High-frequency low-dielectric polyphenylene ether composite resin with excellent comprehensive performance, preparation and application

By introducing benzoxazine functionalization and copolymerization of hydrocarbon resin into polyphenylene ether resin, a polyphenylene ether composite resin with excellent comprehensive properties such as low dielectric constant and high heat resistance is prepared, solving the existing technical problems. The problems of insufficient dielectric performance and poor processing performance have been solved to meet the application needs in the field of high-frequency communications.

CN115627065BActive Publication Date: 2024-10-29HUAIBEI OASIS NEW MATERIAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211203118.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-29
Publication Date
2024-10-29
Estimated Expiration
2042-09-29

AI Technical Summary

Technical Problem

Existing high molecular weight polyphenylene ether resins have insufficient dielectric properties in the field of high-frequency communications, poor processing performance, poor heat resistance and flame retardancy, and the preparation method is complex and costly.

Method used

Using a binary or ternary composite resin system of benzoxazine functionalized polyphenylene ether resin and hydrocarbon resin, low dielectric constant, low dielectric loss, high heat resistance and flexibility are prepared through simple chemical reactions. Polyphenylene ether composite resin uses the copolymerization reaction of benzoxazine functionalized polyphenylene ether and hydrocarbon resin to improve the compatibility and cross-linking density of the resin to achieve self-flaming retardant effect.

Benefits of technology

It achieves low dielectric constant and dielectric loss under ultra-high frequency conditions, provides excellent heat resistance and toughness, reduces preparation costs, simplifies the process flow, and achieves flame retardant effects without the need for external flame retardants. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_6
    Figure SMS_6
Patent Text Reader

Abstract

The present invention relates to a polyphenylene ether composite resin with excellent comprehensive performance, preparation and application. The composite resin is a benzoxazine functionalized polyphenylene ether / benzoxazine binary composite resin, a benzoxazine functionalized polyphenylene ether / carbon resin binary composite resin, or a benzoxazine functionalized polyphenylene ether / benzoxazine / carbon resin ternary composite resin obtained by curing a benzoxazine functionalized polyphenylene ether resin prepolymer, benzoxazine or / and a hydrocarbon resin prepolymer. The composite resin has low dielectric properties, high heat resistance, flexibility, and can even have self-flame retardant properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of organic polymer materials, and in particular to a high-frequency low-dielectric polyphenylene ether composite resin with excellent comprehensive performance, and its preparation and application. Background Art

[0002] Ultra-high frequency communication technology is a major strategic need of our country, a new opportunity to revitalize the real economy, and a new engine for building a network power. Printed circuit boards are important carriers for carrying electronic components and realizing electrical signal transmission. The base copper-clad laminate is made of glass fiber cloth coated (or impregnated) with polymer resin and then hot-pressed with copper foil. With the advent of the ultra-high frequency era, the requirements for the dielectric, heat-resistant and flame-retardant properties of polymer resins are getting higher and higher.

[0003] Polyphenylene ether resin is the fifth largest engineering plastic in the world, with advantages such as high tensile and flexural strength, small thermal expansion coefficient, low water absorption, and good dimensional stability. In particular, its excellent dielectric properties, i.e. low dielectric constant and low dielectric loss, have attracted much attention in the field of electronic communications. However, commercial high molecular weight polyphenylene ether resins have problems such as high melt viscosity, poor processing performance, poor solvent resistance, poor heat resistance and flame retardancy. Moreover, thermoplastic polyphenylene ether resins must be thermally cured when used as the matrix resin of printed circuit boards. The main modification methods of polyphenylene ether resin include preparing low molecular weight polyphenylene ether resin (number average molecular weight <4000g / mol) by monomer copolymerization and redistribution; introducing active groups on the terminal hydroxyl group, side methyl group and main chain of polyphenylene ether resin to prepare self-thermosetting polyphenylene ether resin or hyperbranched polyphenylene ether resin; forming binary and ternary composite resin systems with epoxy resin, cyanate resin, bismaleimide resin, polyolefin, etc.; and inorganic / organic composite with inorganic micro- and nanoparticles such as oligomeric silsesquioxane and nano-silica. In this way, the low dielectric properties of polyphenylene ether resin can be maintained and further improved as much as possible, while improving its processability, solvent resistance and heat resistance.

[0004] So far, benzoxazine resins have been widely used in high-frequency communications, aerospace, automotive industry and other fields. Benzoxazine is a class of nitrogen-oxygen heterocyclic intermediates synthesized by Mannich condensation reaction using phenols, aldehydes and primary amine compounds as raw materials. Benzoxazine resins can be obtained by thermal ring-opening polymerization. Benzoxazine resins have the advantages of good thermal properties, strong adhesion, high mechanical strength, and low dielectric constant (3.4-3.6). However, their dielectric properties still need to be further improved to meet the requirements of high-frequency communications. Based on the respective advantages of polyphenylene ether and benzoxazine resin, the preparation of benzoxazine-modified polyphenylene ether resin is a new research method. In 2018, Chen et al. first introduced benzoxazine functional groups into polyphenylene ether resins (Polymers, 2018, 10(4): 411-425). They used low molecular weight (number average molecular weight of 1600) polyphenylene ether derivative SA90, namely phenol-terminated oligo(2,6-dimethylphenylene oxide), as raw materials, and carried out nucleophilic substitution with fluoronitrobenzene, followed by catalytic hydrogenation to prepare amine-terminated SA90 (APPO). APPO was then used as an amine source to prepare telechelic benzoxazine functionalized polyphenylene ether prepolymers or main-chain benzoxazine functionalized polyphenylene ether prepolymers with polyformaldehyde, phenol or bisphenol A. Finally, a thermosetting resin with a glass transition temperature (218-225°C) and relatively low dielectric properties (k is 2.9, 1GHz) was obtained through self-curing and epoxy resin curing. However, its thermal properties still cannot meet the requirements of high-frequency, high-speed, and high-performance communication equipment. In addition, the preparation method is complicated and requires multiple chemical reactions such as nitration, amination, and benzoxazine functionalization. The steps are cumbersome and there are many side reactions, which also makes purification after synthesis a big problem. In particular, the cost of selecting a derivative of polyphenylene ether resin (SA90) as a reaction raw material is high.

[0005] In order to further meet the high requirements for comprehensive performance such as low dielectric constant, low dielectric loss, high heat resistance, self-flame retardancy and flexibility, it is of great significance to design and research polyphenylene ether composite resins with excellent comprehensive performance. Summary of the invention

[0006] The invention aims to provide a polyphenylene ether composite resin with excellent comprehensive performance, preparation and application. The composite resin has low dielectric properties, high heat resistance, flexibility and even self-flame retardant properties.

[0007] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is as follows:

[0008] Provided is a polyphenylene ether composite resin with excellent comprehensive performance, which is a benzoxazine functionalized polyphenylene ether / benzoxazine binary composite resin, a benzoxazine functionalized polyphenylene ether / carbon resin binary composite resin, or a benzoxazine functionalized polyphenylene ether / benzoxazine / carbon resin ternary composite resin obtained by curing a benzoxazine functionalized polyphenylene ether resin prepolymer, benzoxazine or / and a hydrocarbon resin prepolymer;

[0009] The benzoxazine functionalized polyphenylene ether resin prepolymer is one or more of the benzoxazine functionalized polyphenylene ether compounds described in the following structural formula, and the benzoxazine functionalized polyphenylene ether includes monofunctional benzoxazine, difunctional benzoxazine and end-type main chain benzoxazine functionalized polyphenylene ether, and the structural formula is shown in Formula 1:

[0010]

[0011]

[0012] R1-

[0013] -R 2- for

[0014] -R 3- for

[0015] The n value is 15 to 30, and the m value is 1 to 5.

