Hot press parts
By adding specific corrosion resistance elements to the base material of the aluminum-plated steel plate and controlling its concentration distribution, the problem of insufficient corrosion resistance after coating of hot-pressed parts is solved, and efficient corrosion resistance and coating adhesion are achieved. Suitable for automotive parts.
Patent Information
- Application Number
- CN202180037187.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-08-20
- Filing Date
- 2021-08-20
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-08-20
AI Technical Summary
The existing hot-pressed parts have insufficient corrosion resistance after coating, especially the high-demand level is difficult to meet, and the relationship between corrosion resistance and adhesion after coating is unclear.
By adding corrosion resistance to the base material of the aluminum-plated steel plate, such as W, Mo, Sb, Sn, Cr, Co, Cu, Ni, Ta, Ca, Mg, Sr, Re, Hf, etc., it controls its in Al -The concentration distribution in the Fe alloy coating makes it form a solid corrosion product during the hot pressing process, improving corrosion resistance after coating.
It achieves a significant improvement in corrosion resistance and coating adhesion after coating, and maintains excellent performance even when exposed to corrosion for a long time, and is suitable for automotive parts.
Smart Images

Figure BDA0003956395920000281 
Figure BDA0003956395920000291 
Figure BDA0003956395920000301
Abstract
Description
Technical Field
[0001] The present invention relates to heat pressed parts.
[0002] This application claims priority based on patent application No. 2020-139257 filed in Japan on August 20, 2020, the contents of which are incorporated herein by reference. Background Art
[0003] In recent years, the demand for suppressing the consumption of chemical fuels has increased in order to protect the environment and prevent global warming, and this demand has had an impact on various manufacturing industries. For example, automobiles, which are indispensable as a means of transportation in daily life and activities, are no exception, and there is a demand to improve fuel economy by making the car body lighter, etc. However, for automobiles, simply making the car body lighter may lead to a decrease in safety, so it is not allowed in terms of product quality. Therefore, when making the car body lighter, it is necessary to ensure appropriate safety.
[0004] Many structures of automobiles are formed by iron, especially steel plates, and reducing the weight of steel plates is important for lightweighting the vehicle body. In addition, such requirements for steel plates exist not only in the automobile manufacturing industry, but also in various manufacturing industries. In response to such requirements, if the weight of the steel plates is simply reduced, it is conceivable to reduce the thickness of the steel plates. However, reducing the thickness of the steel plates will lead to a decrease in the strength of the structure, which is not satisfactory. Therefore, in recent years, research and development has been conducted on steel plates that can maintain or improve the mechanical strength of structures composed of steel plates even if they are thinner than the steel plates used before by improving the mechanical strength of the steel plates.
[0005] Generally, steel plates with high mechanical strength tend to have reduced shape freezeability during forming processes such as bending. Therefore, when processing into a complex shape, the processing itself becomes difficult. As one of the means to solve the problem of formability, the so-called "hot pressing method (sometimes also called hot die pressing method, hot stamping method, high temperature pressing method, die quenching method)" can be cited. In this hot pressing method, the material to be formed is heated to a high temperature, and the steel plate softened by heating is pressed to form it, and cooled during or after forming. According to this hot pressing method, since the material is temporarily heated to a high temperature to soften it, it can be easily pressed. In addition, the mechanical strength of the material can be improved by the quenching effect brought about by cooling during or after forming. Therefore, this hot pressing method can be used to obtain a formed product with good shape freezeability and high mechanical strength.
[0006] However, when the hot pressing method is applied to steel plates, in components that require corrosion resistance (e.g., corrosion resistance after painting), it is necessary to perform rust prevention treatment and metal coating on the component surface after processing. Therefore, it is necessary to perform surface cleaning and surface treatment steps on the component, which reduces productivity.
[0007] To address such a problem, Patent Document 1 describes an aluminum-plated steel sheet for hot pressing, wherein an Al-based metal coating layer mainly composed of Al and containing Mg and Si is provided on the surface of steel.
[0008] Patent Document 2 specifies the composition of the surface of a hot-pressed steel sheet and states that the amount of AlN on the surface of the Al-Fe alloy layer on the surface of the steel is 0.01 to 1 g / m 2 .
[0009] Patent Document 3 describes an automobile component having an Al-Fe intermetallic compound layer on the surface of a steel plate, an oxide film on the surface of the Al-Fe intermetallic compound layer, a bcc layer between the steel plate and the Al-Fe intermetallic compound layer, and the bcc layer having Al; and describes the oxide film thickness on the surface of the Al-Fe alloy layer after hot pressing. Patent Document 3 describes that the Al-Fe alloy layer is formed up to the surface layer by heating the aluminum-plated steel plate in such a manner that the oxide film has a predetermined thickness, and that coating defects and a decrease in adhesion after electrodeposition coating are suppressed, thereby ensuring corrosion resistance after coating.
[0010] However, in recent years, the level of corrosion resistance required after painting has become higher, and the aluminum-plated steel sheet for hot pressing described in Patent Document 1 may not necessarily have sufficient corrosion resistance after painting for such high requirements. In addition, the aluminum-plated steel sheet for hot pressing described in Patent Document 1 does not specify the composition and structure of the outermost surface, and the relationship between the composition and structure of the outermost surface and the corrosion resistance after painting is not clear.
[0011] In Patent Document 2, by setting the amount of AlN on the surface of the Al—Fe alloy layer to a predetermined range, a certain degree of improvement in corrosion resistance after coating is observed, but there is room for further improvement.
[0012] In addition, even if the structure and thickness of the Al-Fe alloy layer are controlled as described in Patent Document 3, the corrosion resistance after coating may not be sufficient for the high level required in recent years. The reason may be that the reactivity between the oxide film and the chemical conversion agent is reduced, resulting in a decrease in the amount of chemical conversion agent attached.
