Apparatus and method for preparing carbon-coated copper alloy core-shell structures and low-temperature sintering solder paste
By adopting low-temperature sintered solder paste with carbon-encapsulated copper alloy core-shell structure, the reliability problem of traditional solder paste under high temperature conditions is solved, low-temperature sintering and high-temperature service are achieved, with good conductivity and oxidation resistance, and the sintering time is shortened , meets the high temperature reliability needs of electronic packaging.
Patent Information
- Application Number
- CN202211001323.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-19
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-08-19
AI Technical Summary
Traditional electronic packaging technology has problems with material fuse and packaging unit cracking under high temperature conditions. The existing metal nano solder paste is easy to oxidize and the connection strength after sintering is insufficient, which affects the reliability of electronic devices.
Low-temperature sintered solder paste is adopted for carbon-covered copper alloy core-shell structure. The carbon layer is coated with the outer core of the nano-copper alloy, combined with flux, and low-temperature sintering and high-temperature service are achieved. The carbon-covered copper alloy core is prepared through specific preparation devices and processes. Shell structure.
Replaces expensive silver or Ag@Cu solder, with good conductivity and thermal conductivity, avoid oxidation, achieve low temperature sintering (minimum 200℃) and high temperature service, shorten sintering time, and the shear strength of the sintered joint meets relevant standards .
Smart Images

Figure CN115647655B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of welding materials, and in particular relates to a device and method for preparing a carbon-coated copper alloy core-shell structure and a low-temperature sintering solder paste. Background Art
[0002] Traditional electronic packaging technology will have many new problems under high temperature conditions, such as material melting, packaging unit cracking and other problems, which seriously affect the high temperature reliability of electronic devices. This poses new challenges to electronic packaging technology. Especially the patch interconnection technology. The patch interconnection technology is a key technology for electronic device packaging. The performance of the connection joint not only determines the topological structure of the internal circuit of the module, but also directly affects the electrical and thermal characteristics and reliability of the module. Traditional connection materials and technologies can no longer meet the packaging needs of electronic devices under such high temperature conditions. Therefore, it is very urgent to explore and develop new interconnection technologies suitable for service under high temperature conditions.
[0003] Metal nanoparticle sintering technology is a technology that uses the size effect of nano-metal particles to reduce the process temperature required for connection. The service temperature of the connection layer formed after sintering can approach the melting point of the bulk material of the same material, thereby achieving "low-temperature connection, high-temperature service". Copper is cheap, abundant, and has high conductivity, making it very suitable for interconnection between chips and substrates. However, copper nanoparticles are easily oxidized, resulting in decreased sintering performance and poor dispersibility. Although core-shell structures such as Ag@Cu (CN105127609A) and Sn@Cu (CN105290418B) have been proposed in related technologies, they are expensive and will form brittle intermetallic compounds, resulting in a decrease in connection strength; moreover, during use, different metals and different components in the joints are prone to breakage, affecting reliability. Summary of the invention
[0004] The present invention aims to provide a carbon-coated copper alloy core-shell structure preparation device, method and low-temperature sintering solder paste to solve the problems of easy oxidation and insufficient connection strength of existing metal nano solder paste after sintering.
[0005] In order to solve the above technical problems, a technical solution adopted by the present invention is to provide a carbon-coated copper alloy core-shell structure low-temperature sintering solder paste, including a core-shell structure and a flux, wherein the core of the core-shell structure is a nano-copper alloy, and the core is covered with a shell layer, which is a carbon layer.
[0006] The working principle and beneficial effects of this solution are:
[0007] A new type of solder is formulated using a core-shell structure of carbon-wrapped copper alloy:
[0008] 1. It can replace expensive solders such as silver, Ag@Cu, Sn@Cu, etc., there is no electromigration phenomenon, and it has good electrical conductivity and thermal conductivity.
[0009] 2. The carbon on the surface of copper alloy has good oxidation resistance, which can protect the internal nano copper alloy core from oxidation and can be sintered at a low temperature of at least 200°C. The sintering temperature of silver solder paste and other commonly used solder pastes is usually 300°C ~ 350°C. After sintering, it meets the relevant standard requirements and achieves the effect of low-temperature sintering and high-temperature service.
