A method for preparing a composite mica tape and mica tape prepared using the same
By combining dip coating and micro-concave roller coating, a dense epoxy resin coating is formed and adhesive is applied thereon, which solves the problems of adhesive infiltration and solvent residue and improves the uniform thickness of mica tape and structural performance simplifies process flow and enhances safety.
Patent Information
- Application Number
- CN202211228391.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-08
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-10-08
AI Technical Summary
In the existing mica tape preparation method, adhesive is prone to penetrate into the porous structure, making it difficult to accurately grasp the coating thickness, and solvent residues cause environmental pollution and safety hazards.
Using the combination of dip coating and micro-concave roller coating, a dense epoxy resin coating is formed first, and then adhesive is applied thereon. The organic solvent is removed by drying twice to ensure that the adhesive does not penetrate into the skeleton. In the structure, and facilitates the control of the thickness of the glue layer.
It significantly improves the thickness uniformity and structural performance of mica tape, avoids solvent residues and environmental pollution, simplifies the process flow, and improves production efficiency and safety performance.
Smart Images

Figure CN115651561B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of insulating tapes, and in particular to a method for preparing a composite mica tape and a mica tape prepared by using the method. Background Art
[0002] Mica tape is a kind of insulation material with excellent high temperature resistance and combustion resistance, and is suitable for fire-resistant insulation layers of various fire-resistant electromagnetic cables and coils, as well as widely used in motor insulation and cable fields. During use, mica tape only needs to be adhered to the surface of motors and other equipment to achieve the purpose of heat insulation and insulation of the surface of motors and other electrical appliances, and to achieve the effect of protecting the motor surface, and has good fire-resistant and flame-retardant properties.
[0003] At present, the preparation method of mica tape generally adopts the coating method to apply the adhesive to the reinforcing material through a roller. The specific operation is: first, the mica raw material is adsorbed onto the reinforcing material by using an electrostatic field. In order to further fix the mica raw material, the adhesive is sprayed onto the reinforcing material of the mica raw material, and then a second layer of reinforcing material is compounded to obtain a semi-finished product of a double-sided reinforced mica tape, which is then dried in an oven to remove the organic solvent, and then rolled into a mica tape roll after cooling, and finally a double-sided reinforced mica tape finished product is obtained.
[0004] Such preparation method has the following technical defects and deficiencies:
[0005] ①. The skeleton structure of the mica substrate composed of mica raw materials and reinforcing materials is a loose porous structure. If the adhesive is directly coated on the reinforcing material of the mica raw materials, the adhesive will easily penetrate into the porous layer, thereby affecting the coating thickness of the adhesive, resulting in the inability to accurately control the coating thickness, poor thickness uniformity, and difficulty in achieving thick adhesive coating;
[0006] ② In addition, if the solvent in the adhesive penetrates into the skeleton structure of the mica substrate, that is, remains in the mica tape and is then slowly released from it, it will have an adverse effect on the health of users and the environment. When the solvent inside evaporates into the atmosphere, it will cause environmental pollution and easily lead to safety hazards such as fire. Summary of the invention
[0007] In order to overcome the technical problems that the adhesive in the mica tape preparation method described in the above-mentioned prior art easily penetrates into the porous structure, resulting in difficulty in accurately controlling the coating thickness and easily causing environmental pollution and safety hazards, the present invention provides a method for preparing a composite mica tape and a mica tape prepared using the same.
[0008] The technical solution adopted by the present invention to solve the problem is:
[0009] A method for preparing a composite mica tape comprises the following steps:
[0010] S1. The first fiber reinforced layer and the second fiber reinforced layer are composited on both sides of the mica layer to obtain a mica skeleton structure;
[0011] S2. performing a dip coating operation on the mica skeleton structure so that the surface of the first fiber reinforced layer, the surface of the second fiber reinforced layer, between the first fiber reinforced layer and the mica layer, and between the second fiber reinforced layer and the mica layer are coated with an epoxy resin coating;
[0012] S3. performing a first drying operation on the mica skeleton structure to remove moisture from the epoxy resin coating so that the epoxy resin coating forms a continuous, dense epoxy resin coating to obtain a mica substrate semi-finished product;
[0013] S4. The mica substrate semi-finished product is subjected to a micro-concave roller coating operation to form a continuous and uniform adhesive coating on the epoxy resin coating;
[0014] S5. performing a second drying operation on the mica substrate semi-finished product to remove the organic solvent in the adhesive coating.
[0015] In the first embodiment of the present invention, a technical solution for performing a dip coating operation on a mica skeleton structure is disclosed.