[0013] Prior Art Literature
[0014] Patent Literature
[0015] Patent Document 1: Japanese Patent Application Publication No. 2003-034845
[0016] Patent Document 2: Japanese Patent Application Publication No. 2011-137210
[0017] Patent Document 3: Japanese Patent Application Publication No. 2009-293078 Summary of the invention
[0018] As described above, the conventional technology has a problem that the corrosion resistance of hot-pressed parts after painting cannot be sufficiently ensured. The present invention has been made in view of such a problem, and an object thereof is to provide a hot-pressed part having excellent plating adhesion and corrosion resistance after painting.
[0019] The inventors of the present invention have studied a method for improving the corrosion resistance of hot-pressed parts after painting, based on a manufacturing method in which the surface of the component is not subjected to rust prevention treatment or metal coating after processing. As a result, it was found that by making the base material of the aluminum-plated steel plate provided for hot pressing contain a corrosion resistance-improving element, and diffusing the corrosion resistance-improving element so that it has a predetermined concentration distribution in the Al-Fe alloy coating formed by heating during hot pressing, the Al-Fe alloy coating becomes less soluble than before with respect to corrosion factors such as salt water, or after the Al-Fe alloy coating is partially dissolved, a strong and dense corrosion product is generated on the surface of the Al-Fe alloy coating, and as a result, a hot-pressed part with excellent corrosion resistance after painting can be manufactured.
[0020] In addition, the following insight was obtained: in order to control the corrosion resistance improving elements so that they have a specified concentration distribution in the Al-Fe alloy plating, it is important to concentrate specific elements on the surface of the cold-rolled steel sheet until the plating is completed by appropriately controlling the manufacturing conditions in the hot rolling process and the hot pressing process for manufacturing the base material, and to perform hot pressing in this state.
[0021] The gist of the present invention completed based on the above findings is as follows.
[0022] (1) A hot-pressed component according to one embodiment of the present invention is a hot-pressed component having a base steel plate and an Al-Fe alloy plating layer formed on the base steel plate, wherein the Al-Fe alloy plating layer has a thickness of 10.0 μm or more and contains, by mass%, 30% or more of Al and one or more selected from the group consisting of W, Mo, Sb, Sn, Cr, Co, Cu, Ni, Ta, Ca, Mg, Sr, Se, Re, and Hf as corrosion resistance improving elements, wherein the element having the largest concentration among the corrosion resistance improving elements in a range from the surface of the Al-Fe alloy plating layer to 8.0 μm in the direction of the center of the plate thickness of the hot-pressed component is set to a B1 element, and the maximum concentration of the B1 element is set to a C max, the plate thickness of the hot press component is t, and the position t / 4 from the surface of the hot press component toward the center of the plate thickness is t Q , the t Q The concentration of the B1 element at the position is set to C Q In the case of C max / C Q It is 0.05 or more and 30.00 or less.
[0023] (2) According to the hot-pressed component described in (1) above, the Al—Fe alloy plating layer may be composed of one or more intermetallic compounds.
[0024] (3) According to the hot pressed component described in (1) or (2), the base steel plate may have the following chemical composition: in terms of mass%, it contains C: 0.03-0.60%, Si: 0.005-2.00%, Mn: 0.10-3.00%, P: 0.001-0.100%, S: 0.0001-0.100%, Al: 0.010-0.500% and N: 0.001-0.010%, and W: 0.01-3.00%, Mo: 0.005-2.00%, Sb: 0.005-0.30%, Sn: 0.0 05~0.50%, Cr: 0.005~2.00%, Co: 0.01~2.00%, Cu: 0.01~2.00%, Ni: 0.01~2.00%, Ta: 0.0001~0.300%, Ca: 0.0001~0.300%, Mg: 0.0001~0.300%, Sr: 0.0001~0.300%, Se: 0.0001~0.300%, Re: 0.0001~0.300% and Hf: 0.0001~0.300%, and the balance contains Fe and impurities.
[0025] (4) According to the hot pressed part described in (3) above, the chemical composition of the base steel plate may also contain, in terms of mass%, one or more selected from the group consisting of B: 0.0002-0.0100%, V: 0.005-0.500%, Ti: 0.005-0.500%, Nb: 0.010-0.500%, Zr: 0.005-0.500%, O: 0.0001-0.0070% and REM: 0.0001-0.3000%.
[0026] (5) In the hot-pressed part described in any one of (1) to (4) above, when the concentration of the B1 element at a position 2.0 μm from the surface of the Al-Fe alloy coating toward the center of the plate thickness is set to C2, and the concentration of the B1 element at a position 8.0 μm from the surface toward the center of the plate thickness is set to C8, C2 / C8 is greater than 1.1 and less than 4.0.
[0027] According to the above aspect of the present invention, it is possible to provide a hot-pressed component having excellent plating adhesion and corrosion resistance after painting even when exposed to a corrosive environment for a long period of time.
[0028] The hot-pressed component is suitable as an automobile component. DETAILED DESCRIPTION
[0029] Hereinafter, a hot press component according to a preferred embodiment of the present invention (hot press component according to this embodiment) will be described in detail. First, the reasons for limiting the hot press component according to this embodiment will be described.
[0030] In the numerical ranges described below with "to" between them, the lower limit and the upper limit are included in the range. However, if a numerical value is expressed as "less than" or "exceeds", the value is not included in the numerical range.
[0031] <Hot-pressed parts>
[0032] The hot-pressed component according to the present embodiment includes a base steel plate and an Al—Fe alloy plating layer formed on the base steel plate.
[0033] (About Al-Fe alloy plating)
[0034] The Al—Fe alloy plating layer, which is the most important layer in the hot-pressed component according to the present embodiment, will be described in detail.
[0035] The thickness of the Al-Fe alloy coating layer of the hot-pressed component according to the present embodiment is 10.0 μm or more. When the thickness of the Al-Fe alloy coating layer is less than 10.0 μm, the corrosion resistance after coating is reduced. The thickness of the Al-Fe alloy coating layer is preferably 15.0 μm or more, and more preferably 20.0 μm or more.
[0036] On the other hand, the upper limit of the thickness of the Al-Fe alloy coating is not limited, but when the thickness exceeds 60.0 μm, the coating is thick, so the shear force received by the coating from the mold during hot press forming and the stress during compression deformation become larger. In this case, the coating is easy to peel off, and there is a concern that the corrosion resistance will decrease after coating. Therefore, the thickness of the Al-Fe alloy coating is preferably 60.0 μm or less. More preferably, it is 55.0 μm or less, and more preferably, it is 50.0 μm or less.
