply is insufficient. If the oxygen flow rate is greater than 15 L / min, the oxygen supply is excessive.

[0100] Furthermore, the study found that if the activation liquid is not applied to the surface of the steel material and no activation film is formed, even if oxygen is sprayed on the surface of the roll, the effect of forming the Fe3O4 oxide film is still not ideal, the oxide film is thin and uneven. The reason for this is that if the Fe3O4 oxide film is to be formed quickly, Fe 2+ , Fe 3+ ions. In order to form Fe on the roller surface before laser oxidation 2+ , Fe 3+ ions, we apply the activation solution containing oxygen-containing acid radical ions and / or oxygen-free acid radical ions on the roller surface, such as sulfate ions [SO4 2- ] activation liquid, so that the iron element on the surface of the roller reacts with sulfate ions to form Fe 2+ , Fe3+ ions, thereby increasing the activity of the oxidation reaction. On the other hand, at the same time, (SO4 2- )'s activated film decomposes at high temperatures to produce active [O] elements, which are highly active and more effective than oxygen in promoting the formation of Fe3O4 oxide film. 2- ) concentration is controlled at 0.5-15mol / L. If it is lower than 0.5mol / L, the reaction is too slow. If it is higher than 15mol / L, the concentration is too high and it will volatilize and cause environmental pollution. If the concentration is too high, the surface may be passivated, which is not conducive to the generation of iron ions. Laser oxidation treatment can be carried out 3-60 minutes after the activation solution is applied. If it is lower than 3min, the reaction is incomplete, the degree of activation is low, and the oxide film is thin. If it exceeds 60 minutes, over-reaction occurs, resulting in uneven thickness and color of the activation film, resulting in uneven Fe3O4 oxide film. Preferably, the laser high-temperature flash formation method of the oxide film on the surface of the steel material comprises the steps of:

[0101] S1005, further coating a light absorbent on the surface of the activated film of the steel material to form a light absorbing layer on the surface of the steel material to further improve the light absorbance.

[0102] It is worth mentioning that in a modified embodiment, the activation liquid may not be applied to the surface of the steel material, but the light absorber may be directly applied to the surface of the steel material, and oxygen may be sprayed to the laser spot on the surface of the steel material while the laser beam is irradiated on the surface of the steel material. In this way, the Fe3O4 oxide film may be flash-formed on the surface of the steel material at a high temperature of 1450-1500°C.

[0103] It is understandable that, since the light absorber is coated on the surface of the steel material, when the laser beam is subsequently irradiated on the surface of the steel material, the efficiency of the steel material absorbing the laser can be improved, so that the surface of the steel material can be flash-heated to 1450-1500°C. It is understandable that the melting point of high-speed steel is generally between 1500-1600°C, and the steel material will melt if it exceeds this temperature range. Therefore, the temperature of laser oxidation should be controlled below 1500°C. In order to form the Fe3O4 oxide film on the surface of the steel material, the temperature must be controlled at 1450-1500°C, and this temperature range is very close to the melting range of the steel material. If the laser is used alone to heat the steel material, and the light absorption efficiency of the steel material surface is low, the absorption rate of the laser is difficult to control, which may cause the steel material to melt during the heating process. In other words, the coated light absorber can effectively stabilize the temperature of laser heating and prevent the steel material from melting during the heating process.

[0104] The light absorber is preferably a carbon-based light absorber. The carbon-based light absorber can be set as a carbon-based micropowder dispersion, in which the carbon-based micropowder is evenly dispersed in a solvent. For example, the carbon-based micropowder can be a carbon-based powder material such as flake graphite, graphene, carbon nanotubes, etc. with a characteristic size between 10nm and 100μm. The solvent is formed by adding a surfactant such as sodium carboxymethyl cellulose, polyvinyl alcohol (PVA), polyvinyl pyrrolidone (PVP), sodium dodecylbenzene sulfonate, etc. to an organic or inorganic solvent such as water, ethanol, ethylene glycol or acetone, and then the carbon-based micropowder can be evenly dispersed in the solvent through processes such as stirring and ultrasonic vibration.