[0010] 3. The carbon-coated copper alloy core-shell structure with a nano-copper alloy as the core has extremely strong hydrophobicity, which allows the carbon-coated copper alloy core-shell structure to be stably dispersed in the solvent and is not easy to segregate and aggregate. It is convenient for storage without worrying about oxidation problems, and it can be stably dispersed in large quantities in organic solvents, reducing low-temperature surface diffusion and improving the sintering performance of the solder paste.
[0011] 4. The sintering can be completed within 30 minutes, which is much shorter than the 1h to 3h of Ag@Cu core-shell structure solder paste.
[0012] Optionally, the mass percentage of the core-shell structure in the solder paste is 85% to 90%, and the rest is soldering flux.
[0013] Optionally, the soldering flux includes an organic carrier, a film former, a surfactant, a thixotropic agent and a regulator.
[0014] Optionally, the organic carrier includes at least one of ethanol, ethylene glycol, glycerol, polyethylene glycol, diethylene glycol, terpineol, ethylene glycol butyl ether, diethylene glycol hexyl ether, diethylene glycol octyl ether, tripropylene glycol butyl ether, and diethylene glycol dibutyl ether; the film-forming agent includes at least one of hydrogenated rosin, disproportionated rosin, and acrylic resin; the surfactant includes at least one of OP-10 and EP-10; the thixotropic agent includes at least one of hydrogenated castor oil and polyamide; the regulator includes at least one of isobutanolamine, triethanolamine, diethanolamine, and monoethanolamine.
[0015] In order to solve the above technical problems, another technical solution adopted by the present invention is to provide a preparation device of a carbon-coated copper alloy core-shell structure, including a reaction chamber and a stranded wire, a capacitor is provided in the reaction chamber, two ends of the stranded wire are respectively connected to two electrodes of the capacitor, the capacitor is connected in series with a switch and a pulse power supply, the stranded wire is twisted from multiple metal single-particle wires, and the stranded wire includes at least two metals, one of which is copper.
[0016] Methane gas is used as a source of carbon supply. Methane is added to the reaction chamber to expose the metal strands to the methane gas atmosphere. When the switch is turned off and a high-density pulse current passes through the strands, copper and other metals are heated and evaporated within a few microseconds. Due to the heat generated by the pulse discharge, the methane gas is thermally decomposed into C and H atoms above 600°C. The evaporated copper atoms and other metal atoms first condense to form nanoscale copper alloy cores, and the highly active C atoms are adsorbed on the surface of the copper alloy, inhibiting the growth of the copper alloy core. Since the solubility of C in copper alloys is limited, the adsorbed C atoms can easily diffuse to the Cu surface and move along it, growing into a single layer or multiple layers of carbon, and finally forming a carbon-coated copper alloy core-shell structure.
[0017] Optionally, a vacuum device is also included, and the vacuum device is connected to the reaction chamber. Before preparing the carbon-coated copper alloy core-shell structure, the air in the reaction chamber is firstly evacuated.
[0018] Optionally, the metal single-particle wire has a diameter of 0.1 mm to 1 mm and a length of 60 mm to 80 mm.
[0019] In order to solve the above technical problems, another technical solution adopted by the present invention is to provide a method for preparing a carbon-coated copper alloy core-shell structure. The above preparation device is used to evacuate the reaction chamber to 10 -1 Pa~10 -2 Pa, methane gas was introduced; the capacitor was 2 μF, a pulse current of 32 kV was applied to the capacitor, the pulse discharge duration was 1 μs, and then the solid powder in the reaction chamber was collected.
[0020] Optionally, the gas introduced after vacuuming is a mixed gas of 80% Ar and 20% methane.