[0037] In addition, the Al-Fe alloy plating layer of the hot-pressed part according to the present embodiment contains Al, Fe and one or more selected from "W, Mo, Sb, Sn, Cr, Co, Cu, Ni, Ta, Ca, Mg, Sr, Se, Re, Hf" (B group elements) as corrosion resistance improving elements. Furthermore, it may also contain elements such as Si, Mn, and B. It may also contain Li and Zn.
[0038] In addition, the Al content in the Al-Fe alloy plating layer is 30% by mass or more. The total content of Al and Fe is preferably 80% by mass or more. The corrosion resistance improving element is preferably 0.005% to 8.0% in total content (mass %). More preferably, it is more than 0.005% and less than 8.0%, and further preferably 0.010% to 8.0%.
[0039] The Al—Fe alloy plating layer of the hot-pressed component according to the present embodiment preferably contains one or more intermetallic compounds, and more preferably consists essentially of one or more intermetallic compounds and inevitably contained impurities.
[0040] Specific intermetallic compounds constituting the Al-Fe alloy plating layer include, for example, Fe2Al5, FeAl2, FeAl (also called regular BCC), α-Fe (also called irregular BCC), Al solid solution α-Fe, substances obtained by solid solution of Si in these compositions, and Al-Fe-Si ternary alloy compositions whose detailed stoichiometric compositions cannot sometimes be determined (12 types, τ1 to τ12, are determined, in particular τ5 is also called α phase, and τ6 is also called β phase).
[0041] Examples of impurities contained in the Al—Fe alloy plating layer include components of stainless steel and ceramics generally used as hot-dip plating equipment during hot-dip plating, and thermal sprayed films on these materials.
[0042] The corrosion resistance improving elements (B group elements) exist in the intermetallic compound in the form of solid solution or substitution.
[0043] The reason why the corrosion resistance improving element (B group element) contained in the base material before hot pressing is contained in the Al-Fe alloy coating after hot pressing is not necessarily clear, but it is presumed that it diffuses in the solid phase at the grain boundary of the above-mentioned alloy coating or diffuses into the Al-Fe alloy coating or the outermost surface of the Al-Fe alloy coating by seeking thermodynamic stability through the liquid phase. The results of the inventor's research also show that even if the same degree of B group element is added to the plating bath instead of containing the B group element in the base material, the existence state of the hot pressed part and the B group element involved in the present embodiment is not necessarily the same.
[0044] The Al-Fe alloy coating can be confirmed to contain the above-mentioned intermetallic compound by using the restricted field electron beam diffraction function and EDS function of a transmission electron microscope (Field Emission-Transmission Electron Microscopy: FE-TEM). Specifically, after processing the cross section of the hot-pressed part along the plate thickness direction so that the sample becomes a thickness of about 100nm, in the range from the surface to the center of the plate thickness until 8.0μm, when the diffraction image of the above-mentioned compound is detected, it can be judged that the intermetallic compound is present at its location. Even if the diffraction image derived from the crystal is not measured in the above-mentioned measurement, the compound can be determined according to the ratio of each element by using the EDS function for analysis at the same location. In addition, 5 locations are randomly measured according to the above-mentioned essentials. In the case where the intermetallic compound exists at any location, in the present embodiment, it is judged that the Al-Fe alloy coating is substantially composed of one or more intermetallic compounds.
[0045] Furthermore, in a range (thickness) from the surface of the Al-Fe alloy plating layer having a large influence on the corrosion resistance after coating to the center of the plate thickness of the hot-pressed part up to 8.0 μm, the element with the highest maximum concentration among the corrosion resistance improving elements (B group elements) in the Al-Fe alloy plating layer is defined as the B1 element, and the maximum concentration of the B1 element in the above range is defined as the C max (%), the plate thickness of the hot press part is t, and the position t / 4 from the surface of the hot press part toward the center of the plate thickness is t Q , t Q The concentration (content) of the B1 element (the corrosion resistance improving element with the highest concentration in the range of 8 μm from the surface) at the position of C Q (%), by max / C Q When the ratio is 0.05 or more and 30.00 or less, the corrosion resistance after painting is improved.
[0046] The reason for this is still unclear, but it is presumed that the corrosion resistance improving element (B group element) C in the Al-Fe alloy plating layer max / C QWhen the ratio is 0.05 or more, the corrosion resistance improving element (B group element) becomes relatively stable against corrosion, and the dissolution rate of the Al-Fe alloy plating in the corrosive environment is reduced. It is also believed that this is because the corrosion resistance improving element (B group element) dissolved from the Al-Fe alloy plating can inhibit the further dissolution of the Al-Fe alloy plating, and the dissolved corrosion resistance improving element (B group element) stabilizes the corrosion product (rust) formed by combining with the hydroxide ions and chloride ions in the corrosive environment.
[0047] On the other hand, in C max / C Q When it exceeds 30.00, the reactivity of the surface with respect to the chemical conversion treatment liquid and the treatment liquid for the electrodeposition coating is reduced, so that the electrodeposition coating is easily peeled off during the corrosion test, and the corrosion resistance after coating is reduced.
[0048] In addition, by making C max / C Q When the ratio is 0.05 or more, the adhesion of the coating is also improved. Although the reason is not yet clear, it is believed that the electrical deviation, i.e., the polarity of the Al-Fe alloy coating is changed by the corrosion resistance improving elements (B group elements), thereby strengthening the physical and chemical bonding and improving the resistance to peeling.
[0049] As the corrosion resistance improving element serving as the B1 element (the element having the highest maximum concentration in the range of 8.0 μm from the surface toward the center of the plate thickness), W, Sn, and Cu are preferred because of excellent coating adhesion (secondary adhesion).
[0050] C of elements (B group elements) that improve the corrosion resistance of hot pressed parts max and C Q The analysis is done using the following method.