[0016] Wherein, in step S2, the “immersion coating operation on the mica skeleton structure” is specifically:
[0017] The mica skeleton structure is introduced into an impregnation container filled with epoxy resin coating, so that the surface of the first fiber reinforced layer, the surface of the second fiber reinforced layer, the gap between the first fiber reinforced layer and the mica layer, and the gap between the second fiber reinforced layer and the mica layer are fully saturated and impregnated with the epoxy resin coating.
[0018] Furthermore, the epoxy resin coating is a water-based coating using water as a solvent, and the immersion temperature is controlled at 20° C. to 30° C. The viscosity of the epoxy resin coating under this temperature condition is 400 cps to 2000 cps, and the solid content is 30 wt% to 50 wt%.
[0019] Furthermore, during the dip coating operation, the coating line speed is 40m / min to 60m / min, the residence time of the mica skeleton structure in the dipping container is 0.1s to 0.3s, and its walking time in the dipping container is increased by winding the roller.
[0020] In the second embodiment of the present invention, a technical solution for how to perform an extrusion operation on a mica skeleton structure is disclosed.
[0021] Wherein, between step S2 and step S3, there is further provided step S6, which is specifically:
[0022] S6. Extruding the mica skeleton structure to squeeze out the excess epoxy resin coating, so that the epoxy resin coating is evenly and densely coated on the surface of the first fiber reinforced layer and the surface of the second fiber reinforced layer.
[0023] In the third embodiment of the present invention, a technical solution is disclosed for performing micro-concave roller coating operation on a mica substrate semi-finished product.
[0024] Wherein, in step S4, the “performing a micro-concave roller coating operation on the mica substrate semi-finished product” is specifically:
[0025] The mica substrate semi-finished product is introduced into a coating container filled with an adhesive, and a micro-concave roller is provided in the adhesive, so that the mica substrate semi-finished product and the micro-concave roller are in contact, and the micro-concave roller is driven to rotate by pulling the mica substrate semi-finished product, so that the adhesive is continuously coated on the surface of the mica substrate semi-finished product.
[0026] Furthermore, the solvent of the adhesive includes water, the coating temperature is controlled at 20° C. to 30° C., the viscosity of the adhesive under this temperature condition is 400 cps to 2000 cps, and the solid content is 30 wt % to 50 wt %.
[0027] In the fourth embodiment of the present invention, a technical solution for attaching a release film to a mica substrate semi-finished product is disclosed.
[0028] After step S5, step S7 is further provided, which is specifically:
[0029] S7. Attach a release film to the surface of the adhesive coating to form a release layer, and then press the film to obtain a multi-layer composite mica tape.
[0030] Based on the same design concept, the present invention also provides an embodiment of a mica tape, which includes:
[0031] A mica layer, a first fiber reinforced layer and a second fiber reinforced layer, wherein the first fiber reinforced layer and the second fiber reinforced layer are respectively arranged on both sides of the mica layer;
[0032] a first epoxy resin coating and a second epoxy resin coating, wherein the first epoxy resin coating is disposed between the first fiber reinforced layer and the mica layer and on the surface of the first fiber reinforced layer, and the second epoxy resin coating is disposed between the second fiber reinforced layer and the mica layer and on the surface of the second fiber reinforced layer;
[0033] An adhesive coating, wherein the adhesive coating is disposed on a surface of the first epoxy resin coating;
[0034] A release layer is disposed on the surface of the adhesive coating.
[0035] Further, the thickness of the first epoxy resin coating and the second epoxy resin coating is 2 μm to 6 μm;
[0036] The thickness of the adhesive coating is 4 μm to 50 μm, and the thickness difference of the adhesive coating is less than 2 μm.
[0037] In summary, the preparation method of the composite mica tape provided by the present invention and the mica tape prepared using the same have at least the following technical effects compared with the prior art:
[0038] 1) The preparation method of the composite mica tape provided by the present invention adopts a coating method combining dip coating and micro-concave roller coating. The whole process includes two coating operations and two baking operations. The coating is performed continuously to achieve three-layer composite coating (including two layers of epoxy resin coating and one layer of adhesive coating), and finally a release film is attached. The preparation method is easy to operate and has a simple process flow, which can significantly improve the production efficiency and the performance of the mica tape.