[0016] According to the above scheme, the benzoxazine functionalized polyphenylene ether / benzoxazine binary composite resin comprises: 55 to 95 parts by weight of benzoxazine functionalized polyphenylene ether resin prepolymer; 45 to 5 parts by weight of benzoxazine;

[0017] Benzoxazine functionalized polyphenylene ether / hydrocarbon resin binary composite resin: 55 to 95 parts by weight of benzoxazine functionalized polyphenylene ether resin prepolymer; 45 to 5 parts by weight of hydrocarbon resin prepolymer;

[0018] Benzoxazine functionalized polyphenylene ether / benzoxazine / hydrocarbon resin ternary composite resin: 55-85 parts by weight of benzoxazine functionalized polyphenylene ether resin prepolymer; 15-5 parts by weight of benzoxazine; and 30-10 parts by weight of hydrocarbon resin prepolymer.

[0019] Provided is a method for preparing the composite resin prepolymer of the modified polyphenylene ether:

[0020] Add 55 to 95 parts by weight of benzoxazine functionalized polyphenylene ether resin prepolymer and 45 to 5 parts by weight of benzoxazine into a reaction container, and disperse them in an organic solvent to obtain a composite resin prepolymer with a solid content of 20 to 90 wt%, pre-react for a period of time, and heat and cure the resin prepolymer obtained by the pre-reaction to obtain a benzoxazine functionalized polyphenylene ether / benzoxazine binary composite resin;

[0021] 55 to 95 parts by weight of benzoxazine functionalized polyphenylene ether resin prepolymer and 45 to 5 parts by weight of hydrocarbon resin prepolymer are added into a reaction container and dispersed in an organic solvent to obtain a composite resin prepolymer with a solid content of 20 to 90 wt%. The prepolymer is pre-reacted for a period of time, and the resin prepolymer obtained by the pre-reaction is heated and cured to obtain a benzoxazine functionalized polyphenylene ether / hydrocarbon resin binary composite resin.

[0022] 55-85 parts by weight of benzoxazine functionalized polyphenylene ether resin prepolymer, 15-5 parts by weight of benzoxazine, and 30-10 parts by weight of hydrocarbon resin prepolymer are added into a reaction container and dispersed in an organic solvent to obtain a composite resin prepolymer with a solid content of 20-90wt%, and a pre-reaction is performed for a period of time, and the resin prepolymer obtained by the pre-reaction is heated and cured to obtain a benzoxazine functionalized polyphenylene ether / benzoxazine / hydrocarbon resin ternary composite resin after curing.

[0023] According to the above scheme, the benzoxazine is one of the following or a combination thereof: monofunctional benzoxazine, difunctional benzoxazine, multifunctional benzoxazine, main chain benzoxazine, end-capped main chain benzoxazine, naphthoxazine, and other organic substances containing oxazine rings.

[0024] According to the above scheme, the benzoxazine is an intrinsic flame retardant benzoxazine, specifically one or more combinations of intrinsic flame retardant benzoxazine compounds, and the chemical structure of the intrinsic flame retardant benzoxazine is shown in Formula 2:

[0025]

[0026] According to the above scheme, the hydrocarbon resin prepolymer is one of the following prepolymers or a combination thereof: styrene-maleic anhydride copolymer, polybutadiene resin, hydrogenated diene-butadiene-styrene copolymer, butadiene-styrene resin, styrene-isoprene copolymer, styrene-butadiene copolymer, cyclic olefin copolymer, polyisoprene rubber, styrene-butadiene-divinylbenzene copolymer.

[0027] According to the above scheme, the organic solvent is one of the following or a combination thereof: toluene, ethanol, methanol, xylene, ether, acetone, butanone, cyclohexanone, ethyl acetate, N,N'-dimethylformamide, N,N'-dimethylacetamide, ethylene glycol methyl ether, propylene glycol methyl ether, dioxane, and chloroform.

[0028] According to the above scheme, the pre-reaction is 1 to 12 hours at 60 to 120° C., and the curing condition of the polyphenylene ether composite resin is 2 to 24 hours at 100 to 220° C.

[0029] The preparation method of the above benzoxazine functionalized polyphenylene ether resin prepolymer:

[0030] Adding reactants into a reaction container in a one-step or multi-step manner, wherein the reactants are a phenol source, an amine source and an aldehyde compound, reacting at 70-120° C. for 5-60 hours under a nitrogen atmosphere, and post-treating to obtain a benzoxazine functionalized polyphenylene ether resin prepolymer, wherein the one-step addition method is to add all the raw materials into the reaction container at the same time, and then add a polar / non-polar mixed solvent to dissolve and react; and the multi-step addition method is to first add an aldehyde compound and an amine compound into the reaction container, and then add a polar / non-polar mixed solvent, and then add a phenol source after sufficient stirring;

[0031] in:

[0032] The phenol source in the preparation of the monofunctional benzoxazine functionalized polyphenylene ether resin prepolymer (Formula 1(a)) is a redistributed polyphenylene ether resin, and the amine source is aniline, furfurylamine, allylamine, or p-vinylaniline;

[0033] The phenol source in the preparation of the bifunctional benzoxazine functionalized polyphenylene ether resin prepolymer (Formula 1(b)) is the redistributed polyphenylene ether resin, and the amine source is 4,4'-diaminodiphenylmethane and hexamethylenediamine;

[0034] In the preparation of the end-capped main chain benzoxazine functionalized polyphenylene ether resin prepolymer (Formula 1(c)), the phenol source is dihydric phenol and redistributed polyphenylene ether resin, the dihydric phenol is bisphenol A, bisphenol F, bisphenol S, dicyclopentadiene bisphenol A, 4,4'-dihydroxybiphenyl, 4,4'-dihydroxydiphenyl ether, and the amine source is 4,4'-diaminodiphenylmethane and hexamethylenediamine.

[0035] According to the above scheme, the redistributed polyphenylene ether resin is The value range of n is: 15 to 30.

[0036] According to the above scheme, the number average molecular weight of the redistributed polyphenylene ether resin is 2027-3827.

[0037] According to the above scheme, the aldehyde compound is formaldehyde, paraformaldehyde, etc.

[0038] According to the above scheme, the molar ratio of the phenolic hydroxyl group, amino group and aldehyde group of the reactants is 1::1:2.

[0039] According to the above scheme, in the preparation of the end-capped main chain benzoxazine functionalized polyphenylene ether resin prepolymer, the molar ratio of the dihydric phenol compound to the functional group of the phenolic hydroxyl group in the redistributed polyphenylene ether resin is 1:1.

[0040] According to the above scheme, the polar / non-polar mixed solvent is obtained by mixing a polar solvent and a non-polar solvent in a volume ratio of 1:5 to 5:1. The polar solvent is cyclohexanone, acetone, ethyl acetate, methanol, ether, N,N′-dimethylformamide, dioxane, chloroform, ethanol, tetrahydrofuran, etc., and the non-polar solvent is toluene, butanone, xylene, etc.

