A method for preparing a metallic transition metal chalcogenide film
By introducing VB group transition metal element doping into the two-dimensional semiconducting transition metal chalcogenide film, a stable two-dimensional metallic transition metal chalcogenide ternary alloy film is generated, which solves the material instability and problem in the existing technology. The problem of low preparation efficiency has been achieved, and large-scale, large-scale, high-efficiency controllable preparation has been achieved, improving device performance.
Patent Information
- Application Number
- CN202211404269.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-10
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-11-10
AI Technical Summary
Existing technology is difficult to achieve large-scale, large-scale, high-efficiency, and high-quality controllable preparation of two-dimensional metallic transition metal chalcogenide thin films, and the material instability and low preparation efficiency affect device performance.
By introducing VB group transition metal element doping during the CVD growth process of the two-dimensional semiconducting transition metal chalcogenide binary alloy film, the proportion is adjusted to generate a more stable two-dimensional metallic transition metal chalcogenide ternary alloy film, using VIB The high saturated vapor pressure of oxides of transition metal elements ensures sufficient source powder vapor, and a dual-temperature zone tube furnace is used for growth.
The controllable preparation of metallic transition metal chalcogen compound ternary alloy films in a large range, large size, high efficiency and high quality has been achieved. The material is more stable in the air, avoids contact problems and improves device performance.
Smart Images

Figure CN115652276B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a metallic transition metal chalcogenide compound film, belonging to the technical field of nano material preparation. Background Art
[0002] As we all know, semiconducting two-dimensional transition metal sulfide compounds represented by molybdenum disulfide (MoS2) (which can be represented by MX2, where M=W, Mo, belonging to the VIB group; X=S, Se, Te) as channel materials of field effect transistors can effectively avoid the "short channel effect", meet the requirements of small size and high integration of modern integrated circuits, and have broad application prospects in the post-Moore era. When preparing two-dimensional electronic devices based on two-dimensional transition metal sulfide compound semiconductor materials, the traditional thermal evaporation method is used to evaporate bulk metal electrodes, which usually forms a very high contact resistance at the interface, reducing device performance and severely limiting the application of the device. Studies have found that using two-dimensional metallic transition metal sulfide compound materials instead of metal bulk materials as electrodes can effectively reduce contact resistance and improve device performance. Therefore, the realization of large-area, large-size, high-efficiency, high-quality controllable preparation of two-dimensional metallic transition metal sulfide compound materials is of great significance to the application of two-dimensional electronic devices.
[0003] The two-dimensional metallic transition metal chalcogenides (MX2, where M = V, Nb, Ta, belonging to the VB group; X = S, Se, Te) materials mainly include niobium disulfide (NbS2), niobium diselenide (NbSe2), tantalum disulfide (TaS2), titanium diselenide (TiSe2), etc. The transition metal elements come from the VB group. People mainly use "top-down" mechanical or chemical exfoliation methods and "bottom-up" chemical synthesis methods to achieve the preparation of these materials. Among them, chemical vapor deposition (CVD) has more advantages in the controllable preparation of two-dimensional materials.
[0004] After investigating the existing technical literature, it was found that some two-dimensional metallic transition metal chalcogenide thin films have been successfully prepared by CVD. Professor Liu Zheng's research group at Nanyang Technological University, Singapore, reported on the 394th page of the 8th volume of Nature Communications in 2017 that niobium oxide (NbO x, x≤2.5) and selenium powder (Se) as precursors, sodium chloride (NaCl) as an auxiliary growth material, and niobium diselenide (NbSe2) thin films were synthesized by CVD. The partially oxidized niobium oxide they used was obtained by burning Nb powder in advance. The entire growth process has many steps and the operation is relatively complicated. In 2020, Liu Kai's research group at the School of Materials Science and Engineering at Tsinghua University reported in ACS Nano, Volume 14, 2020, pages 175-184, that NbS2 thin films were epitaxially grown on single-layer MoS2 using NbCl5 as a Nb source powder. NbS2 thin films are unstable in the air and are easily oxidized. Therefore, when used as electrodes to construct optoelectronic devices, it will affect the performance of the device and hinder the practical application of the device.