[0039] 2) In the preparation method of the composite mica tape provided by the present invention, the mica skeleton structure is first dip-coated to form a dense epoxy resin coating on the surface of the mica skeleton structure, so that when the adhesive coating is subsequently applied, the adhesive is not easy to penetrate into the mica skeleton structure, that is, no solvent residue phenomenon is generated, thereby avoiding environmental pollution and safety hazards; and when the adhesive coating is directly applied on the epoxy resin coating by a micro-concave roller coating method, it is convenient to control the thickness of the adhesive, and it is easy to apply a thicker adhesive layer;
[0040] 3) In the mica tape prepared by the preparation method of the composite mica tape provided by the present invention, the first epoxy resin coating and the second epoxy resin coating can respectively play a role in adhesive bonding and structural reinforcement between the first fiber reinforced layer and the mica layer, and between the second fiber reinforced layer and the mica layer, and can significantly improve the overall structural properties of the mica tape, such as tensile strength and elongation at break. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 The process flow chart of the preparation method of the composite mica tape of the present invention;
[0042] Figure 2 It is a schematic diagram of the interlayer structure of the mica tape of the present invention;
[0043] Figure 3 is a scatter plot with a smooth line for epoxy coating thickness versus tensile strength;
[0044] Figure 4 is a scatter plot with a smooth line of epoxy coating thickness and elongation at break;
[0045] The meanings of the reference numerals are as follows:
[0046] 1. Mica layer; 2. First fiber reinforcement layer; 3. Second fiber reinforcement layer; 4. First epoxy resin coating; 5. Second epoxy resin coating; 6. Adhesive coating; 7. Release layer. DETAILED DESCRIPTION
[0047] For better understanding and implementation, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the embodiments of the present invention.
[0048] In the description of the present invention, it should be noted that the terms "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside" and "outside" etc. indicating directions or positional relationships are based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as a limitation on the present invention.
[0049] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0050] See also Figure 1 and Figure 2 As shown, according to an embodiment of the present invention, the method for preparing the composite mica tape comprises the following steps:
[0051] Step S1: Compounding the first fiber reinforced layer 2 and the second fiber reinforced layer 3 on both sides of the mica layer 1 to obtain a mica skeleton structure. The first fiber reinforced layer 2 and the second fiber reinforced layer 3 can be compounded on the mica layer 1 by electrostatic adsorption in an electrostatic field, or other processes can be used to achieve the compounding of the three.
[0052] Step S2: The mica skeleton structure obtained in step S1 is dip-coated to coat the surface of the first fiber reinforced layer 2, the surface of the second fiber reinforced layer 3, between the first fiber reinforced layer 2 and the mica layer 1, and between the second fiber reinforced layer 3 and the mica layer 1 with epoxy resin coating.
[0053] Step S3: The mica skeleton structure obtained in step S2 is subjected to the first drying operation to remove moisture from the epoxy resin coating on the surface of the first fiber reinforced layer 2, the surface of the second fiber reinforced layer 3, between the first fiber reinforced layer 2 and the mica layer 1, and between the second fiber reinforced layer 3 and the mica layer 1, so that the epoxy resin coating forms a continuous and dense epoxy resin coating to obtain a mica substrate semi-finished product. The epoxy resin coating formed includes a first epoxy resin coating 4 and a second epoxy resin coating 5. Specifically, the oven used for the drying operation in this step can preferably be a six-stage suspension oven, the length of a single-stage oven is 3m to 6m, and the temperature of each oven can be set to 90°C / 100°C / 120°C / 120°C / 100°C / 80°C in sequence, with a tolerance of ±10°C.
[0054] Step S4: The mica substrate semi-finished product obtained in step S3 is subjected to a micro-concave roller coating operation to form a continuous and uniform adhesive coating 6 on the epoxy resin coating. In this step, the adhesive coating 6 is specifically coated on the surface of the first epoxy resin coating 4, the surface of the second epoxy resin coating 5, or the surfaces of both, so that the mica tape has single-sided or double-sided adhesive properties.
[0055] Step S5: The mica substrate semi-finished product obtained in step S4 is dried for the second time to remove the organic solvent in the adhesive coating 6. The drying operation in this step can be carried out in a five-stage oven, the length of a single-stage oven is 3m to 5m, and the temperature of each oven can be set to 90°C / 100°C / 120°C / 100°C / 80°C in sequence, with a tolerance of ±10°C.