[0051] The sample is cut out from any position of the hot-pressed part that is 50 mm or more from the end face (the end face of the steel plate in the width direction and rolling direction as the raw material) (if it is not possible to produce from this position, it is a position avoiding the end face) so that a cross section (plate thickness cross section) perpendicular to the surface can be observed. The size of the sample depends on the measuring device, but it is set to a size that can observe about 10 mm in the rolling direction.
[0052] The above sample was embedded in a resin and polished. Then, the layer structure of the plate thickness cross section was measured by point analysis at 17 locations (surface, 0.5 μm from the surface, 1.0 μm from the surface, ..., 8.0 μm from the surface) in a linear manner at intervals of 0.5 μm in a range from the surface (the surface of the Al-Fe alloy plating layer) to 8.0 μm in the plate thickness direction. The maximum concentration of the element (B1 element) having the largest maximum concentration among the above-mentioned corrosion resistance improving elements (B group elements) at the location where the total of the Al concentration (Al content) and the Fe concentration (Fe content) was 80% or more was set as C. max In addition, the average Al concentration among the above 17 points was defined as the Al concentration in the Al-Fe alloy plating layer.
[0053] In addition, C Q The following method was used for determination.
[0054] The above sample was used. At a position t that was 1 / 4 of the plate thickness t from the surface toward the center of the plate thickness (position t / 4), Q The concentration of the B group elements (particularly the B1 element) was determined by point analysis using EPMA.
[0055] The thickness of the Al-Fe alloy plating layer was measured by the following method.
[0056] A sample was prepared in such a way that the thickness direction of the coating could be observed. The sample was embedded in resin and polished. The Al concentration and Fe concentration were measured from the surface of the component to the center of the plate thickness by point analysis using EPMA. Q The plate thickness position within the range of 0.9 to 1.1 times the Al concentration is judged as the interface between the steel plate and the coating, and the distance between the interface and the component surface in the secondary electron image or reflected electron image of EPMA can be taken as the thickness of the Al—Fe alloy coating.
[0057] In order to ensure corrosion resistance as a hot-pressed component, it is preferred that the Al-Fe alloy plating layer covers 90% or more of the surface in terms of area ratio (coverage is 90% or more).
[0058] (About oxide layer)
[0059] In the hot-pressed part involved in the present embodiment, from the viewpoint of improving coating adhesion (secondary adhesion), it is preferred that the surface of the Al-Fe alloy plating layer also has an oxide layer composed of Al oxide and Mg and / or Ca oxide and having a thickness of 0.05 μm to 3.0 μm. By forming an oxide layer containing Mg and / or Ca oxides on the surface of the Al-Fe alloy plating layer, the formation of a chemical conversion film can be promoted, thereby improving coating adhesion. The oxide of Mg may also be a composite oxide of Mg and Al, and the oxide of Ca may also be a composite oxide of Ca and Al.
[0060] When the thickness of the oxide layer is less than 0.05 μm, the above-mentioned effect cannot be obtained, and when the thickness of the oxide layer exceeds 3.00 μm, the adhesion of the oxide layer decreases, which may cause peeling of the electrodeposition coating film formed later, which is not preferable.
[0061] The oxide layer containing oxides of Mg and / or Ca referred to herein is a layer containing Mg and Ca in a total amount of 2 mass % or more.
[0062] As a method for determining the thickness and composition of the oxide layer containing oxides of Mg and / or Ca, the following method can be listed in the same manner as the above-mentioned method: after cross-section grinding of the coating, the cross-section obtained is observed using EPMA without performing corrosion, and elemental analysis is continuously performed linearly perpendicular to the surface, and the thickness (distance from the surface) of the region where the total amount of Mg and / or Ca is 2 mass% or more is determined.
[0063] Regarding the hot-pressed parts involved in this embodiment, the base material and the Al-Fe alloy plating are the same as described above. When the hot-pressed parts are used as automotive parts, they will be subjected to various treatments such as welding, chemical conversion treatment, and electrodeposition coating to become the final product.
[0064] (About base steel plate)
[0065] The hot-pressed component according to the present embodiment has a great feature in terms of the Al-Fe alloy plating layer, and is not necessarily limited to the base steel plate. However, the base steel plate preferably has a chemical composition that contains, by mass%, C: 0.03-0.60%, Si: 0.005-2.00%, Mn: 0.10-3.00%, P: 0.001-0.100%, S: 0.0001-0.100%, Al: 0.010-0.50%, N: 0.001-0.010%, and one or more selected from corrosion resistance improving elements (B group elements: W, Mo, Sb, Sn, Cr, Co, Cu, Ni, Ta, Ca, Mg, Sr, Se, Re, Hf), and the balance contains Fe and impurities.
[0066] Hereinafter, the preferred range of each element of the base steel plate of the hot-pressed component and the reasons thereof will be described in detail. All % in chemical composition indicates mass %.
[0067] C: 0.03~0.60%
[0068] C is an element that has a great influence on the strength of the hot-pressed steel sheet (hot-pressed component) after hot pressing. If the C content is low, the strength of the hot-pressed component decreases, and the energy absorption during collision decreases. Therefore, the C content is preferably set to 0.03% or more. The C content is more preferably 0.04% or more.
[0069] On the other hand, if the C content is high, the strength of the hot-pressed part is too high, and cracks may occur during deformation during collision. Therefore, the C content is preferably 0.60% or less. The C content is more preferably 0.40% or less, or 0.35% or less.
[0070] Si: 0.005~2.00%
[0071] Si is a solid solution strengthening alloy element and is an element required to ensure the strength of hot pressed parts. This effect cannot be achieved when the Si content is significantly low, so the Si content is preferably set to 0.005% or more. The Si content is more preferably 0.01% or more, 0.02% or more.
[0072] On the other hand, if the Si content exceeds 2.00%, the problem of surface scale will occur. That is, after the scale generated during hot rolling is pickled, a pattern caused by surface unevenness is generated, and the surface appearance becomes inferior. In addition, when the steel sheet surface is plated, the plating property deteriorates if the Si content is high. Therefore, the Si content is preferably set to 2.00% or less. The Si content is more preferably 1.50% or less, 1.00% or less, or 0.60% or less.