[0005] In the preparation process of metallic two-dimensional transition metal sulfide compound binary alloy thin films, oxides of VB group transition metals are usually used as transition metal source powders. These oxides have particularly high melting points and low saturated vapor pressures, which make the growth temperature of two-dimensional metallic transition metal sulfide compound binary alloy thin films high and the source powder vapor supply insufficient, resulting in uncontrollable single crystal shape of thin films and difficulty in achieving large-scale and large-size growth of thin films. In addition, when chlorides of transition metal elements are used as source powders, these chlorides are relatively active and are easily oxidized in the air to become metal oxides, which leads to the same growth problem. So far, the types of two-dimensional metallic transition metal sulfide compound binary alloy thin film materials successfully prepared by CVD are still very limited, and it is difficult to achieve large-scale and large-size high-quality growth. Moreover, during the transfer and device processing of such two-dimensional metallic transition metal sulfide compound binary alloy thin film materials in the air, a natural oxide layer several nanometers thick will quickly form on its surface, such as NbS2 is easily oxidized in the air to form NbS2-NbOx, which will also cause contact problems in device applications and reduce device performance. Furthermore, there are currently no reports on the controllable preparation of metallic two-dimensional transition metal chalcogenide ternary alloy films.
[0006] Therefore, it is of great practical significance to find two-dimensional metallic transition metal sulfide compound thin film materials that are stable, easy to synthesize, and can be prepared in a large area, large size, high efficiency, and high quality. Summary of the invention
[0007] [Technical issues]
[0008] In view of the difficulties that currently exist in the large-scale preparation of two-dimensional metallic transition metal sulfide binary alloy films, the purpose of the present invention is to provide a more stable and easy-to-prepare two-dimensional metallic transition metal sulfide compound, and to provide a method that can achieve large-area, large-size, high-efficiency, high-quality controllable preparation of such materials, thereby solving the problems of instability and low preparation efficiency of two-dimensional metallic transition metal sulfide compound films, and providing more choices for two-dimensional metal electrode materials.
[0009] In order to solve the existing problems of instability of two-dimensional metallic transition metal sulfide compound binary alloy thin films, and difficulty in large-scale, large-size, high-efficiency, high-quality controllable preparation, the present invention introduces VB group transition metal elements (such as V, Nb or Ta) doping during the CVD growth process of two-dimensional semiconductor transition metal sulfide compound binary alloy thin films, regulates the ratio between VB group and VIB group transition metal elements, generates a two-dimensional metallic transition metal sulfide compound ternary alloy thin film that is more stable in air, and provides a large-scale, large-size, high-efficiency, high-quality controllable preparation method of such two-dimensional metallic transition metal sulfide compound ternary alloy thin film material. This preparation method can effectively solve the problem of insufficient source powder vapor caused by low saturated vapor pressure of VB group transition metal oxide source powder in the preparation process of two-dimensional metallic binary alloy thin films, change binary film growth to ternary film growth, and use the characteristics of high saturated vapor pressure of VIB group transition metal element oxide to ensure sufficient source powder vapor in the growth process of metallic ternary alloy thin films, thereby realizing easy preparation of a metallic transition metal sulfide compound thin film material. This preparation method is simple and easy to operate, and like two-dimensional semiconductor transition metal sulfide binary alloy films, it is easier to achieve large-scale, large-size, high-efficiency, and high-quality controllable preparation, which can provide more material options for two-dimensional metal electrodes.
[0010] [Technical solution]
[0011] The first object of the present invention is to provide a method for preparing a metallic transition metal chalcogenide compound thin film, which comprises the following specific steps: a dual-temperature zone tubular furnace is selected as a growth device, a VIB group transition metal element source powder and a VB group transition metal element source powder are placed in the high temperature zone of the tubular furnace, and the molar ratio of the VIB group transition metal element to the VB group transition metal element in the two source powders is less than 1:2. Chalcogen element source powder is placed in the low temperature zone of the tubular furnace; a growth substrate is inverted on top of a ceramic boat containing a transition metal element (VB group or VIB group) source powder with a lower melting point, and is placed in the center of the high temperature zone with the ceramic boat.