[0056] In the technical solution of this embodiment, the preparation method of the composite mica tape adopts a coating method combining dip coating and micro-concave roller coating. The entire preparation process includes two coating operations and two baking operations, and the coating is continuously performed to achieve the composite coating of the first epoxy resin coating 4, the second epoxy resin coating 5 and the adhesive coating 6. The preparation method is easy to operate and has a simple process flow, which can significantly improve the production efficiency and the performance of the mica tape. More specifically, the preparation method first performs a dip coating operation on the mica skeleton structure to form a dense first epoxy resin coating 4 and a second epoxy resin coating 5 on the surface of the mica skeleton structure, so that when the adhesive coating 6 is subsequently coated with the micro-concave roller, the adhesive is not easy to penetrate into the mica skeleton structure, that is, no solvent residue phenomenon will be generated, and the residual solvent is prevented from being released from the mica skeleton structure, causing adverse effects on the health and environment of the user, and it can also prevent the residual solvent from evaporating into the atmosphere, causing environmental pollution and causing safety hazards such as fire and explosion. In addition, when the adhesive coating 6 is directly coated on the first epoxy resin coating 4 and / or the second epoxy resin coating 5 by means of a micro-concave roller coating method, the thickness of the adhesive can be easily controlled, and a thicker adhesive layer can be easily coated.
[0057] Furthermore, the dip-coated first epoxy resin coating 4 and the second epoxy resin coating 5 can respectively play a role in adhesive bonding and structural reinforcement between the first fiber reinforced layer 2 and the mica layer 1, and between the second fiber reinforced layer 3 and the mica layer 1, thereby significantly improving the overall structural properties of the mica tape, such as tensile strength and elongation at break.
[0058] Example 1
[0059] In the first embodiment of the present invention, a technical solution for performing a dip coating operation on a mica skeleton structure is disclosed.
[0060] In the technical solution of this embodiment, in step S2, "immersion coating operation on the mica skeleton structure" is specifically: introducing the mica skeleton structure obtained in step S1 into an immersion container filled with epoxy resin coating, so that the surface of the first fiber reinforced layer 2, the surface of the second fiber reinforced layer 3, the gap between the first fiber reinforced layer 2 and the mica layer 1, and the gap between the second fiber reinforced layer 3 and the mica layer 1 are fully saturated with the epoxy resin coating. Wherein. The immersion container can be preferably an immersion tank, which contains a preset volume of water-based epoxy resin coating. After this immersion coating process, the mica skeleton structure can have better waterproof, moisture-proof and anti-corrosion effects, and at the same time, the mica skeleton structure has better mechanical properties, and has better adhesion with the adhesive applied in the subsequent steps, thereby increasing its adhesion.
[0061] In a preferred embodiment of the present invention, the epoxy resin coating is a water-based coating using water as a solvent. In step S2, the immersion temperature in the immersion tank (i.e., the feeding temperature of the mica skeleton structure) is controlled at 20°C to 30°C. The viscosity of the epoxy resin coating under this temperature condition is 400cps to 2000cps, and the solid content is 30wt% to 50wt%. The glass transition temperature of the first epoxy resin coating 4 and the second epoxy resin coating 5 formed after the glue is dried and cured is 90°C to 120°C.
[0062] In another preferred embodiment of this embodiment, when the dip coating operation is performed, the coating line speed is 40m / min to 60m / min, and the residence time of the mica skeleton structure obtained in step S1 in the dipping container is 0.1s to 0.3s. In addition, this step also increases the walking time of the mica skeleton structure in the dipping container by winding the roller, ensuring that the surface of the first fiber reinforced layer 2, the surface of the second fiber reinforced layer 3, the gap between the first fiber reinforced layer 2 and the mica layer 1, and the gap between the second fiber reinforced layer 3 and the mica layer 1 are fully saturated and impregnated with the epoxy resin coating.
[0063] Example 2
[0064] In the second embodiment of the present invention, a technical solution for how to perform an extrusion operation on a mica skeleton structure is disclosed.
[0065] In the technical solution of this embodiment, step S6 is further provided between step S2 and step S3, specifically: extruding the mica skeleton structure obtained in step S2 to squeeze out the excess epoxy resin coating, so that the epoxy resin coating is evenly and densely coated on the surface of the first fiber reinforced layer 2 and the surface of the second fiber reinforced layer 3. The mica skeleton structure after the extrusion and impregnation operation can be squeezed out by an extrusion roller, so that the excess epoxy resin coating in the gap between the first fiber reinforced layer 2 and the mica layer 1 and the gap between the second fiber reinforced layer 3 and the mica layer 1 is squeezed out, ensuring the subsequent formation of a continuous and dense epoxy resin coating; and under the extrusion action of the extrusion roller, it can be ensured that the epoxy resin coating is evenly and densely coated on the surface of the first fiber reinforced layer 2 and the surface of the second fiber reinforced layer 3.