[0021] Optionally, the twisted wires are twisted-pair wires formed by twisting copper wires and silver wires, or twisted-triple wires formed by twisting copper wires, zinc wires, and nickel wires. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a schematic diagram of the preparation principle of the carbon-coated copper alloy core-shell structure in Example 1 of the present invention;
[0023] Figure 2 This is an enlarged schematic diagram of the carbon-coated copper alloy core-shell structure in Example 1 of the present invention;
[0024] Figure 3 TEM image of the copper-silver alloy core particle in Example 1 of the present invention;
[0025] Figure 4 TEM image of the carbon-coated copper-silver alloy core-shell structure in Example 1 of the present invention;
[0026] Figure 5This is a TEM image of the copper-zinc-nickel alloy core particle in Example 2 of the present invention;
[0027] Figure 6 TEM image of the carbon-coated copper-zinc-nickel alloy core-shell structure in Example 2 of the present invention;
[0028] Figure 7 It is a curve diagram showing the changes in the anti-oxidation experiments of the carbon-coated copper-silver alloy core-shell structure and the carbon-coated copper-zinc-nickel alloy core-shell structure in Examples 1 and 2 of the present invention;
[0029] Figure 8 This is a Raman spectrum test diagram of the carbon-coated copper-silver alloy core-shell structure in Example 1;
[0030] Fig. 9 This is a Raman spectrum test diagram of the carbon-coated copper-zinc-nickel alloy core-shell structure in Example 2. DETAILED DESCRIPTION
[0031] The following is further described in detail through specific implementation methods:
[0032] The symbols in the drawings of the specification include: power supply 1, switch 2, capacitor 3, twisted wire 4, core-shell structure 5, core 501, and carbon layer 502.
[0033] Embodiment 1
[0034] Preparation of carbon-coated copper alloy core-shell structure of low-temperature sintering solder paste: The preparation principle is as shown in the attached Figure 1 As shown, the wire explosion method is used for preparation: the reaction chamber is prepared with quartz, and an air inlet and an exhaust port are opened on the side wall of the reaction chamber. The air inlet is connected to the gas source, which is a mixture of 80% Ar and 20% methane. The exhaust port is connected to the vacuum device. In this embodiment, the vacuum device is a strong pole 2XZ-1. A capacitor 3 is bonded to the inner wall of the reaction chamber. The capacitor 3 is 2μF. The capacitor 3 is connected in series with a switch 2 and a pulse power supply 1. The pulse power supply 1 selected in this embodiment is ANS / JP60100D. The two plates of the capacitor 3 are connected by a twisted pair 4. The twisted pair 4 is a twisted pair 4 made of copper wire and silver wire. The diameter of the copper wire and the silver wire is 0.3mm and the length is 80mm. The purity of the copper wire and the silver wire is >99.9%. Start the vacuum device first, and evacuate the reaction chamber to 10 -2 After 100 0.05 0.05 0.06 0.08 0.06 ... Figure 2 A small amount of powder was dissolved in ethanol and sampled on a molybdenum mesh and observed under a transmission electron microscope. The TEM image of the particles of the carbon-coated copper-silver alloy core-shell structure 5 is shown in the attached figure. Figure 4 As shown. For comparison, using the above-mentioned preparation device and preparation method, no gas is introduced into the air inlet, and only copper-silver alloy powder particles are prepared. A small amount of powder is also dissolved in ethanol and a sample is prepared on a molybdenum mesh. The TEM image of the copper-silver alloy powder particles is shown in the attached figure. Figure 3 As shown, compare Figure 3 and attached Figure 4 The carbon layer 502 covering the copper-silver alloy powder particles can be clearly seen.
[0035] Preparation of low-temperature sintering solder paste: The prepared core-shell structure 5 powder is mixed with the flux in a mass percentage of 85%:15%. The flux includes an organic carrier, a film former, a surfactant, a thixotropic agent and a regulator. The organic carrier is ethylene glycol, the film former is an acrylic resin; the surfactant is a mixture of OP-10 and EP-10; the thixotropic agent is a mixture of hydrogenated castor oil and polyamide; the regulator is isobutanolamine, and the pH of the solder paste is adjusted to 7 with the regulator.