[0012] In one embodiment of the present invention, the carrier gas of the tube furnace flows from the low temperature zone to the high temperature zone.
[0013] In one embodiment of the present invention, the source powders can be evaporated simultaneously and arrive at the surface of the growth substrate along with the carrier gas.
[0014] In one embodiment of the present invention, the Group VIB transition metal source powder includes one or more oxides, chlorides or other compounds containing Group VIB transition metal elements.
[0015] In one embodiment of the present invention, the Group VB transition metal source powder includes one or more oxides, chlorides or other compounds containing Group VIB transition metal elements of the Group VB transition metal elements.
[0016] In one embodiment of the present invention, the chalcogen source powder includes S source powder and Se source powder.
[0017] In one embodiment of the present invention, the high temperature zone where the growth substrate is located is raised to a preset growth temperature and maintained at that temperature until the film grows stably.
[0018] In one embodiment of the present invention, the preset growth temperature is 750-1100°C.
[0019] In one embodiment of the present invention, the carrier gas includes one or more of hydrogen, argon, and nitrogen.
[0020] In one embodiment of the present invention, the carrier gas is a mixed gas of hydrogen and argon or nitrogen.
[0021] In one embodiment of the present invention, the carrier gas flow rate is 50-100 sccm.
[0022] In one embodiment of the present invention, before the high temperature zone starts to heat up, the tubes of the tube furnace are first flushed with a carrier gas at a high speed; after the temperature starts to heat up, the flow rate of the carrier gas is kept constant.
[0023] In one embodiment of the present invention, the growth is performed by heating only the high temperature zone located downstream of the gas to allow the alloy film to grow.
[0024] In one embodiment of the present invention, the growth substrate includes a silicon wafer, quartz, sapphire or mica substrate with an oxide layer.
[0025] In one embodiment of the present invention, the growth substrate is placed upside down on top of a transition metal element source powder having a relatively high melting point.
[0026] In one embodiment of the present invention, the insulation time is 10-25 minutes.
[0027] In one embodiment of the present invention, the preparation method uses a dual-temperature zone tubular furnace as a chemical vapor deposition device for growth, and the tube in the reaction chamber of the tubular furnace is a ceramic tube with a diameter of 5 cm; MoO3 powder, Nb2O5 powder and S powder are selected as Mo source, Nb source and S source respectively, and these source powders are placed in a ceramic boat respectively, Nb2O5 powder is placed in the center of the high-temperature zone downstream of the air flow of the tubular furnace, MoO3 powder is placed upstream of the air flow, 10 cm away from the position where the Nb2O5 powder is located, and S powder is placed upstream of the air flow, 42 cm away from the position where the MoO3 powder is located; nitrogen containing 5% hydrogen is used as the carrier gas in the entire preparation process; before the temperature control program is started, the air in the tube is first flushed out using the flushing mode, and then the air flow rate is maintained at 50 sccm until the growth is completed and the tubular furnace naturally drops to room temperature to obtain a single layer of metallic Nb x Mo 1-x S2 ternary alloy film.
[0028] The present invention discloses a metallic transition metal sulfide compound film prepared by the method.
[0029] The second purpose of the present invention is to utilize the above-mentioned metallic transition metal chalcogenide compound film and apply it to the field of electronic device processing.