[0066] More specifically, the extrusion rollers in this step may preferably adopt vertical three-roll extrusion, and the extrusion pressure is 0.05MPa to 0.1MPa, and the extrusion pressure can be adjusted by adjusting the air pressure.
[0067] Example 3
[0068] In the third embodiment of the present invention, a technical solution is disclosed for performing micro-concave roller coating operation on a mica substrate semi-finished product.
[0069] In the technical solution of this embodiment, in step S4, "performing micro-concave roller coating operation on the mica substrate semi-finished product" is specifically:
[0070] The mica substrate semi-finished product obtained in step S3 is introduced into a coating container containing adhesive, and a micro-concave roller is provided in the adhesive, so that the mica substrate semi-finished product and the micro-concave roller are in contact, and the micro-concave roller is driven to rotate by pulling the mica substrate semi-finished product, so that the adhesive is continuously coated on the surface of the mica substrate semi-finished product. Specifically, the coating container can preferably be a coating tank containing a preset volume of adhesive, and the coating tank is provided with a micro-concave roller, and the bottom of the micro-concave roller is immersed in the adhesive coating liquid, and the top is in contact with the mica substrate semi-finished product, so in the process of pulling the mica substrate semi-finished product to move, the adhesive coating liquid in the coating tank can be evenly coated on the surface of the mica substrate semi-finished product, that is, the surface of the first epoxy resin coating 4 / the second epoxy resin coating 5.
[0071] More specifically, the micro-concave roller in this step can be a serpentine roller, anilox roller, hexagonal dots, quadrilateral dots and other roller patterns, the roller diameter is 30mm-90mm, the roller material is chrome-plated stainless steel, and the roller mesh number is 20-300 meshes.
[0072] In a preferred embodiment of the present invention, the solvent of the adhesive contained in the coating tank includes water, PMA, butanone, xylene, etc. The coating temperature (i.e., the feeding temperature of the mica substrate semi-finished product) is controlled at 20°C to 30°C. The viscosity of the adhesive under this temperature condition is 400cps to 2000cps, and the solid content is 30wt% to 50wt%.
[0073] Example 4
[0074] In the fourth embodiment of the present invention, a technical solution for attaching a release film to a mica substrate semi-finished product is disclosed.
[0075] After step S5, step S7 is further provided, specifically: attaching a release film to the surface of the adhesive coating to form a release layer, and then laminating to obtain a multi-layer composite mica tape. The laminating pressure of the laminating operation is 0.05MPa to 0.10MPa, and the pressure is adjusted by adjusting the air pressure. By providing the release layer, the structure of the mica tape can be protected.
[0076] In summary, the preparation method of the composite mica tape provided by the present invention adopts a coating method combining dip coating and micro-concave roller coating. The entire process includes two coating operations and two baking operations. The coating is performed continuously to achieve a composite coating of two layers of epoxy resin coating and one layer of adhesive coating. Finally, a release film is attached. The preparation method is easy to operate and has a simple process flow, which can significantly improve the production efficiency and the performance of the mica tape. In addition, in the preparation method of the composite mica tape provided by the present invention, the mica skeleton structure is first dip-coated to form a dense epoxy resin coating on the surface of the mica skeleton structure, so that when the adhesive coating is subsequently applied, the adhesive is not easy to penetrate into the mica skeleton structure, that is, no solvent residue phenomenon will be generated, thereby avoiding environmental pollution and safety hazards. Moreover, when the adhesive coating is directly applied on the epoxy resin coating by micro-concave roller coating, it is convenient to control the thickness of the glue, and it is easy to apply a thicker adhesive layer.
[0077] Example 5
[0078] Based on the same design concept, the present invention also provides a mica tape, which is prepared by the preparation method of the composite mica tape described in the above embodiment.
[0079] See also Figure 2As shown, in the technical solution of this embodiment, the mica tape specifically includes a mica layer 1, a first fiber reinforced layer 2 and a second fiber reinforced layer 3, and the first fiber reinforced layer 2 and the second fiber reinforced layer 3 are respectively arranged on both sides of the mica layer 1. Among them, the surface of the first fiber reinforced layer 2 is provided with a first epoxy resin coating 4, the surface of the second fiber reinforced layer 3 is provided with a second epoxy resin coating 5, and the surface of the first epoxy resin coating 4 is also provided with an adhesive coating 6.