[0073] Mn: 0.10~3.00%
[0074] Mn is an element that improves the hardenability of steel and the strength of hot-pressed parts. When the Mn content is less than 0.10%, the hot-pressed parts cannot obtain sufficient strength. Therefore, the Mn content is preferably set to 0.10% or more. The Mn content is more preferably 0.20% or more, 0.40% or more, 0.70% or more, or 1.00% or more.
[0075] On the other hand, even if the Mn content exceeds 3.00%, the above effect is saturated. Therefore, the Mn content is preferably 3.00% or less. The Mn content is more preferably 2.80% or less, or 2.60% or less.
[0076] P: 0.001~0.100%
[0077] P is a solid solution strengthening alloy element and is an element useful for improving the strength of hot pressed parts. Therefore, the P content is preferably set to 0.001% or more.
[0078] On the other hand, if the P content exceeds 0.100%, welding crack resistance and toughness are adversely affected. Therefore, the P content is preferably 0.100% or less. The P content is more preferably 0.020% or less.
[0079] S: 0.0001~0.100%
[0080] S is an element that affects non-metallic inclusions in steel and deteriorates the ductility of hot-pressed steel sheets. Therefore, the S content is preferably limited to 0.100% or less. The S content is more preferably 0.080% or less, 0.050% or less, 0.008% or less, or 0.005% or less.
[0081] On the other hand, if the S content is excessively reduced, the production cost of the desulfurization step increases. Therefore, the S content is preferably set to 0.0001% or more, and more preferably 0.001% or more.
[0082] Al: 0.010~0.500%
[0083] Al is an element used as a deoxidizing material for molten steel. In order to sufficiently deoxidize the molten steel, the Al content is preferably 0.010% or more. The Al content is more preferably 0.020% or more, or 0.030% or more.
[0084] On the other hand, if the Al content exceeds 0.500%, a large number of non-metallic inclusions are formed, and surface flaws are easily generated in the product. Therefore, the Al content is preferably set to 0.500% or less. The Al content is more preferably 0.100% or less, or 0.060% or less.
[0085] N: 0.001~0.010%
[0086] N is an element contained in steel as an impurity. If the N content exceeds 0.010%, the ductility of the hot-pressed steel sheet may deteriorate due to the coarsening of nitrides. Therefore, the N content is preferably limited to 0.010% or less. The N content is more preferably 0.008% or less, or 0.006% or less.
[0087] On the other hand, if the N content is excessively reduced, the production cost of the steelmaking process increases. Therefore, the N content is preferably set to 0.001% or more.
[0088] Elements that improve corrosion resistance (Group B elements)
[0089] Hereinafter, W, Mo, Sb, Sn, Cr, Co, Cu, Ni, Ta, Ca, Mg, Sr, Se, Re, and Hf as corrosion resistance improving elements (B group elements) are described in detail. The corrosion resistance improving elements (B group elements) preferably contain one or more of them in the range shown below, but the total content of the B group elements is preferably set to 10.00% or less. In the case where the total content of the B group elements exceeds 10.00%, the alloy cost increases, so it is economically disadvantageous. Regarding the B group elements, if one or more of them are contained in the range shown below, the elements other than them may also be 0% or less than the lower limit shown below.
[0090] W: 0.01~3.00%
[0091] W is an element effective in improving the corrosion resistance of hot-pressed parts. To achieve this effect, the W content is preferably 0.01% or more. More preferably, the W content is 0.015% or more, 0.03% or more, 0.045% or more, or 0.06% or more.
[0092] On the other hand, when the W content exceeds 3.00%, castability may be reduced. Therefore, the W content is preferably 3.00% or less. The W content is more preferably 2.00% or less and 1.50% or less.
[0093] Mo: 0.005~2.00%
[0094] Mo is an element that improves the corrosion resistance and hardenability of steel, and is also an element that has the effect of increasing the strength of hot-pressed parts. In order to reliably exert this effect, the Mo content is preferably set to 0.005% or more. The Mo content is more preferably 0.01% or more.
[0095] On the other hand, when the Mo content exceeds 2.00%, carbides present after hot rolling, cold rolling or annealing (including after plating treatment) are stabilized, dissolution of carbides during heating during hot pressing is delayed, and hardenability may be reduced. Therefore, the Mo content is preferably set to 2.00% or less.
[0096] Sb: 0.005~0.30%
[0097] Sb is an element effective in improving the corrosion resistance of hot-pressed parts. In order to obtain this effect, the Sb content is preferably set to 0.005% or more. The Sb content is more preferably 0.01% or more, 0.03% or more, 0.04% or more, or 0.06% or more.
[0098] On the other hand, even if the Sb content exceeds 0.30%, the above-mentioned effect is saturated. Therefore, the Sb content is preferably set to 0.30% or less. The Sb content is more preferably set to 0.22% or less.
[0099] Sn: 0.005~0.50%
[0100] Sn is an element effective in improving the corrosion resistance of hot-pressed parts. To achieve this effect, the Sn content is preferably set to 0.005% or more. The Sn content is more preferably 0.01% or more, 0.03% or more, 0.04% or more, or 0.06% or more.
[0101] On the other hand, even if the Sn content exceeds 0.50%, the above-mentioned effect is saturated. Therefore, the Sn content is preferably 0.50% or less. The Sn content is more preferably 0.18% or less, or 0.16% or less.
[0102] Cr: 0.005~2.00%
[0103] Cr is an element effective in improving the hardenability and corrosion resistance of steel. In order to reliably exert this effect, the Cr content is preferably set to 0.005% or more. The Cr content is more preferably set to 0.01% or more.
[0104] On the other hand, if the Cr content exceeds 2.00%, carbides present after hot rolling, cold rolling or annealing (including after plating treatment) are stabilized, dissolution of carbides during heating during hot pressing is delayed, and hardenability may be reduced. Therefore, the Cr content is preferably set to 2.00% or less.
[0105] Co: 0.01~2.00%
[0106] Co is an element effective in improving the corrosion resistance of hot-pressed parts. In order to obtain this effect, the Co content is preferably 0.01% or more. The Co content is more preferably 0.02% or more, or 0.03% or more.