[0030] [Beneficial Effects]:
[0031] 1. Simple operation. The present invention is based on the existing relatively mature CVD method for preparing two-dimensional semiconductor transition metal sulfide binary alloy thin films. The distance between the source powders is adjusted according to the difference in the melting points of the various source powders selected, and their relative positions in the tube furnace are adjusted to ensure that they can evaporate simultaneously when the temperature in the high temperature zone of the tube furnace reaches the preset growth temperature, and then reach the growth substrate at the same time with the help of the carrier gas. During the growth process, only the high temperature zone located downstream of the gas is heated, and the source powder placed in other areas is heated by the thermal radiation of the high temperature zone. If the sulfide source powder is close to the high temperature zone, it will melt before the high temperature zone reaches the preset growth temperature, causing the transition metal source powder to be sulfided or selenized in advance, hindering the continued evaporation of these source powders, resulting in the alloy film not being able to grow successfully on the substrate, or not being able to form a large-size film; if the distance is too far, when the transition metal sulfide source powder has reached the growth substrate, the sulfide source powder has not evaporated, which will also cause the alloy film to fail to grow on the substrate, and the equipment requirements are low and easy to implement.
[0032] 2. High sample cleanliness. By adding a relatively low proportion of VB group transition metal elements, the obtained ternary alloy film can exhibit metallic properties. Therefore, there is no need to use NaCl as an auxiliary growth material to increase the amount of VB group transition metal element source powder vapor and avoid introducing unnecessary impurities.
[0033] 3. Large sample size. The side length of the triangular single crystal thin film sample can reach hundreds of microns, which is larger than the size of metallic transition metal chalcogenide film commonly reported in existing literature.
[0034] 4. Easy to achieve large-scale, high-efficiency and controllable preparation. It can avoid the shortcomings of difficult evaporation and high saturated vapor pressure of VB group transition metal element source powder in the preparation process of metallic transition metal chalcogenide binary alloy thin films, and easily achieve large-scale, high-efficiency and controllable preparation of metallic ternary alloy thin films.
[0035] 5. The sample is highly stable in the air. Compared with the same type of binary alloy film, the number of VB group transition metal atoms exposed on the surface of the prepared two-dimensional metallic transition metal chalcogenide ternary alloy film is greatly reduced. Therefore, it is more stable in the air and can be stored for a longer time. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 The two-dimensional metallic Nb grown on the silicon dioxide substrate in Example 1 x Mo 1-x Optical microscopy of S2 ternary alloy film
[0037] Figure 2 Example 1Nb x Mo 1-x Raman spectrum of S2 ternary alloy film
[0038] Figure 3 Example 1Nb x Mo 1-x Fluorescence (PL) spectrum of S2 ternary alloy film
[0039] Figure 4 Example 1Nb x Mo 1-x X-ray photoelectron spectroscopy (XPS) of S2 ternary alloy film
[0040] Figure 5 This is a light microscope image of the NbS2 binary alloy film of Example 4. DETAILED DESCRIPTION
[0041] The technical solution of the present invention is further described below in conjunction with the embodiments and drawings, but the present invention is by no means limited to the embodiments.
[0042] Example 1
[0043] Growth substrate treatment: The silicon dioxide / silicon (SiO2 / Si) substrate was ultrasonically treated with acetone, anhydrous ethanol, and deionized water in sequence for 10 minutes each, and finally dried with high-purity nitrogen for later use.
[0044] Growth control: A dual-temperature zone tubular furnace is used as a chemical vapor deposition equipment for growth. The tube in the reaction chamber of the tubular furnace is a ceramic tube with a diameter of 5 cm. MoO3 powder (3 mg), Nb2O5 powder (10 mg) and S powder (30 mg) are selected as Mo source, Nb source and S source respectively. These source powders are placed in a ceramic boat respectively. Nb2O5 powder is placed in the center of the high-temperature zone downstream of the airflow of the tubular furnace, and MoO3 powder is placed upstream of the airflow, 10 cm away from the position where the Nb2O5 powder is located. S powder is placed upstream of the airflow, 42 cm away from the position where the MoO3 powder is located. Nitrogen containing 5% hydrogen is used as the carrier gas in the entire preparation process. Before the temperature control program is started, the air in the tube is flushed out using the flushing mode, and then the airflow rate is maintained at 50 sccm until the growth is completed and the tubular furnace naturally drops to room temperature.
[0045] During the entire growth process, only the temperature zone where the Nb2O5 powder is located is activated. First, the high temperature zone of the tube furnace is raised from room temperature to 850°C, and then kept warm for 10 minutes. After that, the temperature control program ends and the tube furnace is naturally cooled to room temperature.