[0080] Through this structural design, a dense epoxy resin coating can be formed on the mica skeleton structure (composed of the mica layer 1, the first fiber reinforced layer 2 and the second fiber reinforced layer 3), so when the adhesive coating 6 is applied, the solvent in the adhesive coating 6 will not penetrate into the mica skeleton structure, that is, no solvent residue will be generated, ensuring safety and environmental protection, and because the adhesive coating 6 will not penetrate into the mica skeleton structure, the thickness uniformity of the adhesive coating 6 can be ensured. In addition, by arranging the first epoxy resin coating 4 on the mica substrate, the adhesive coating 6 can be directly applied on the first epoxy resin coating 4 during processing, so that it is easy to control the thickness of the adhesive layer, and it is easy to apply a thicker adhesive coating 6, and the structural design is simple and reasonable and the operation process is simple.
[0081] More specifically, a first epoxy resin coating 4 is also provided between the first fiber reinforced layer 2 and the mica layer 1, and a second epoxy resin coating 5 is also provided between the second fiber reinforced layer 3 and the mica layer 1. The first epoxy resin coating 4 and the second epoxy resin coating 5 respectively play a role in adhesive bonding and structural reinforcement between the first fiber reinforced layer 2 and the mica layer 1, and between the second fiber reinforced layer 3 and the mica layer 1, which can significantly improve the structural properties of the mica tape of the present invention, such as the tensile strength and elongation at break. In addition, in the structural design of the present invention, since the water in the adhesive coating 6 and the two epoxy resin coatings is baked out as a solvent during processing, there is no solvent residue in the finished mica tape, and the safety performance is high and the pollution is small.
[0082] Furthermore, the mica tape further includes a release layer 7, which is disposed on the surface of the adhesive coating 6. The release layer 7 is disposed on the outermost side of the mica tape of the present invention, and the release layer 7 is attached at the end of the process flow, which can play a structural protection role for the mica tape. More specifically, the release agent used in the release layer 7 in this embodiment can preferably be a silicon-free, low silicon content, or organic silicon release agent; and the thickness of the release layer 7 is set to 10 μm to 50 μm, and the release force is 50 g to 300 g.
[0083] In an optional solution of this embodiment, the thickness of the adhesive coating 6 can be set to 4 μm to 50 μm, and the specific thickness setting depends on the bonding ability requirement of the mica tape. Based on the structural design of the first epoxy resin coating 4, the mica tape can be coated with a relatively thick adhesive coating 6. In addition, the thickness difference of the adhesive coating 6 is less than 2 μm, that is, in the applied adhesive coating 6, the difference between the maximum thickness and the minimum thickness of the adhesive coating 6 is less than 2 μm, ensuring that the thickness distribution of the adhesive coating 6 is uniform.
[0084] In another optional scheme of this embodiment, the thickness of the first epoxy resin coating 4 and the second epoxy resin coating 5 is set to 2μm~6μm, and the following test examples are used to test the mechanical properties of the mica tape of the present invention at different thicknesses of the first epoxy resin coating 4 and the second epoxy resin coating 5.
[0085] Test Case
[0086] Test object: 7 groups of mica tapes with different epoxy resin coating thicknesses, with the number of mica tapes in each group being greater than or equal to 3.
[0087] Test items: Testing the mechanical performance parameters of mica tape under different first epoxy resin coating 4 / second epoxy resin coating 5 thickness parameters (hereinafter referred to as epoxy resin coating thickness). It is worth mentioning that the present invention can be tested by measuring tools, clamps, tensile devices and other devices, and can also be tested by professional tensile testing machines. The specific test method is not limited.
[0088] Test results:
[0089] This test was conducted on 7 groups of mica tapes with different epoxy resin coating thicknesses, and 7 groups of tensile strength and 7 groups of elongation at break data were obtained. The specific test results are shown in Table 1 below.
[0090] It is worth mentioning that due to the influence of factors such as supplier materials, ambient temperature and humidity, it is impossible to accurately determine the mechanical performance parameters under the sum of various thickness conditions to a certain value through a single test. This test example uses the stable values in multiple tests as the calculation and comparison object to obtain the test conclusions in Table 1 below.