[0107] On the other hand, even if the Co content exceeds 2.00%, the above effect is saturated. Therefore, the Co content is preferably 2.00% or less. The Co content is more preferably 1.80% or less, or 1.00% or less.
[0108] Cu: 0.01~2.00%
[0109] Cu is an element effective in improving the corrosion resistance of hot-pressed parts. To achieve this effect, the Cu content is preferably 0.01% or more. The Cu content is more preferably 0.02% or more, 0.03% or more, 0.05% or more, or 0.06% or more.
[0110] On the other hand, if the Cu content exceeds 2.00%, the castability may be reduced. Therefore, the Cu content is preferably 2.00% or less. The Cu content is more preferably 1.80% or less, or 1.00% or less.
[0111] Ni: 0.01~2.00%
[0112] Ni is an element effective in improving the corrosion resistance of hot-pressed parts. In order to obtain this effect, the Ni content is preferably set to 0.01% or more. The Ni content is more preferably 0.02% or more, 0.03% or more, 0.05% or more, or 0.06% or more.
[0113] On the other hand, when the Ni content exceeds 2.00%, castability may be reduced. Therefore, the Ni content is preferably 2.00% or less. The Ni content is more preferably 1.80% or less, or 1.00% or less.
[0114] Ta: 0.0001~0.300%
[0115] Ta is an element effective in improving the corrosion resistance of hot-pressed parts. To achieve this effect, the Ta content is preferably set to 0.0001% or more. The Ta content is more preferably 0.001% or more, 0.003% or more, 0.004% or more, or 0.006% or more.
[0116] On the other hand, even if the Ta content exceeds 0.300%, the above-mentioned effect is saturated. Therefore, the Ta content is preferably set to 0.300% or less. The Ta content is more preferably set to 0.280% or less, or 0.260% or less.
[0117] Ca: 0.0001~0.300%
[0118] Ca is an element effective in improving the corrosion resistance of hot-pressed parts. To achieve this effect, the Ca content is preferably 0.0001% or more. The Ca content is more preferably 0.0005% or more, 0.001% or more, or 0.002% or more.
[0119] On the other hand, even if the Ca content exceeds 0.300%, the above-mentioned effect is saturated. Therefore, the Ca content is preferably 0.300% or less. The Ca content is more preferably 0.010% or less, or 0.005% or less.
[0120] Mg: 0.0001~0.300%
[0121] Mg is an element effective in improving the corrosion resistance of hot-pressed parts. To achieve this effect, the Mg content is preferably 0.0001% or more. The Mg content is more preferably 0.0005% or more, 0.001% or more, or 0.002% or more.
[0122] On the other hand, even if the Mg content exceeds 0.300%, the above effect is saturated. Therefore, the Mg content is preferably 0.300% or less. The Mg content is more preferably 0.010% or less, or 0.005% or less.
[0123] Sr: 0.0001~0.300%
[0124] Sr is an element effective in improving the corrosion resistance of hot-pressed parts. In order to obtain this effect, the Sr content is preferably set to 0.0001% or more. The Sr content is more preferably 0.0005% or more, 0.001% or more, or 0.002% or more.
[0125] On the other hand, even if the Sr content exceeds 0.300%, the above-mentioned effect is saturated. Therefore, the Sr content is preferably 0.300% or less. The Sr content is more preferably 0.010% or less, or 0.005% or less.
[0126] Se: 0.0001~0.300%
[0127] Se is an element effective in improving the corrosion resistance of hot-pressed parts. To achieve this effect, the Se content is preferably 0.0001% or more. The Se content is more preferably 0.0005% or more, 0.001% or more, or 0.002% or more.
[0128] On the other hand, even if the Se content exceeds 0.300%, the above-mentioned effect is saturated. Therefore, the Se content is preferably 0.300% or less. The Se content is more preferably 0.010% or less, or 0.005% or less.
[0129] Re: 0.0001~0.300%
[0130] Re is an element effective in improving the corrosion resistance of hot-pressed parts. To obtain this effect, the Re content is preferably 0.0001% or more. The Re content is more preferably 0.0005% or more, 0.001% or more, or 0.002% or more.
[0131] On the other hand, even if the Re content exceeds 0.300%, the above-mentioned effect is saturated. Therefore, the Re content is preferably 0.300% or less. The Re content is more preferably 0.010% or less, or 0.005% or less.
[0132] Hf: 0.0001~0.300%
[0133] Hf is an element effective in improving the corrosion resistance of hot-pressed parts. In order to obtain this effect, the Hf content is preferably 0.0001% or more. The Hf content is more preferably 0.0005% or more, 0.001% or more, or 0.002% or more.
[0134] On the other hand, even if the Hf content exceeds 0.300%, the above-mentioned effect is saturated. Therefore, the Hf content is preferably 0.300% or less. The Hf content is more preferably 0.010% or less, or 0.005% or less.
[0135] [Other elements]
[0136] The rest (remainder) of the chemical composition of the base steel plate of the hot-pressed part according to the present embodiment is Fe and impurities. Impurities include elements that are mixed from steel raw materials or scraps and / or mixed in the steelmaking process and are allowed within the range that does not damage the characteristics of the hot-pressed steel plate according to the present embodiment.
[0137] The base steel plate of the hot-pressed component involved in this embodiment may also contain the following elements as arbitrary elements in the range shown below instead of a part of Fe. The following arbitrary elements may not be contained, so the lower limit of the content is 0%. In addition, even if the content is less than the lower limit of the following range, it does not have an adverse effect on the characteristics, etc.
[0138] B: 0.0002~0.0100%
[0139] B is an element that has the effect of improving the hardenability during hot pressing or during cooling after hot pressing, thereby improving the strength of the hot pressed part. Therefore, it can be contained as needed. In order to reliably exert this effect, the B content is preferably set to 0.0002% or more.
[0140] On the other hand, when the B content becomes excessive, the above-mentioned effect is saturated, and cracks may be generated during hot rolling. Therefore, when B is contained, the B content is preferably made 0.0100% or less.