[0041] According to the above scheme, the post-treatment is as follows: after the reaction is completed, the reaction solution is poured into a methanol solution to obtain a precipitate, washed multiple times, and then the product is dissolved in a polar / non-polar mixed solvent, precipitated with methanol, and washed multiple times. The above process is repeated multiple times to purify the prepared sample, and finally dried and ground to obtain a light yellow benzoxazine functionalized polyphenylene ether resin prepolymer.

[0042] According to the above scheme, the redistributed polyphenylene ether resin is obtained by redistributing commercial high molecular weight polyphenylene ether.

[0043] According to the above scheme, the preparation method of the redistributed polyphenylene ether resin is as follows: commercial high molecular weight polyphenylene ether, bisphenol A, and peroxide are used as raw materials, dissolved in a polar / non-polar mixed solvent, reacted at 60-125° C. for 4-50 hours, and post-processed to obtain a low molecular weight polyphenylene ether resin after the redistribution reaction, namely, a redistributed polyphenylene ether resin, and the reaction formula is as follows:

[0044]

[0045] According to the above scheme, the peroxide includes benzoic acid peroxide, methyl ethyl ketone peroxide, tert-amyl peroctanoate, dibenzoyl peroxide, benzoyl peroxide, 3,3′,5,5′-tetramethylbiphenylquinone, tri-tert-butylphenoxy free radical, benzoyl peroxide, etc.

[0046] According to the above scheme, the number average molecular weight of the commercial high molecular weight polyphenylene ether resin is 12000-24000, and the n' value is 100-200.

[0047] Preferably, the mass of the peroxide and bisphenol A are 25-30% and 20-25% of the mass of the polyphenylene ether resin, respectively.

[0048] According to the above scheme, the polar / non-polar mixed solvent is obtained by mixing a polar solvent and a non-polar solvent in a volume ratio of 1:5 to 5:1, the polar solvent is cyclohexanone, acetone, ethyl acetate, methanol, ether, N,N′-dimethylformamide, dioxane, chloroform, ethanol, tetrahydrofuran, etc., and the non-polar solvent is toluene, butanone, xylene, etc.

[0049] According to the above scheme, the post-treatment process after the redistribution reaction is to pour the reaction solution into distilled water for precipitation, then dissolve the product in a polar / non-polar mixed solvent, and then precipitate with distilled water, and repeat the precipitation and dissolution process many times until the pH value of the solution is neutral.

[0050] The polyphenylene ether composite resin with excellent comprehensive performance is used for preparing resin varnish or prepreg or laminate or multilayer printed circuit board. The resin varnish is composed of the polyphenylene ether composite resin prepolymer according to claim 1 and an organic solvent; the prepreg is prepared by adding inorganic filler and / or flame retardant to the resin varnish; the laminate is formed by uniformly coating the prepreg on non-woven fabric; and the multilayer printed circuit board is made of the laminate.

[0051] A multilayer printed wiring board is provided, comprising a copper foil and a laminate made of a prepreg containing a polyphenylene ether composite resin supported on the copper foil.

[0052] The benzoxazine functionalized polyphenylene ether resin prepolymer used in the present invention can be based on the redistributed polyphenylene ether resin, and only one-step chemical reaction is required to prepare the benzoxazine functionalized polyphenylene ether resin prepolymer, which is low in cost and simple in preparation method. In addition, by selecting amine compounds and phenolic compounds with different chemical structures, monofunctional benzoxazines, difunctional benzoxazines and end-type main chain benzoxazine functionalized polyphenylene ether resin prepolymers with different chemical structures can be synthesized according to application needs. The benzoxazine functionalized polyphenylene ether resin prepolymer prepared based on the low molecular weight redistributed polyphenylene ether has a low molecular weight and good processability. The thermosetting resin obtained by curing the benzoxazine functionalized polyphenylene ether resin prepolymer has excellent solvent resistance, thermal properties (glass transition temperature: 238-269° C.) and high-frequency dielectric properties (k value: 2.0-2.8).

[0053] Based on the benzoxazine functionalized polyphenylene ether resin prepolymer, the present invention further combines benzoxazine and / or hydrocarbon resin prepolymer to construct a binary or ternary copolymer resin system with excellent comprehensive performance.

[0054] In the binary composite system constructed by benzoxazine functionalized polyphenylene ether and benzoxazine, copolymerization based on the shared oxazine ring can improve the compatibility and crosslinking density of the composite resin system. This is because the compatibility of the two resins is improved through the ring-opening polymerization of the oxazine ring. Moreover, due to the copolymerization of the two oxazine rings and the entanglement and interlacing of the long polyphenylene ether chains in the crosslinked network structure of the benzoxazine resin, the crosslinking density of the benzoxazine resin is increased. It is worth noting that the introduction of intrinsic flame-retardant benzoxazine resin can make the composite resin system self-flame-retardant without the addition of external flame retardants.

[0055] In the binary composite system constructed by benzoxazine functionalized polyphenylene ether and hydrocarbon resin, the hydrocarbon resin has a regular structure and contains a long carbon chain chemical structure with low polarity. The introduction of hydrocarbon resin into the polyphenylene ether composite resin can improve the dielectric properties of the entire composite resin system. Moreover, the hydrocarbon resin can complete self-polymerization during the polymerization and curing process of the benzoxazine resin, and form an interpenetrating cross-linked network (IPN) structure with the benzoxazine resin, thereby effectively improving the cross-linking density and high temperature resistance of the composite resin. In addition, the double bonds of the benzoxazine functionalized polyphenylene ether can form a chemical copolymerization reaction with the double bond structure contained in the hydrocarbon resin, which also effectively improves the compatibility of the two and the cross-linking density of the copolymer, so that the thermal properties are improved. In addition, the carbonyl functional group contained in the hydrocarbon resin can react with the phenolic hydroxyl group formed by the ring opening of benzoxazine to form an aromatic ester, forming a chemical cross-linking structure, further improving the cross-linking density of the copolymer resin, which also greatly improves the thermal properties of the composite resin. At the same time, the reduction of polar phenolic hydroxyl functional groups formed by the ring-opening curing of benzoxazine functionalized polyphenylene ether is also conducive to the improvement of the dielectric properties of the composite resin. In addition, since the hydrocarbon resin has a long carbon chain structure, it can give the composite resin flexibility, which significantly improves the flexibility of the benzoxazine functionalized polyphenylene ether resin / hydrocarbon resin binary composite resin.

[0056] In particular, each resin in the benzoxazine functionalized polyphenylene ether / benzoxazine / hydrocarbon resin ternary composite resin has its own properties, and they interact and influence each other. In addition to the above-mentioned reactions of the benzoxazine functionalized polyphenylene ether with the benzoxazine resin and the hydrocarbon resin, the small molecule benzoxazine is equivalent to a diluent in the processing of the binary and ternary composite resins, which can effectively reduce the viscosity of the composite resin system and improve the process performance of the binary and ternary composite resin systems. The hydrocarbon resin is a catalyst for the benzoxazine ring-opening reaction, which can effectively reduce the curing temperature of the composite resin system, improve the processing performance, and increase the cross-linking density of the composite resin, thereby further improving the thermal and dielectric properties. And the hydrocarbon resin has a long carbon chain structure, which can give the composite resin flexibility, so that the flexibility of the benzoxazine functionalized polyphenylene ether / benzoxazine / hydrocarbon resin ternary composite resin body is significantly improved. In addition, the introduction of intrinsic flame-retardant benzoxazine resin can also make the ternary composite resin system self-flame-retardant without the need for an external flame retardant.