[0091] Table 1 Effect of epoxy resin coating thickness on mechanical properties
[0092]
[0093]
[0094] Analytical methods
[0095] With the epoxy resin coating thickness as the horizontal axis and the tensile strength as the vertical axis, a scatter plot can be drawn. By connecting each scatter point in sequence with a smooth line, we can get Figure 3 The scatter plot with smoothed line for epoxy coating thickness vs. tensile strength is shown in Figure 2. Figure 3 It can be seen that:
[0096] When the epoxy resin coating thickness is 2 μm, the tensile strength (or tensile strength) value is 72 N / mm 2 Considering that the function of the first epoxy resin coating 4 / the second epoxy resin coating 5 is to strengthen the structural performance of the mica tape, if the tensile strength is lower than 72N / mm 2 It is difficult to achieve the structural strengthening effect of enhancing the fracture resistance, so the optimal value of the minimum thickness of the epoxy resin coating should be 2μm;
[0097] When the thickness of the epoxy resin coating is in the range of 2 to 6 μm, the slope of the curve in the coordinate graph is large, that is, the growth rate of the tensile strength with increasing thickness is high, indicating that when the sum of the coating thickness is in the range of 2 to 6 μm, the tensile strength can be increased by increasing the coating thickness, and the effect of this method is more obvious;
[0098] When the thickness of the epoxy resin coating is greater than 6 μm, the slope of the curve in the coordinate graph is small, that is, the growth rate of the tensile strength (or tensile strength) with increasing thickness is low, and it approaches zero infinitely with the increase of the thickness of the epoxy resin coating. This means that when the thickness of the epoxy resin coating is greater than 6 μm, it is difficult to increase the tensile strength by increasing the thickness of the coating. Considering the cost of the material, the optimal value of the maximum thickness of the epoxy resin coating should be 6 μm.
[0099] It can be seen from this that the optimal value of the thickness of the epoxy resin coating of the present invention is 2 to 6 μm.
[0100] With the epoxy resin coating thickness as the horizontal axis and the elongation at break as the vertical axis, a scatter plot can be drawn. By connecting each scatter point in sequence with a smooth line, we can get Figure 4 The scatter plot with smoothed line of epoxy coating thickness and elongation at break is shown in Figure 4 It can be seen that:
[0101] When the thickness of the epoxy resin coating is 2 μm, the value of the elongation at break is 17%. Considering that the function of the two epoxy resin coatings is to strengthen the structure of the mica tape, if the elongation at break is lower than 17%, it is difficult to play the structural strengthening effect of strengthening toughness. Therefore, the optimal value of the minimum thickness of the epoxy resin coating should be 2 μm.
[0102] When the thickness of the epoxy resin coating is in the range of 2 to 6 μm, the slope of the curve in the coordinate graph is large, that is, the growth rate of the elongation at break with increasing thickness is high, indicating that when the sum of the coating thickness is in the range of 2 to 6 μm, the elongation at break can be increased by increasing the coating thickness, and the effect of this method is more obvious;
[0103] When the thickness of the epoxy resin coating is greater than 6μm, the slope of the curve in the coordinate graph is small, that is, the growth rate of the elongation at break with increasing thickness is low, and it approaches zero infinitely with the increase of the thickness of the epoxy resin coating. This means that when the thickness of the epoxy resin coating is greater than 6μm, it is difficult to increase the elongation at break by increasing the thickness of the coating. Considering the cost of the material, the optimal value of the maximum thickness of the epoxy resin coating should be 6μm.
[0104] It can be seen from this that the optimal value of the thickness of the epoxy resin coating of the present invention is 2 to 6 μm.
[0105] In summary, whether based on the fracture resistance of the mica tape of the present invention (characterized by the tensile strength in Table 1) or the toughness of the mica tape (characterized by the elongation at break in Table 1), the optimal value of the thickness of the epoxy resin coating of the present invention should be 2 to 6 μm.
[0106] The technical means disclosed in the scheme of the present invention are not limited to the technical means disclosed in the above-mentioned implementation mode, but also include technical schemes composed of any combination of the above-mentioned technical features. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications are also regarded as the protection scope of the present invention.