[0105] When the light absorber is implemented as a carbon-based light absorber, the carbon-based light absorber will cover the surface of the Fe3O4 oxide film with a layer of carbon-based lubricating film, which can reduce the surface friction of the steel material and thus reduce the wear of the steel material.

[0106] According to another aspect of the present invention, the present invention also provides a rolling mill having the Fe3O4 oxide film on its surface formed by the above-mentioned laser high-temperature flash forming method of the oxide film on the surface of the steel material.

[0107] Example 1

[0108] On a hot finishing rolling 1780 production line, the F1 mill roll was originally a high-speed steel roll. On the basis of the high-speed steel roll, a layer of Fe3O4 oxide film was prepared. The thickness of the oxide film was 5μm. The average millimeter rolling volume of the original roll was 4300 tons. After the new Fe3O4 oxide film composite roll was used, the millimeter rolling volume reached 12360 tons, and the service life was increased by 3 times. The preparation method of the Fe3O4 oxide film consists of three steps. The first step is the roller surface treatment. The F1 roller is ground on a grinder after it is removed from the machine. The surface roughness after grinding is 0.5μm. Alkaline washing is used for degreasing, and finally it is washed and dried. The surface of the roller after pretreatment is bright silver; the second step is surface pre-activation. The activation liquid is a H2SO4 solution with a concentration of 3mol / L. The activation liquid is coated on the roller surface to form a layer of yellow activation film on the roller surface to form an active Fe 2+ , Fe 3+ ions, the roller surface after surface pre-activation treatment is yellow-brown; the third step, laser rapid oxidation, laser power 6kw, circular spot, spot diameter 3mm, overlap rate 50%, roller speed 160rpm, laser head axial feed speed 200mm / min, oxygen flow 5L / min, for the roller that has been fully laser oxidized, the roller is covered with a black Fe3O4 oxide film.

[0109] Example 2

[0110] On a hot finishing rolling 1422 production line, the F2 mill roll was originally a high-speed steel roll. On the basis of the high-speed steel roll, a layer of black Fe3O4 oxide film was prepared. The thickness of the oxide film was 7μm. The average millimeter rolling volume of the original roll was 8200 tons. After the new Fe3O4 oxide film composite roll was used, the millimeter rolling volume reached 46300 tons, and the service life was increased by more than 5 times. The preparation method of the Fe3O4 oxide film consists of three steps. The first step is the surface treatment of the roll. The F2 roll is ground on a grinder after it is removed from the machine. The surface roughness after grinding is 0.3μm. Alkaline washing is used for degreasing, and finally it is washed with water and dried. The second step is surface pre-activation. The activation liquid is a NiSO4 solution with a sulfate ion concentration of 6mol / L. A yellow-green activation film is generated on the surface of the roll to form an active Fe 2+ , Fe 3+ ions; the third step is laser rapid oxidation, laser power 8kw, circular spot, square spot with side length of 2.5mm, overlap rate 30%, roller speed 200rpm, laser head axial feed speed 260mm / min, oxygen flow rate 10L / min.

[0111] Example 3

[0112] On a hot finishing rolling 2250 production line, the F4 mill roll was originally a high-speed steel roll. On the basis of the high-speed steel roll, a layer of black Fe3O4 oxide film was prepared. The thickness of the oxide film was 8μm. The average millimeter rolling volume of the original roll was 6500 tons. After the new Fe3O4 oxide film composite roll was used, the millimeter rolling volume reached 26370 tons, and the service life was increased by more than 4 times. The preparation method of the Fe3O4 oxide film consists of three steps. The first step is the surface treatment of the roll surface. The F4 roll after the machine is ground on a grinder. The surface roughness after grinding is 0.6μm. Alkaline washing is used for degreasing, and finally it is washed with water and dried. The second step is surface pre-activation. The activation solution is a mixed solution of Cu(NO3)2 and Y(NO3)3 with a nitrate ion concentration of 12mol / L. A brown activation film is generated on the surface of the roll to form an active Fe 2+ , Fe 3+ ions; the third step is laser rapid oxidation, the laser power is 10000kw, a rectangular laser spot is used, the spot length is 3mm, the width is 2mm, the overlap rate is 50%, the roller speed is 300rpm, the laser head axial feed speed is 300mm / min, and the oxygen flow rate is 12xL / min.