[0057] Moreover, considering that benzoxazine functionalized polyphenylene ether resin has low dielectric constant and dielectric loss under UHF conditions, and the copolymerization reaction with benzoxazine resin and hydrocarbon resin can effectively increase the crosslinking density to suppress polarization orientation, binary and ternary composite resins have lower dielectric constant (1.8-2.5) and dielectric loss (0.0007-0.005) under UHF conditions, so that it has application prospects in emerging fields such as UHF communication. It can be used in laminates, copper clad boards, multilayer printed circuit boards, semiconductor packaging materials and other composite materials.

[0058] The beneficial effects of the present invention are:

[0059] The invention has simple preparation process, low cost and is easy to industrialize.

[0060] The polyphenylene ether composite resin provided by the present invention has excellent heat resistance (glass transition temperature 253-394°C) and toughness (tensile strength 96-127MPa); excellent dielectric properties under ultra-high frequency conditions (dielectric constant at 10GHz is between 1.8 and 2.5, and dielectric loss is between 0.0007 and 0.005). It can be widely used in laminates, copper-clad boards, multi-layer printed circuit boards, semiconductor packaging materials and other composite materials, and is particularly suitable for emerging communication fields such as ultra-high frequency communications.

[0061] The binary and ternary resins containing intrinsically flame-retardant benzoxazine can achieve flame-retardant effect of the composite resin without adding external flame retardant. BRIEF DESCRIPTION OF THE DRAWINGS

[0062] Figure 1Infrared spectra (FTIR) of the resin prepolymer products synthesized in Examples 1-3 in the preparation of the redistributed low molecular weight polyphenylene ether resin and benzoxazine functionalized polyphenylene ether resin prepolymer.

[0063] in:

[0064] Figure 1 a redistributed low molecular weight polyphenylene ether resin;

[0065] Figure 1 b Example 1, aniline / bisphenol A type benzoxazine functionalized polyphenylene ether resin prepolymer;

[0066] Figure 1 c Example 2, furfurylamine / bisphenol A type benzoxazine functionalized polyphenylene ether resin prepolymer;

[0067] Figure 1 d Example 3, 4,4′-diaminodiphenylmethane / bisphenol A type benzoxazine functionalized polyphenylene ether resin prepolymer. DETAILED DESCRIPTION

[0068] The following is a detailed description of the embodiments of the present invention.

[0069] Example 1

[0070] Take 95 parts of aniline / bisphenol A type benzoxazine functionalized polyphenylene ether resin prepolymer (chemical structure shown below), 5 parts of styrene-butadiene-divinylbenzene copolymer prepolymer, adjust the solid content of the resin composition to 90wt% with butanone solvent, stir for 1 hour at 60°C, and mix evenly. Then the obtained prepolymer is cured at 220°C for 2h to obtain a binary composite resin. Its glass transition temperature (dynamic thermomechanical analyzer) is 253°C, the tensile strength (universal mechanical testing machine) is 96MPa, the dielectric constant (network vector analyzer) at 10GHz is 2.5, and the dielectric loss (network vector analyzer) is 0.005.

[0071]

[0072] Example 2

[0073] Take 55 parts of the prepolymer of furfurylamine / bisphenol A type benzoxazine functionalized polyphenylene ether (chemical structure is shown below).

[0074]

[0075] Then take 45 parts of aniline / bisphenol A type benzoxazine, and the chemical reaction formula is shown below.

[0076]

[0077] The above resin raw materials are adjusted to a solid content of 20wt% by using a toluene / ethanol (2:1v / v) mixed solvent, and stirred at 80°C for 12 hours to mix evenly. The obtained prepolymer is then cured at 100°C for 24 hours to obtain a binary composite resin. Its glass transition temperature (dynamic thermomechanical analyzer) is 297°C, the tensile strength (universal mechanical testing machine) is 101MPa, the dielectric constant (network vector analyzer) at 10GHz is 2.4, and the dielectric loss (network vector analyzer) is 0.004.

[0078] Example 3

[0079] Take 30 parts of the prepolymer of aniline / bisphenol A type benzoxazine functionalized polyphenylene ether (chemical structure is shown below).

[0080]

[0081] Then, 30 parts of a prepolymer of 4,4′-diaminodiphenylmethane / bisphenol A type benzoxazine functionalized polyphenylene ether (chemical structure shown below) were taken.

[0082]

[0083] Finally, 40 parts of styrene-maleic anhydride copolymer prepolymer were taken. The above resin raw materials were adjusted to a solid content of 80wt% by using N,N′-dimethylformamide solvent, stirred at 120°C for 3 hours, and mixed evenly. Then the obtained prepolymer was cured at 200°C for 4 hours to obtain a binary composite resin. Its glass transition temperature (dynamic thermomechanical analyzer) is 299°C, the tensile strength (universal mechanical testing machine) is 105MPa, the dielectric constant (network vector analyzer) at 10GHz is 2.3, and the dielectric loss (network vector analyzer) is 0.004.

[0084] Example 4

[0085] Take 35 parts of the prepolymer of furfurylamine / bisphenol A type benzoxazine functionalized polyphenylene ether (chemical structure shown below).

[0086]

[0087] Take 30 parts of a terminal-type main-chain benzoxazine-functionalized polyphenylene ether resin prepolymer (chemical structure shown below).

[0088]

[0089] Where: R2 is R3 is

[0090] Then take 35 parts of furfurylamine / bisphenol A type benzoxazine, and the chemical reaction formula is shown below.

[0091]

[0092] The above resin raw materials are adjusted to a solid content of 50wt% by using a toluene / ethanol (2:1v / v) mixed solvent, and stirred at 80°C for 2 hours to mix evenly. The obtained prepolymer is then cured at 180°C for 10h to obtain a binary composite resin. Its glass transition temperature (dynamic thermomechanical analyzer) is 334°C, the tensile strength (universal mechanical testing machine) is 126MPa, the dielectric constant (network vector analyzer) at 10GHz is 2.2, and the dielectric loss (network vector analyzer) is 0.003.

[0093] Example 5

[0094] Take 10 parts of furfurylamine / bisphenol A type benzoxazine, and the chemical reaction formula is shown below.

[0095]

[0096] and 5 parts of end-capped main chain benzoxazine, and the chemical reaction formula is shown below.

[0097]

[0098] Where: R1 is

[0099] Then, 15 parts of furfurylamine / bisphenol A type benzoxazine functionalized polyphenylene ether resin prepolymer (chemical structure is shown below) were taken.

[0100]

[0101] Take 50 parts of a terminal-type main-chain benzoxazine-functionalized polyphenylene ether resin prepolymer (chemical structure shown below).

[0102]

[0103] Where: R2 is R3 is

[0104] Finally, 20 parts of styrene-maleic anhydride copolymer prepolymer were taken.