[0036] The prepared solder paste was screen printed to prepare an 80μm solder paste layer on the copper substrate, and then another copper plate was added on top of the solder paste. It was preheated at 60°C for 5 minutes, kept warm at 200°C and 10MPa pressure in air for 5 minutes, and then switched to a 90% Ar and 10% H2 mixed gas atmosphere for 20 minutes, and then cooled with the furnace. The shear strength of the sintered solder paste joint was tested to be 20.8MPa, which meets the "GB / T 4937.19-2018" (Mechanical and Climatic Test Methods for Semiconductor Devices Part 19: Chip Shear Strength) standard.
[0037] Embodiment 2
[0038] The difference between this embodiment and the first embodiment is that: when preparing the carbon-coated copper alloy core-shell structure of the low-temperature sintered solder paste, the stranded wire 4 is a three-stranded wire 4 twisted by copper wire, zinc wire and nickel wire, and the diameters of the copper wire, zinc wire and nickel wire are 0.64 mm, 0.18 mm and 0.18 mm respectively, and the lengths are all 80 mm. The obtained carbon-coated copper alloy core-shell structure 5 is a carbon-coated copper-zinc-nickel alloy core-shell structure 5. Take a small amount of powder and dissolve it in ethanol, prepare a sample on a molybdenum mesh, and observe it under a transmission electron microscope. The TEM image of the particles of the carbon-coated copper-zinc-nickel alloy core-shell structure 5 is shown in the attached figure. Figure 6 As shown. For comparison, using the above-mentioned preparation device and preparation method, no gas is introduced into the air inlet, and only copper-zinc-nickel alloy powder particles are prepared. A small amount of powder is also dissolved in ethanol, and a sample is prepared on a molybdenum mesh. The TEM image of the copper-zinc-nickel alloy powder particles is shown in the attached figure. Figure 5 As shown, compare Figure 6 and attached Figure 5The carbon layer 502 covering the copper-zinc-nickel alloy powder particles can be clearly seen.
[0039] The preparation of low-temperature sintering solder paste is the same as that in the embodiment. The prepared solder paste is screen-printed to prepare an 80μm solder paste layer on a copper substrate, and then another copper plate is added on top of the solder paste. After preheating at 60°C for 5 minutes, it is kept warm for 5 minutes in air at 200°C and 10MPa pressure, and then converted to an atmosphere of 90% Ar and 10% H2 mixed gas for 20 minutes, and then cooled with the furnace. The shear strength of the joint sintered with solder paste was tested, which was 29.6MPa, meeting the standard of "GB / T 4937.19-2018" (Mechanical and Climatic Test Methods for Semiconductor Devices Part 19: Chip Shear Strength).
[0040] In the above embodiment, the solder paste prepared based on the carbon-clad copper alloy core-shell structure 5 achieves low-temperature sintering at 200°C, and the shear strength of the sintered joint fully meets and significantly exceeds the requirements of the "GB / T 4937.19-2018" standard, has excellent service performance, and the sintering time does not exceed 30 minutes, which reduces the sintering time.
[0041] Antioxidant test:
[0042] Take 10g of the solid powder of the carbon-coated copper-silver alloy core-shell structure 5 in Example 1, and then take 10g of the solid powder of the carbon-coated copper-zinc-nickel alloy core-shell structure 5 in Example 2, and perform antioxidant experiments in a constant temperature and humidity chamber under the conditions of 85°C and 85%RH. The total antioxidant time is 1000h. The resistivity of each powder is measured at 0h, 24h, 48h, 96h, 168h, 500h, and 1000h. The changes in the resistivity of the solid powders in Examples 1 and 2 are shown in the attached figure. Figure 7 From the results of the anti-oxidation experiment, the resistivity of the carbon-coated copper-silver alloy core-shell structure 5 and the carbon-coated copper-zinc-nickel alloy core-shell structure 5 prepared in Examples 1 and 2 hardly changed after the anti-oxidation experiment, which proves that the structure is stable and the anti-oxidation property is good.