Claims
1. A method for preparing a composite mica tape, characterized in that: The following steps are involved: S1. The first fiber reinforced layer and the second fiber reinforced layer are composited on both sides of the mica layer to obtain a mica skeleton structure; S2. performing a dip coating operation on the mica skeleton structure so that the surface of the first fiber reinforced layer, the surface of the second fiber reinforced layer, between the first fiber reinforced layer and the mica layer, and between the second fiber reinforced layer and the mica layer are coated with an epoxy resin coating; S3. Extruding the mica skeleton structure to squeeze out the excess epoxy resin coating so that the epoxy resin coating is evenly and densely coated on the surface of the first fiber reinforced layer and the surface of the second fiber reinforced layer; S4. performing a first drying operation on the mica skeleton structure to remove moisture from the epoxy resin coating so that the epoxy resin coating forms a continuous and dense epoxy resin coating to obtain a mica substrate semi-finished product; S5. The mica substrate semi-finished product is subjected to a micro-concave roller coating operation to form a continuous and uniform adhesive coating on the epoxy resin coating; S6. performing a second drying operation on the mica substrate semi-finished product to remove the organic solvent in the adhesive coating, wherein the thickness of the adhesive coating is 4 μm to 50 μm, and the thickness difference of the adhesive coating is less than 2 μm; In step S2, the mica skeleton structure is dip-coated by introducing the mica skeleton structure into an impregnation container filled with epoxy resin coating, so that the surface of the first fiber reinforced layer, the surface of the second fiber reinforced layer, the gap between the first fiber reinforced layer and the mica layer, and the gap between the second fiber reinforced layer and the mica layer are fully saturated and dipped with the epoxy resin coating; The epoxy resin coating is a water-based coating using water as a solvent, and the immersion temperature is controlled at 20° C. to 30° C. The viscosity of the epoxy resin coating under this temperature condition is 400 cps to 2000 cps, and the solid content is 30 wt% to 50 wt%; During the dip coating operation, the coating line speed is 40m / min to 60m / min, the residence time of the mica skeleton structure in the dipping container is 0.1s to 0.3s, and the walking time in the dipping container is increased by winding the roller; In step S5, the micro-concave roller coating operation on the mica substrate semi-finished product is specifically as follows: the mica substrate semi-finished product is introduced into a coating container filled with an adhesive, the adhesive is provided with a micro-concave roller, the mica substrate semi-finished product is brought into contact with the micro-concave roller, and the micro-concave roller is driven to rotate by pulling the mica substrate semi-finished product, so that the adhesive is continuously coated on the surface of the mica substrate semi-finished product; The solvent of the adhesive includes water, the coating temperature is controlled at 20°C to 30°C, the viscosity of the adhesive under this temperature condition is 400cps to 2000cps, and the solid content is 30wt% to 50wt%; The mica tape prepared according to the above preparation method has the following structure: A mica layer, a first fiber reinforced layer and a second fiber reinforced layer, wherein the first fiber reinforced layer and the second fiber reinforced layer are respectively arranged on both sides of the mica layer, and the mica layer is filled with epoxy resin; a first epoxy resin coating and a second epoxy resin coating, wherein the first epoxy resin coating is disposed between the first fiber reinforced layer and the mica layer and on the surface of the first fiber reinforced layer, and the second epoxy resin coating is disposed between the second fiber reinforced layer and the mica layer and on the surface of the second fiber reinforced layer, and the first epoxy resin coating and the second epoxy resin coating disposed on two surfaces of the mica layer are connected by epoxy resin filled in the mica layer; The thickness of the first epoxy resin coating layer and the second epoxy resin coating layer is 2 μm to 6 μm.
2. The method for preparing the composite mica tape according to claim 1, characterized in that: After step S6, step S8 is further provided, which is specifically: S8. Attach a release film to the surface of the adhesive coating to form a release layer, and then press the film to obtain a multi-layer composite mica tape.
3. A mica tape prepared according to the preparation method of claim 2, characterized in that: include: A mica layer, a first fiber reinforced layer and a second fiber reinforced layer, wherein the first fiber reinforced layer and the second fiber reinforced layer are respectively arranged on both sides of the mica layer, and the mica layer is filled with epoxy resin; a first epoxy resin coating and a second epoxy resin coating, wherein the first epoxy resin coating is disposed between the first fiber reinforced layer and the mica layer and on the surface of the first fiber reinforced layer, and the second epoxy resin coating is disposed between the second fiber reinforced layer and the mica layer and on the surface of the second fiber reinforced layer, and the first epoxy resin coating and the second epoxy resin coating disposed on two surfaces of the mica layer are connected by epoxy resin filled in the mica layer; An adhesive coating, wherein the adhesive coating is disposed on the surface of the first epoxy resin coating, the thickness of the adhesive coating is 4 μm to 50 μm, and the thickness difference of the adhesive coating is less than 2 μm; A release layer, the release layer is disposed on the surface of the adhesive coating; The thickness of the first epoxy resin coating layer and the second epoxy resin coating layer is 2 μm to 6 μm.
Citation Information
Patent Citations
Resin-impregnated plane paper and pressure-sensitive adhesive tape employing the same
CN101680183A
Production method for medical pressure-sensitive adhesive tape or sheet
CN102885672A
Mica tape manufacturing method suitable for energy conservation, emission reduction and reduction of environmental pollution
CN104409187A
Preparation of pressure-sensitive double-coated adhesive tape
JP1982115479A