[0141] V: 0.005~0.500%
[0142] Ti: 0.005~0.500%
[0143] Nb: 0.010~0.500%
[0144] Zr: 0.005~0.500%
[0145] In addition to the above elements, the base steel plate of the hot pressed part according to the present embodiment may contain V, Ti, Nb, and / or Zr. These elements form carbonitrides in steel and have the effect of improving the strength of the hot pressed part by precipitation strengthening.
[0146] In order to obtain this effect, it is preferable to contain V: 0.005% or more, Ti: 0.005% or more, Nb: 0.010% or more, and / or Zr: 0.005% or more.
[0147] On the other hand, even if the content of one of these elements exceeds 0.500%, a large amount of carbonitrides is generated, and the ductility of the base steel sheet of the hot-pressed component is reduced. Therefore, when V, Ti, Nb, and Zr are contained, the contents are preferably set to 0.500% or less.
[0148] O: 0.0001~0.0070%
[0149] O is an element contained in steel as an impurity, for example. O is an element that forms oxides and may improve corrosion resistance, but on the other hand, may cause degradation of the characteristics of hot-pressed parts. For example, oxides present near the surface of a steel plate cause surface flaws. If oxides are present on the cut surface, notch-shaped flaws are formed on the end surface, and the characteristics of the hot-pressed parts deteriorate. Therefore, it is preferred that the O content is low. In particular, when the O content exceeds 0.0070%, the degradation of the characteristics becomes significant, and therefore, the O content is preferably set to 0.0070% or less. The O content is more preferably set to 0.0050% or less.
[0150] On the other hand, from the perspective of economic cost at the refining limit, the O content is preferably 0.0001% or more.
[0151] REM: 0.0001~0.3000%
[0152] In addition, the base steel plate of the hot pressed component according to the present embodiment may contain REM in addition to the above-mentioned elements.
[0153] REM is an element that has the effect of refining inclusions in steel and improving the hydrogen embrittlement resistance of steel parts after quenching, similarly to Ca. To obtain the above-mentioned effect, the REM content is preferably 0.0001% or more, more preferably 0.0002% or more, or 0.0200% or more.
[0154] However, when the REM content exceeds 0.3000%, the effect is saturated and the cost increases. Therefore, when REM is contained, the REM content is preferably 0.3000% or less. The REM content is more preferably 0.2000% or less.
[0155] Here, REM refers to 17 elements in total, including Sc, Y, La, Nd and other lanthanoid elements, and the content of REM refers to the total content of these elements. REM is added to molten steel using, for example, Fe-Si-REM alloy, and the alloy contains, for example, La, Nd, Ce, and Pr.
[0156] The chemical composition of the base steel plate of the above-mentioned hot-pressed parts can be measured by general analytical methods. For example, ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry) can be used for measurement. C and S can be measured using the combustion-infrared absorption method, N can be measured using the inert gas melting-thermal conductivity method, and O can be measured using the inert gas melting-non-dispersive infrared absorption method. In the case where the steel plate for hot pressing has a coating on the surface, the chemical composition can be analyzed after the coating on the surface is removed by mechanical grinding.
[0157] In the hot-pressed part according to the present embodiment, when the concentration (mass %) of the B1 element (corrosion resistance improving element) at a position of 2.0 μm from the surface of the Al-Fe alloy coating toward the center of the plate thickness (thickness direction) is set to C2, and the concentration (mass %) of the B1 element (corrosion resistance improving element) at a position of 8.0 μm from the surface toward the center of the plate thickness (thickness direction) is set to C8, C2 / C8 is preferably 1.1 or more and 4.0 or less. In this case, the effect of improving the coating adhesion (secondary adhesion) can be obtained.
[0158] When C2 / C8 is less than 1.1, the potential near the surface of the Al-Fe alloy coating is relatively too small, so the coating is easily dissolved when immersed in warm water, etc., and the effect of improving secondary adhesion cannot be fully obtained. On the other hand, when C2 / C8 is greater than 4.0, the potential near the surface of the Al-Fe alloy coating is relatively too large, and it becomes easy to dissolve unevenly, and the effect of improving secondary adhesion cannot be fully obtained. C2 / C8 is more preferably set to 1.5 or more and 3.0 or less.
[0159] The hot-pressed component involved in the present embodiment can also be used in automobiles by changing the strength within the component. As for the method of changing the strength, a steel plate called a tailor welded blank can be used, in which two or more steel plates are joined together by welding or the like in such a way that they have different strengths after hot pressing. Various methods such as laser welding, seam welding, arc welding, and plasma welding can be considered as welding methods, but there are no special limitations. In addition, the hot-pressed component involved in the present embodiment can also be manufactured without using a tailor welded blank. In addition, the hot-pressed component involved in the present embodiment can also be obtained by hot pressing a patchwork blank, which is formed by joining and overlapping two or more steel plates by spot welding.
[0160] <Method for manufacturing hot-pressed parts>
[0161] The hot press component involved in this embodiment can be appropriately manufactured according to a manufacturing method that satisfies the manufacturing conditions described below. However, of course, the manufacturing method of the hot press component involved in this embodiment is not particularly limited. That is, the hot press component having the above-mentioned structure is regarded as the hot press component involved in this embodiment regardless of its manufacturing conditions.
[0162] The method for manufacturing a hot-pressed component according to the present embodiment comprises:
[0163] (I) a step of hot-rolling a steel slab to obtain a hot-rolled steel sheet (hot rolling step);
[0164] (II) a step of coiling the hot-rolled steel sheet (coiling step);
[0165] (III) a step of pickling the hot-rolled steel sheet (pickling step);
[0166] (IV) a step of cold-rolling the hot-rolled steel sheet to obtain a cold-rolled steel sheet (cold rolling step);
[0167] (V) a step of continuously annealing and hot-dip aluminum coating the cold-rolled steel sheet (annealing step and hot-dip aluminum coating step); and
[0168] (VI) A hot pressing step of heating and forming the hot-dip aluminum-plated steel sheet.
[0169] Preferred conditions for each step are described below. For conditions not described below, known conditions can be adopted.