[0046] Through the above growth process, a large-scale, large-area uniform single-layer metallic Nb x Mo 1-x S2 ternary alloy film.
[0047] Figure 1 The optical microscope image of the prepared sample is shown. From the image, it can be seen that the optical contrast of the film is very uniform, indicating that the number of layers is uniform. The samples are mostly triangular and single crystals, and their maximum size can reach 200μm.
[0048] Figure 2 The Raman spectrum of the prepared sample is shown. It can be seen from the figure that Nb x Mo 1-x The main Raman peaks of S2 ternary alloy film are located at 186.3 cm -1 , 224.4cm -1 , 301.4cm -1 , 350.1, 382.8cm -1 , 403.3cm -1 , with characteristic peaks of both MoS2 and NbS2, indicating that the prepared sample is Nb x Mo 1-x S2 alloy film.
[0049] Figure 3 The prepared Nb x Mo 1-xFluorescence emission spectrum of S2 (x = 0.2) alloy film sample. As can be seen from the figure, when X = 0.2, the sample has no fluorescence signal, combined with theoretical calculations, indicating that the sample is metallic.
[0050] Figure 4 The XPS graph of the obtained sample is shown. It can be seen from the figure that the sample contains Nb, Mo and S elements, which is consistent with Nb x Mo 1-x Characteristics of S2 ternary alloy films.
[0051] Example 2 refers to Example 1, but the amount of Nb2O5 powder in the growth control step is changed to 1 mg, and the other conditions remain unchanged, but the obtained film does not have metallic properties.
[0052] Example 3 refers to Example 1, changing the temperature control temperature from 850°C to 950°C, and keeping the other conditions unchanged.
[0053] Example 4 Referring to Example 1, the amount of MoO3 powder in the growth control step was changed to 0 mg, and the other conditions remained unchanged. The obtained NbS2 film had an irregular shape and could not achieve large-scale growth on the substrate. Figure 5 An optical microscope image of the obtained NbS2 sample is shown.
Claims
1. A method for preparing a metallic transition metal chalcogenide thin film, characterized in that: The specific steps are as follows: a dual-temperature zone tubular furnace is selected as the growth equipment for growth, the tube in the reaction chamber of the tubular furnace is a ceramic tube with a diameter of 5 cm, 3 mg of MoO3 powder, 10 mg of Nb2O5 powder and 30 mg of S powder are selected as the Mo source, Nb source and S source respectively, and these source powders are placed in a ceramic boat respectively, the Nb2O5 powder is placed in the center of the high-temperature zone downstream of the air flow of the tubular furnace, the MoO3 powder is placed upstream of the air flow, 10 cm away from the position where the Nb2O5 powder is located, and the S powder is placed upstream of the air flow, 42 cm away from the position where the MoO3 powder is located, and nitrogen containing 5% hydrogen is used as the carrier gas throughout the preparation process. Before the temperature control program is started, the air in the tube is first flushed out using the flushing mode, and then the air flow rate is maintained at 50 sccm until the tubular furnace naturally cools to room temperature after the growth is completed; The carrier gas of the tube furnace flows from the low temperature zone to the high temperature zone.
2. The method according to claim 1, characterized in that The growth substrate is inverted on top of the ceramic boat and placed in the center of the high-temperature zone with the ceramic boat. The high-temperature zone where the growth substrate is located is raised to a preset growth temperature and kept warm until the film grows stably; the preset growth temperature is 750-1100°C.
3. The method according to claim 1, characterized in that The carrier gas includes one or more of hydrogen, argon, and nitrogen.
4. The method according to claim 2, characterized in that The growth substrate includes a silicon wafer with an oxide layer, a quartz, a sapphire or a mica substrate.
5. A metallic transition metal chalcogenide thin film prepared by the method according to any one of claims 1 to 4.
6. Use of the metallic transition metal chalcogenide compound thin film according to claim 5 in the field of electronic device processing.