[0105] The above resin raw materials are adjusted to a solid content of 45wt% by using dioxane solvent, and stirred at 80°C for 4 hours to mix evenly. The obtained prepolymer is then cured at 160°C for 20 hours to obtain a ternary composite resin. Its glass transition temperature (dynamic thermomechanical analyzer) is 345°C, its tensile strength (universal mechanical testing machine) is 127MPa, its dielectric constant (network vector analyzer) is 2.0 at 10GHz, and its dielectric loss (network vector analyzer) is 0.002.

[0106] Example 6

[0107] Take 5 parts of furfurylamine / bisphenol A type benzoxazine, and the chemical reaction formula is shown below.

[0108]

[0109] and 10 parts of end-capped main chain benzoxazine, and the chemical reaction formula is shown below.

[0110]

[0111] Where: R1 is

[0112] Then, 65 parts of a terminal-type main-chain benzoxazine functionalized polyphenylene ether resin prepolymer (chemical structure shown below) were taken.

[0113]

[0114] Where: R2 is R3 is

[0115] Finally, 10 parts of styrene-maleic anhydride copolymer prepolymer and 10 parts of styrene-butadiene copolymer prepolymer were taken. The above resin raw materials were adjusted to a solid content of 40wt% by using a toluene / ethanol (2:1v / v) mixed solvent, stirred at 70°C for 12 hours, and mixed evenly. The obtained prepolymer was then cured at 190°C for 6h to obtain a ternary composite resin. Its glass transition temperature (dynamic thermomechanical analyzer) is 394°C, the tensile strength (universal mechanical testing machine) is 121MPa, the dielectric constant (network vector analyzer) at 10GHz is 1.8, and the dielectric loss (network vector analyzer) is 0.0007.

[0116] 100 parts of the polyphenylene ether resin composition prepared in Example 6 above (solid content of 40wt%, solvent is toluene / ethanol (2:1v / v) mixed solvent). 70 parts of nano-magnesium hydroxide (solid content of 70wt%, solvent is toluene / ethanol (2:1v / v) mixed solvent), which is used as both a reinforcing material and a flame retardant. The two are mixed and ultrasonically treated for 120min at an ultrasonic power of 500W to obtain a uniformly dispersed inorganic / organic nano-composite resin solution. The inorganic / organic composite resin solution is evenly coated on a non-woven fabric (thickness 0.05mm), dried at room temperature, and transferred to a blast oven at 110°C for precuring to obtain a semi-cured sheet. Cut the semi-cured sheet of regular shape, stack ten layers, give copper foil on one side, place it in a hot press at a temperature of 170°C and a pressure of 10.0MPa for 2 hours, and degas once every ten minutes. The inorganic / organic polyphenylene ether nano-composite resin is easy to process and not easy to flow. Finally, the obtained plate is processed by hole opening, metal plating, etching and other processing methods to obtain a copper clad laminate.

[0117] The test results of the physical properties of the prepared copper clad laminate are as follows. The peel strength test result of the copper foil is 1.2N / mm, indicating that the polyphenylene ether composite resin has good bonding properties. The copper clad laminate after copper etching is cut into small pieces of a certain size and placed in a pressure cooker. After being boiled under the conditions of 105kPa, 121℃, and 360min, the soldering heat resistance test (PCT, tin bath 288℃) shows that there is no blistering or stratification for more than 5min, and the copper clad laminate exhibits good water boiling resistance. The thermal expansion coefficient (CTE) of the thermomechanical analysis test is 34ppm / ℃, indicating that the copper clad laminate has good dimensional stability. The glass transition temperature of the copper clad laminate tested by dynamic thermomechanical analysis is 376℃, and the residual carbon rate at 800℃ (thermogravimetric analyzer) is 65%, showing excellent thermal properties. When the test frequency is 10GHz, the dielectric constant and dielectric loss are 2.37 and 0.0031, respectively. The results show that the copper clad laminate has excellent ultra-high frequency dielectric properties. The flame retardancy of the copper clad laminate obtained by the UL-94 vertical test method is still V-0.

[0118] Example 7

[0119] Take 95 parts of the prepolymer of furfurylamine / bisphenol A type benzoxazine functionalized polyphenylene ether (chemical structure shown below).

[0120]

[0121] Take 5 parts of intrinsic flame retardant benzoxazine, the chemical structure of which is shown below.

[0122]

[0123] The above resin raw materials are adjusted to a solid content of 20wt% in a mixed solvent of ethanol / toluene (3:1v / v), and stirred at 60°C for 4 hours to mix evenly. The obtained prepolymer is then cured at 100°C for 24 hours to obtain a binary composite resin. Its glass transition temperature (dynamic thermomechanical analyzer) is 296°C, the tensile strength (universal mechanical testing machine) is 99MPa, the dielectric constant (network vector analyzer) at 10GHz is 2.4, and the dielectric loss (network vector analyzer) is 0.004. The residual carbon rate at 800°C (thermogravimetric analyzer) can reach 50%, the limiting oxygen index (GB 2406-80) is as low as 43.5, and the heat release capacity (micro combustion calorimeter) reaches 100J g -1 K -1 , flame retardant performance V-0 grade (UL-94).

[0124] Example 8

[0125] Take 30 parts of the prepolymer of furfurylamine / bisphenol A type benzoxazine functionalized polyphenylene ether (chemical structure is shown below).

[0126]

[0127] Take 25 parts of a terminal-type main-chain benzoxazine-functionalized polyphenylene ether resin prepolymer (chemical structure shown below).

[0128]

[0129] Where: R2 is R3 is

[0130] Then take 45 parts of intrinsic flame retardant benzoxazine, the chemical structure of which is shown below.

[0131]

[0132] The above resin raw materials are adjusted to a solid content of 50wt% by using butanone solvent, and stirred at 85°C for 2 hours to mix evenly. The obtained prepolymer is then cured at 180°C for 12 hours to obtain a binary composite resin. Its glass transition temperature (dynamic thermomechanical analyzer) is 334°C, the tensile strength (universal mechanical testing machine) is 106MPa, the dielectric constant (network vector analyzer) at 10GHz is 2.2, and the dielectric loss (network vector analyzer) is 0.003. The residual carbon rate at 800°C (thermogravimetric analyzer) can reach 55%, the limiting oxygen index (GB 2406-80) can reach 32.6, and the heat release capacity (micro combustion calorimeter) can reach 57J g - 1 K -1 , flame retardant performance V-0 grade (UL-94).

[0133] Example 9

[0134] Take 5 parts of furfurylamine / bisphenol A type benzoxazine functionalized polyphenylene ether prepolymer (chemical structure shown below).

[0135]

[0136] Take 50 parts of a terminal-type main-chain benzoxazine-functionalized polyphenylene ether resin prepolymer (chemical structure shown below).

[0137]

[0138] Where: R2 is R3 is

[0139] Then take 10 parts of intrinsic flame retardant benzoxazine, the chemical structure of which is shown below.

[0140]

[0141] and 5 parts of intrinsic flame retardant benzoxazine, the chemical structure of which is shown below.