[0043] Raman spectroscopy experiment:
[0044] The carbon-coated copper-silver alloy core-shell structure 5 in Example 1 and the carbon-coated copper-zinc-nickel alloy core-shell structure 5 in Example 2 were tested for Raman spectroscopy. Since there is only one atom in the unit cell of the metal, it only has an acoustic branch that moves in the same direction, which is not easy to cause a change in polarizability. Raman activity is determined by whether the polarizability changes, so the metal does not have Raman activity. After the nano-copper alloy particles are coated with a carbon layer, the Raman spectrum measures two peaks, as shown in the attached figure. Figure 8 and Fig. 9 As shown, they are located at 1350cm -1 and 1580cm-1 , which correspond to the defect peak D and the intrinsic peak G of carbon respectively, proving that the substance wrapped on the surface of the copper-silver alloy particles in Example 1 and the substance wrapped on the surface of the copper-zinc-nickel alloy particles in Example 2 are both carbon layers 502, and both successfully produce carbon-coated nano-copper alloy core-shell structures 5.
[0045] The above are only embodiments of the present invention. The invention is not limited to the fields involved in this implementation case. The common sense such as the known specific structures and characteristics in the scheme is not described in detail here. The ordinary technicians in the relevant field know all the common technical knowledge in the technical field to which the invention belongs before the application date or the priority date, can obtain all the existing technologies in the field, and have the ability to apply the conventional experimental means before that date. The ordinary technicians in the relevant field can improve and implement this scheme in combination with their own abilities under the enlightenment given by this application. Some typical known structures or known methods should not become obstacles for ordinary technicians in the relevant field to implement this application. It should be pointed out that for those skilled in the art, without departing from the structure of the present invention, several deformations and improvements can be made, which should also be regarded as the protection scope of the present invention, which will not affect the effect of the implementation of the present invention and the practicality of the patent. The protection scope required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to explain the content of the claims.
Claims
1. A method for preparing a carbon-coated copper alloy core-shell structure using a carbon-coated copper alloy core-shell structure preparation device, characterized in that: A carbon-coated copper alloy core-shell structure low-temperature sintering solder paste comprises a core-shell structure and a soldering flux, wherein the core of the core-shell structure is a nano copper alloy, and the core is covered with a shell layer, which is a carbon layer; A preparation device for a carbon-coated copper alloy core-shell structure comprises a reaction chamber and a twisted wire, wherein a capacitor is arranged in the reaction chamber, two ends of the twisted wire are respectively connected to two electrodes of the capacitor, the capacitor is connected in series with a switch and a pulse power supply, the twisted wire is twisted by a plurality of metal single-particle wires, the twisted wire comprises at least two metals, one of which is copper; a vacuum device is also included, and the vacuum device is connected to the reaction chamber; the diameter of the metal single-particle wire is 0.1 mm to 1 mm, and the length is 60 mm to 80 mm; the twisted wire is a twisted pair of copper wires and silver wires, or a twisted triple of copper wires, zinc wires and nickel wires; The preparation method comprises: evacuating the reaction chamber to 10 -1 Pa~10 -2 After Pa, a mixed gas of 80% Ar and 20% methane was introduced; the capacitor was 2 μF, a pulse current of 32 kV was applied to the capacitor, the pulse discharge duration was 1 μs, and then the solid powder in the reaction chamber was collected; The mass percentage of the core-shell structure in the solder paste is 85% to 90%, and the rest is flux; The flux includes organic carrier, film former, surfactant, thixotropic agent and regulator.
2. The method for preparing a carbon-coated copper alloy core-shell structure using a carbon-coated copper alloy core-shell structure preparation device according to claim 1, characterized in that: The organic carrier includes at least one of ethanol, ethylene glycol, glycerol, polyethylene glycol, diethylene glycol, terpineol, ethylene glycol butyl ether, diethylene glycol hexyl ether, diethylene glycol octyl ether, tripropylene glycol butyl ether, and diethylene glycol dibutyl ether; the film-forming agent includes at least one of hydrogenated rosin, disproportionated rosin, and acrylic resin; the surfactant includes at least one of OP-10 and EP-10; the thixotropic agent includes at least one of hydrogenated castor oil and polyamide; the regulator includes at least one of isobutanolamine, triethanolamine, diethanolamine, and monoethanolamine.