[0113] Example 4

[0114] On a hot finishing rolling 1780 production line, the F3 mill roll was originally a high-speed steel roll. On the basis of the high-speed steel roll, a layer of black Fe3O4 oxide film was prepared. The thickness of the oxide film was 4μm. The average millimeter rolling volume of the original roll was 9100 tons. After the new Fe3O4 oxide film composite roll was used, the millimeter rolling volume reached 27650 tons, and the service life was increased by more than 3 times. The preparation method of the Fe3O4 oxide film consists of three steps. The first step is the surface treatment of the roll surface. The F3 roll is ground on a grinder after it is removed from the machine. The surface roughness after grinding is 0.3μm. Alkaline washing is used for degreasing, and finally it is washed with water and dried. The second step is surface pre-activation. The activation solution is a FeCl3 mixed solution with a chloride ion concentration of 7mol / L. A brown-black activation film is generated on the surface of the roll to form an active Fe 2+ , Fe 3+ ions; the third step is laser rapid oxidation, the laser power is 6000kw, a rectangular laser spot is used, the spot length is 2mm, the width is 2mm, the overlap rate is 50%, the roller speed is 200rpm, the laser head axial feed speed is 200mm / min, and the oxygen flow rate is 15L / min.

[0115] It should be understood by those skilled in the art that the embodiments of the present invention described above and shown in the accompanying drawings are only examples and do not limit the present invention. The advantages of the present invention have been fully and effectively achieved. The functional and structural principles of the present invention have been demonstrated and explained in the embodiments, and the embodiments of the present invention may be deformed or modified in any way without departing from the principles.

Claims

1. A laser high-temperature flash method for forming an oxide film on the surface of a steel material, characterized in that: The laser high-temperature flash method for forming an oxide film on the surface of a steel material comprises: Applying an activation liquid on the surface of a steel material on which a Fe3O4 oxide film is to be formed, so as to form an activation film on the surface of the steel material; Coating a light absorber on the surface of the activated film; Scanning the surface of the steel material on which the Fe3O4 oxide film is to be formed by a laser beam for heating, so that the laser scanning spot on the surface of the steel material is heated to 1450-1500° C., and the Fe3O4 oxide film is formed at a flash speed; While the surface of the steel material is irradiated with a laser beam for heating, oxygen is sprayed toward the laser spot on the surface of the steel material.

2. The laser high-temperature flash forming method for the oxide film on the surface of steel material according to claim 1, characterized in that: Pre-treating the surface of the steel material comprises: Grinding the surface of steel materials to remove the surface fatigue layer; and / or Clean the emulsion or oil on the surface of the steel material by alkali, and remove the emulsion or oil on the surface of the steel material by water washing; and / or Wipe the steel surface with alcohol.

3. The laser high-temperature flash forming method for the oxide film on the surface of steel material according to claim 1, characterized in that: The light absorber is a carbon-based light absorber.

4. The laser high-temperature flash forming method for the oxide film on the surface of steel material according to claim 1, characterized in that: The flow rate of the oxygen is 0.1 to 15 L / min.

5. The laser high-temperature flash forming method for the oxide film on the surface of a steel material according to any one of claims 1 to 3, characterized in that: The time for generating the oxide film is 0.01 to 10 milliseconds.

6. The laser high-temperature flash method for forming an oxide film on the surface of a steel material according to any one of claims 1 to 3, characterized in that: The spot shape formed by the laser beam is selected from a small spot of a circle, a square or a rectangle.

7. The laser high-temperature flash forming method for the oxide film on the surface of steel material according to claim 6, characterized in that: The small spot refers to a spot area of ​​0.05 to 10 mm 2 .

8. The laser high-temperature flash forming method for the oxide film on the surface of steel material according to claim 6, characterized in that: The steel material is a rolling mill roll.

9. The laser high-temperature flash forming method for the oxide film on the surface of steel material according to claim 6, characterized in that: The speed range of the roller speed ω during the preparation process is 50 to 500 rpm.

10. The laser high-temperature flash forming method for the oxide film on the surface of steel material according to claim 6, characterized in that: The linear feed speed v of the laser head forming the laser beam along the axial direction of the roller is in the range of 50 to 500 mm / min.