[0142]

[0143] Finally, 30 parts of styrene-maleic anhydride copolymer prepolymer were taken. The solid content of the resin composition of the above resin raw materials was adjusted to 45wt% with dioxane solvent, and stirred at 80°C for 4 hours to mix evenly. The obtained prepolymer was then cured at 160°C for 8h to obtain a ternary composite resin. Its glass transition temperature (dynamic thermomechanical analyzer) is 375°C, the tensile strength (universal mechanical testing machine) is 127MPa, the dielectric constant at 10GHz (network vector analyzer) is 2.1, and the dielectric loss (network vector analyzer) is 0.002. The residual carbon rate at 800°C (thermogravimetric analyzer) can reach 57%, the limiting oxygen index (GB 2406-80) can reach 35.2, and the heat release capacity (micro combustion calorimeter) can reach 69J g -1 K -1 , flame retardant performance V-0 grade (UL-94).

[0144] Example 10

[0145] Take 5 parts of a prepolymer of 4,4′-diaminodiphenylmethane / bisphenol A type benzoxazine functionalized polyphenylene ether resin (chemical structure shown below).

[0146]

[0147] Take 50 parts of a terminal-type main-chain benzoxazine-functionalized polyphenylene ether resin prepolymer (chemical structure shown below).

[0148]

[0149] Where: R2 is R3 is

[0150] Then take 9 parts of intrinsic flame retardant benzoxazine, the chemical structure of which is shown below.

[0151]

[0152] And 6 parts of another intrinsic flame retardant benzoxazine, the chemical structure of which is shown below.

[0153]

[0154] Finally, 10 parts of styrene-maleic anhydride copolymer prepolymer and 20 parts of styrene-butadiene copolymer prepolymer were taken. The solid content of the resin composition of the above resin raw materials was adjusted to 45wt% with ethanol / toluene (3:1v / v) mixed solvent, and stirred at 60°C for 1 hour to mix evenly. Then the obtained prepolymer was cured at 190°C for 6h to obtain a ternary composite resin. Its glass transition temperature (dynamic thermomechanical analyzer) is 379°C, the tensile strength (universal mechanical testing machine) is 125MPa, the dielectric constant at 10GHz (network vector analyzer) is 2.0, and the dielectric loss (network vector analyzer) is 0.001. The residual carbon rate at 800°C (thermogravimetric analyzer) can reach 60%, the limiting oxygen index (GB 2406-80) can reach 35, and the heat release capacity (micro combustion calorimeter) can reach 30.3J g -1 K -1 , flame retardant performance V-0 grade (UL-94).

[0155] Embodiment 11

[0156] 100 parts of the polyphenylene ether resin composition prepared in Example 10 (solid content of 45wt%, solvent is ethanol / toluene (3:1v / v) mixed solvent) and 80 parts of nano-silicon dioxide (solid content of 70wt%, solvent is ethanol / toluene (3:1v / v) mixed solvent) were mixed and ultrasonically treated for 60min at an ultrasonic power of 500W to obtain a uniformly dispersed nano-composite resin solution. The inorganic / organic composite resin solution was evenly coated on a non-woven fabric (thickness 0.05mm), dried at room temperature, and transferred to a blast oven at 100-120°C for precuring to obtain a semi-cured sheet. The semi-cured sheet of regular shape was cut, stacked in six layers, copper foil was given to one side, and placed in a hot press at a temperature of 160°C and a pressure of 10.0MPa for 1 hour, and degassed every ten minutes. The composite resin has good processability and is easy to process without glue flow. Finally, the obtained sheet is processed by hole opening, metal plating, etching and other processing methods to obtain a copper-clad laminate.

[0157] The test results of the physical properties of the prepared copper clad laminate are as follows. The peel strength test result of the copper foil is 1.4N / mm, indicating that the polyphenylene ether composite resin has good bonding properties. The copper clad laminate after copper etching is cut into small pieces of a certain size and placed in a pressure cooker. After being boiled under the conditions of 105kPa, 121℃, and 360min, the soldering heat resistance test (PCT, tin bath 288℃) shows that there is no blistering or stratification for more than 5min, and the copper clad laminate exhibits good water boiling resistance. The thermal expansion coefficient (CTE) of the thermomechanical analysis test is 40ppm / ℃, indicating that the copper clad laminate has good dimensional stability. The glass transition temperature of the copper clad laminate tested by dynamic thermomechanical analysis is 365℃, and the residual carbon rate at 800℃ (thermogravimetric analyzer) is 55%, showing excellent thermal properties. When the test frequency is 10GHz, the dielectric constant and dielectric loss are 2.35 and 0.0027, respectively. The results show that the copper clad laminate has excellent ultra-high frequency dielectric properties. It is worth noting that the flame retardancy of the copper clad laminate obtained by the UL-94 vertical test method is still V-0.

[0158] Preparation of benzoxazine functionalized polyphenylene ether:

[0159] Redistributed low molecular weight polyphenylene ether resin

[0160] 100 g of commercial high molecular weight polyphenylene ether resin (number average molecular weight of 12000 g / mol), 20 g of bisphenol A and 30 g of benzoic acid peroxide were mixed in a toluene / ethanol (5:1 v / v) solvent and reacted at 60°C for 50 h. After the reaction, the mixture was precipitated and washed with distilled water several times to obtain a low molecular weight polyphenylene ether resin (number average molecular weight of 2027 g / mol).

[0161] Example 1

[0162] 100 g of commercial high molecular weight polyphenylene ether resin (number average molecular weight of 12000 g / mol), 25 g of bisphenol A and 25 g of benzoic acid peroxide were mixed in a toluene / ethanol (5:1 v / v) solvent and reacted at 60°C for 50 h. After the reaction, the mixture was precipitated and washed with distilled water several times to obtain a low molecular weight polyphenylene ether resin (number average molecular weight of 2027 g / mol).

[0163] According to the molar ratio of phenolic hydroxyl, amino and aldehyde functional groups of 1:1:2, 0.025mol of the prepared low molecular weight polyphenylene ether resin, 0.025mol of aniline and 0.05mol of paraformaldehyde were added to a four-necked flask equipped with a condenser, magnetic stirring, thermometer and temperature sensor, and 70mL of toluene / ethanol (1:5v / v) mixed solvent was added, and the mixture was slowly heated to 70℃ for 60h. After the reaction, the reaction solution was poured into 200mL of methanol solution (concentration 99wt%) and allowed to stand for 24h to obtain a precipitate, which was washed several times. The precipitation and washing process was repeated several times. Finally, the obtained precipitate was vacuum dried at 60℃ for 12h, and the light yellow powder obtained by grinding the dried product was the prepolymer of aniline / bisphenol A type benzoxazine functionalized polyphenylene ether resin (chemical structure is shown below).

[0164]

[0165] Example 2

[0166] 100 g of commercial high molecular weight polyphenylene ether resin (number average molecular weight of 24000 g / mol), 25 g of bisphenol A and 30 g of benzoic acid peroxide were mixed in a butanone / N,N′-dimethylformamide (1:5 v / v) solvent and reacted at 125°C for 4 h. After the reaction, the mixture was precipitated and washed with distilled water several times to obtain a low molecular weight polyphenylene ether resin (number average molecular weight of 3827 g / mol).

[0167] According to the molar ratio of phenolic hydroxyl, amino and aldehyde functional groups of 1:1:2, 0.025mol of the prepared low molecular weight polyphenylene ether resin, 0.025mol of furfurylamine and 0.05mol of paraformaldehyde were added to a four-necked flask equipped with a condenser, magnetic stirring, thermometer and temperature sensor, and 70mL of toluene / N,N′-dimethylformamide (5:1v / v) mixed solvent was added, and the mixture was slowly heated to 105°C for 5h. After the reaction, the reaction solution was poured into 200mL of methanol solution (concentration 95wt%) and allowed to stand for 24h to obtain a precipitate, which was washed several times. The precipitation and washing process was repeated several times. Finally, the obtained precipitate was vacuum dried at 60°C for 12h, and the light yellow powder obtained by grinding the dried product was the furfurylamine / bisphenol A type benzoxazine functionalized polyphenylene ether prepolymer (chemical structure shown below).

[0168]

[0169] Example 3

[0170] 100 g of commercial high molecular weight polyphenylene ether resin (number average molecular weight of 20000 g / mol), 20 g of bisphenol A and 25 g of 3,3′,5,5′-tetramethylbiphenyl diquinone were mixed in a butanone / dioxane (1:3 v / v) solvent and reacted at 100°C for 24 h. After the reaction, it was precipitated and washed with distilled water several times to obtain a low molecular weight polyphenylene ether resin (number average molecular weight of 2645 g / mol).

[0171] According to the molar ratio of phenolic hydroxyl, amino and aldehyde functional groups of 1:1:2, 0.025mol of the prepared low molecular weight polyphenylene ether resin, 0.0125mol of 4,4′-diaminodiphenylmethane and 0.05mol of polyformaldehyde were added to a four-necked flask equipped with a condenser, magnetic stirring, thermometer and temperature sensor, and 70mL of toluene / N,N′-dimethylformamide (1:1v / v) mixed solvent was added, and the mixture was slowly heated to 120°C for 25h. After the reaction, the reaction solution was poured into 200mL of methanol solution (concentration 90wt%) and allowed to stand for 24h to obtain a precipitate, which was washed several times. The precipitation and washing process was repeated several times. Finally, the obtained precipitate was vacuum dried at 60°C for 12h, and the light yellow powder obtained by grinding the dried product was 4,4′-diaminodiphenylmethane / bisphenol A type benzoxazine functionalized polyphenylene ether prepolymer (chemical structure shown below).

[0172] Example 4

[0173] 100 g of commercial high molecular weight polyphenylene ether resin (number average molecular weight of 12000 g / mol), 20 g of bisphenol A and 30 g of benzoic acid peroxide were mixed in a toluene / ethanol (5:1 v / v) solvent and reacted at 60°C for 50 h. After the reaction, the mixture was precipitated and washed with distilled water several times to obtain a low molecular weight polyphenylene ether resin (number average molecular weight of 2027 g / mol).

[0174] According to the molar ratio of phenolic hydroxyl, amino and aldehyde functional groups being 1:1:2, and the molar ratio of phenolic hydroxyl functional groups in bisphenol A and redistributed polyphenylene ether resin being 1:1, 0.05 mol of the prepared low molecular weight polyphenylene ether resin, 0.025 mol of bisphenol A, 0.05 mol of 1,6-hexanediamine and 0.2 mol of paraformaldehyde were added into a 250 mL three-necked flask equipped with a condenser, a magnetic stirring device and a thermometer, and then 51 mL of a toluene / ethanol mixed solvent (1:2 v / v) was added. After mixing evenly, the mixture was heated to 90°C and reacted for 48 hours. After the reaction was completed, the reaction solution was poured into 100 mL of a methanol solution (concentration 40 wt%) to obtain a suspension, which was allowed to stand for 24 hours. The supernatant was removed to obtain a precipitate, and the precipitate was vacuum dried at 50°C for 8 hours. Finally, the dried product was ground to obtain a powder, which was a capped main chain benzoxazine functionalized polyphenylene ether resin prepolymer (chemical structure shown below).

[0175]

[0176] Where: R2 is R3 is

[0177] The molecular structural formulas of 1,6-hexanediamine, bisphenol A, and redistributed polyphenylene ether resin used in this embodiment are:

[0178]

[0179] The products synthesized in the comparative example and the example were characterized by infrared spectroscopy (FTIR). The infrared spectroscopy characterization results showed that the present invention successfully synthesized three prepolymers of benzoxazine functionalized polyphenylene ether resin based on the redistributed polyphenylene ether resin.

[0180] Wherein: The products synthesized in the comparative examples and embodiments are shown in Figure 1 .

[0181] in:

[0182] Figure 1 a: redistributed low molecular weight polyphenylene ether resin prepared in comparative example;

[0183] Figure 1 b: aniline / bisphenol A type benzoxazine functionalized polyphenylene ether resin prepolymer synthesized in Example 1;

[0184] Figure 1 c: the furfurylamine / bisphenol A type benzoxazine functionalized polyphenylene ether resin prepolymer of Example 2;

[0185] Figure 1 d: 4,4′-diaminodiphenylmethane / bisphenol A type benzoxazine functionalized polyphenylene ether prepolymer of Example 3).

[0186] like Figure 1 As shown in a, 3460cm-1 is the characteristic absorption peak of the stretching vibration of the hydroxyl group, 1306, 1189, 1020cm-1 are the characteristic absorption peaks of the vibration of phenyl ether, and 857cm-1 is the characteristic absorption peak of the CH bending vibration on the benzene ring. The infrared spectrum of the low molecular weight polyphenylene ether resin is basically consistent with the infrared spectrum of the high molecular weight polyphenylene ether resin, which shows that the redistribution reaction only changes the length of the molecular chain and does not change the chemical structure of the polyphenylene ether. It is worth noting that the prepolymers of the polyphenylene ether resins synthesized in the embodiments of the present invention all contain benzoxazine functional groups, and the characteristic absorption peaks of the oxazine rings are all located at 935cm -1 The COC of the benzoxazine structure (1229 cm -1 ) and CNC(1180cm -1 ) has a characteristic absorption peak of asymmetric stretching vibration at 1498 cm -1 The position corresponds to the characteristic absorption peak of CC stretching vibration in the plane of trisubstituted benzene ring. For the prepolymer of furfurylamine / bisphenol A type benzoxazine functionalized polyphenylene ether resin ( Figure 1 c) It is also possible to observe the -1 The above infrared spectrum results show that the prepolymer of benzoxazine functionalized polyphenylene ether resin is successfully synthesized based on the redistributed polyphenylene ether resin in the present invention.

[0187] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A polyphenylene ether composite resin with excellent comprehensive performance, which is a benzoxazine functionalized polyphenylene ether / benzoxazine binary composite resin, or a benzoxazine functionalized polyphenylene ether / carbon resin binary composite resin, or a benzoxazine functionalized polyphenylene ether / benzoxazine / carbon resin ternary composite resin obtained by curing a benzoxazine functionalized polyphenylene ether resin prepolymer, benzoxazine or / and a hydrocarbon resin prepolymer; in the benzoxazine functionalized polyphenylene ether / benzoxazine binary composite resin, the benzoxazine functionalized polyphenylene ether resin prepolymer is 55 to 95 parts by weight; and the benzoxazine is 45 to 5 parts by weight; In the benzoxazine functionalized polyphenylene ether / hydrocarbon resin binary composite resin, benzoxazine functionalized polyphenylene ether resin prepolymer is 55 to 95 parts by weight; hydrocarbon resin prepolymer is 45 to 5 parts by weight; In the benzoxazine functionalized polyphenylene ether / benzoxazine / hydrocarbon resin ternary composite resin, benzoxazine functionalized polyphenylene ether resin prepolymer 55-85 weight parts; benzoxazine 15-5 weight parts; hydrocarbon resin prepolymer 30-10 weight parts, The benzoxazine functionalized polyphenylene ether resin prepolymer is one or more of the benzoxazine functionalized polyphenylene ether compounds described in the following structural formula, and the benzoxazine functionalized polyphenylene ether includes monofunctional benzoxazine, difunctional benzoxazine and end-type main chain benzoxazine functionalized polyphenylene ether, and the structural formula is shown in Formula 1: R1- -R 2- for -R 3- for The n value is 15 to 30, and the m value is 1 to 5.

2. The polyphenylene ether composite resin with excellent comprehensive performance according to claim 1, characterized in that: The benzoxazine is one of the following or a combination thereof: monofunctional benzoxazine, difunctional benzoxazine, multifunctional benzoxazine, main chain benzoxazine, end-capped main chain benzoxazine, and naphthoxazine.

3. The polyphenylene ether composite resin with excellent comprehensive performance according to claim 1, characterized in that: The benzoxazine is an intrinsic flame retardant benzoxazine.

4. The polyphenylene ether composite resin with excellent comprehensive performance according to claim 3, characterized in that: The benzoxazine is one or more intrinsic flame retardant benzoxazine compounds, and the chemical structure of the intrinsic flame retardant benzoxazine is shown in Formula 2:

5. The polyphenylene ether composite resin with excellent comprehensive performance according to claim 1, characterized in that: The hydrocarbon resin prepolymer is one of the following prepolymers or a combination thereof: styrene-maleic anhydride copolymer, polybutadiene resin, hydrogenated diene-butadiene-styrene copolymer, styrene-butadiene resin, styrene-isoprene copolymer, styrene-butadiene copolymer, cyclic olefin copolymer, polyisoprene rubber, styrene-butadiene-divinylbenzene copolymer.

6. The method for preparing the polyphenylene ether composite resin with excellent comprehensive performance according to claim 1, characterized in that: Add 55 to 95 parts by weight of benzoxazine functionalized polyphenylene ether resin prepolymer and 45 to 5 parts by weight of benzoxazine into a reaction container, and disperse them in an organic solvent to obtain a composite resin prepolymer with a solid content of 20 to 90 wt%, pre-react for a period of time, and heat and cure the resin prepolymer obtained by the pre-reaction to obtain a benzoxazine functionalized polyphenylene ether / benzoxazine binary composite resin; Add 55 to 95 parts by weight of benzoxazine functionalized polyphenylene ether resin prepolymer and 45 to 5 parts by weight of hydrocarbon resin prepolymer into a reaction container, and disperse them in an organic solvent to obtain a composite resin prepolymer with a solid content of 20 to 90 wt%, pre-react for a period of time, and heat and cure the resin prepolymer obtained by the pre-reaction to obtain a benzoxazine functionalized polyphenylene ether / hydrocarbon resin binary composite resin; 55-85 parts by weight of benzoxazine functionalized polyphenylene ether resin prepolymer, 15-5 parts by weight of benzoxazine, and 30-10 parts by weight of hydrocarbon resin prepolymer are added into a reaction container and dispersed in an organic solvent to obtain a composite resin prepolymer with a solid content of 20-90wt%, and a pre-reaction is performed for a period of time, and the resin prepolymer obtained by the pre-reaction is heated and cured to obtain a benzoxazine functionalized polyphenylene ether / benzoxazine / hydrocarbon resin ternary composite resin after curing.

7. The preparation method according to claim 6, characterized in that: The organic solvent is one of the following or a combination thereof: toluene, ethanol, methanol, xylene, ether, acetone, butanone, cyclohexanone, ethyl acetate, N,N'-dimethylformamide, N,N'-dimethylacetamide, ethylene glycol methyl ether, propylene glycol methyl ether, dioxane, and chloroform.

8. The preparation method according to claim 6, characterized in that: The pre-reaction is carried out at 60-120° C. for 1-12 hours, and the curing condition of the polyphenylene ether composite resin is carried out at 100-220° C. for 2-24 hours.

9. The preparation method according to claim 6, characterized in that: The preparation method of the benzoxazine functionalized polyphenylene ether resin prepolymer is as follows: reactants are added to a reaction container in a one-step or multiple-step addition method, wherein the reactants are a phenol source, an amine source and an aldehyde compound, react at 70 to 120° C. for 5 to 60 hours under a nitrogen atmosphere, and post-process to obtain the benzoxazine functionalized polyphenylene ether resin prepolymer. The one-step addition method is to add all the raw materials to the reaction container at the same time, and then add a polar / non-polar mixed solvent to dissolve and react; the multiple-step addition method is to first add an aldehyde compound and an amine compound to the reaction container, and then add a polar / non-polar mixed solvent, and then add a phenol source after sufficient stirring; in: The phenol source in the preparation of the monofunctional benzoxazine functionalized polyphenylene ether resin prepolymer (Formula 1(a)) is a redistributed polyphenylene ether resin, and the amine source is aniline, furfurylamine, allylamine, or p-vinylaniline; The phenol source in the preparation of the bifunctional benzoxazine functionalized polyphenylene ether resin prepolymer (Formula 1(b)) is the redistributed polyphenylene ether resin, and the amine source is 4,4'-diaminodiphenylmethane and hexamethylenediamine; In the preparation of the end-capped main chain benzoxazine functionalized polyphenylene ether resin prepolymer (Formula 1(c)), the phenol source is dihydric phenol and redistributed polyphenylene ether resin, the dihydric phenol is bisphenol A, bisphenol F, bisphenol S, dicyclopentadiene bisphenol A, 4,4'-dihydroxybiphenyl, 4,4'-dihydroxydiphenyl ether, and the amine source is 4,4'-diaminodiphenylmethane and hexamethylenediamine.

10. The preparation method according to claim 9, characterized in that: The redistributed polyphenylene ether resin is obtained by redistributing commercial high molecular weight polyphenylene ether, and the number average molecular weight of the redistributed polyphenylene ether resin is 2027-3827.

11. The use of the polyphenylene ether composite resin with excellent comprehensive performance as claimed in claim 1 in the preparation of resin varnish or prepreg or laminate or multilayer printed circuit board, wherein the resin varnish is composed of the polyphenylene ether composite resin prepolymer as claimed in claim 1 and an organic solvent; the prepreg is prepared by adding inorganic filler and / or flame retardant to the resin varnish; the laminate is formed by uniformly coating the prepreg on non-woven fabric; and the multilayer printed circuit board is made of the laminate.

12. A multilayer printed wiring board comprising a copper foil and a laminate made of a prepreg containing the polyphenylene ether composite resin according to claim 1 supported on the copper foil.

Citation Information

Patent Citations

  • Thermoset resin composition, and prepreg and laminated board made of same

    US20180304604A1

  • Copper-clad laminate using modified polyphenylene oxide

    WO2015046953A1