[0170] (Steelmaking process, casting process, hot rolling process)
[0171] Prior to hot rolling, the chemical composition of the steel is adjusted in a steelmaking process so as to satisfy the chemical composition of the base steel plate described above, and then the steel is made into a steel slab by continuous casting in a casting process.
[0172] The obtained steel slab is heated to a temperature of, for example, 1300° C. or lower (eg, 1000 to 1300° C.), hot rolling is started, and hot rolling is completed at about 900° C. (eg, 850 to 950° C.), thereby obtaining a hot-rolled steel sheet.
[0173] (Coiling process)
[0174] The hot-rolled steel sheet after hot rolling is coiled at a predetermined coiling temperature CT. The coiling temperature CT (hereinafter sometimes referred to as CT) is one of the important conditions for the manufacture of hot-pressed parts with excellent corrosion resistance after painting. By controlling the coiling temperature after the hot rolling process, excellent corrosion resistance after painting can be obtained after hot pressing.
[0175] Hot rolling is performed in an atmospheric atmosphere. Therefore, during the period from hot rolling to coiling, Fe scale is formed on the surface of the base steel plate (hot-rolled steel plate), and elements other than Fe that reach the surface of the base steel plate are also easily oxidized to form a composite scale of Fe and elements other than Fe, and a secondary scale is formed at the interface between the Fe scale and the base steel plate. The above scales are all removed in the subsequent pickling process, but the concentration of elements other than Fe on the surface of the base steel plate is reduced.
[0176] Generally, the coiling temperature CT is mostly carried out at a low temperature of 480°C or more and less than 580°C for the purpose of suppressing the generation of carbides that are generated in the base steel plate during natural cooling after coiling and deteriorate the ductility of the blank. However, the inventors have found that by setting the coiling temperature CT to a temperature range of 580 to 780°C (hereinafter referred to as medium CT), it is possible to control the corrosion resistance after hot pressing to be excellent. The reason for this is still uncertain, but the inventors presume as follows.
[0177] When the coiling temperature CT is too high (over 780°C: hereinafter referred to as high CT), the diffusion of the corrosion resistance improving elements (B group elements) contained in the base steel plate to the surface of the steel plate is promoted, and the concentration of the corrosion resistance improving elements (B group elements) in the surface layer of the base steel plate after coiling is high. On the other hand, since the thickness of the oxide scale formed until the coiling is completed is thick, the thickness of the oxide scale removed in the pickling process described later also becomes larger. As a result, the concentration of the corrosion resistance improving elements (B group elements) near the surface of the steel plate after the oxide scale is removed is significantly reduced compared to before the oxide scale is removed.
[0178] On the other hand, when the coiling temperature CT is too low (480°C or more and less than 580°C: hereinafter referred to as low CT), it is difficult to cause the corrosion resistance improving elements (B group elements) contained in the base steel plate to diffuse to the surface of the steel plate, and the concentration of the corrosion resistance improving elements (B group elements) in the surface layer of the base steel plate after coiling is lower than that in the case of high CT. Since the thickness of the oxide scale formed until the coiling is completed is thin, the thickness of the oxide scale removed in the pickling process is also small, but since the concentration of the corrosion resistance improving elements (B group elements) after the coiling is completed is low, the concentration of the corrosion resistance improving elements (B group elements) in the surface of the base steel plate after the oxide scale is removed is also low.
[0179] In contrast, by setting the coiling temperature CT to the preferred coiling temperature (580-780°C: referred to as medium CT), the diffusion of corrosion resistance improving elements (B group elements) to the surface of the base steel plate can be moderately promoted. Therefore, the concentration of corrosion resistance improving elements (B group elements) in the surface layer of the base steel plate after coiling is relatively high. In addition, since the thickness of the oxide scale formed until the coiling is completed is not as thick as in the case of high CT, the thickness of the oxide scale removed in the pickling process is not large. As a result, the concentration of corrosion resistance improving elements (B group elements) in the surface of the base steel plate after the oxide scale is removed becomes higher than that in either the high CT or low CT cases.
[0180] The concentration of the corrosion resistance improving element (B group element) after the oxide scale is removed by the pickling process is high, and the concentration of the corrosion resistance improving element (B group element) on the surface of the base steel plate is high even after the cold rolling process, hot dip plating process, and hot pressing process described later. As a result, excellent corrosion resistance after painting can be obtained.
[0181] Furthermore, although carbides are sometimes generated by setting the temperature to medium CT, carbides are dissolved by heating during hot pressing. Therefore, even if the coiling temperature CT is set to 580° C. or higher, the material of the hot pressed part after hot pressing, which is important as a part property, does not deteriorate.
[0182] In order to obtain the above effects, the coiling temperature CT of the steel sheet is set to medium CT (580-780°C). The lower limit of the coiling temperature CT of the hot-rolled steel sheet is preferably 610°C, more preferably 620°C. In addition, the upper limit of the coiling temperature CT of the steel sheet is preferably 770°C, more preferably 760°C.
[0183] <Pickling process>
[0184] The conditions for pickling of the hot-rolled steel sheet after coiling are not particularly limited, and any method such as hydrochloric acid pickling and sulfuric acid pickling can be used, but compared with sulfuric acid pickling, hydrochloric acid pickling is easy to suppress the reduction of the concentration of elements other than Fe on the surface of the steel sheet, so hydrochloric acid pickling is preferably used. In addition, it is also possible to form an oxide-containing region inside the base material after hot-dip aluminum plating in the subsequent process by leaving a part of the composite oxide scale of Fe and elements other than Fe and the secondary oxide scale generated at the interface of the Fe oxide scale and the base material. Therefore, the pickling time is preferably set to less than 600 seconds. However, when the pickling time is less than 10 seconds, the Fe oxide scale remains, forming a part that cannot be plated during hot-dip plating, so it is not practical. Therefore, the pickling time is preferably more than 10 seconds and less than 600 seconds. More preferably, it is more than 20 seconds and less than 400 seconds.
[0185] The concentration of the acid used is not particularly limited, but is preferably 5 to 20% by mass.
[0186] The treatment temperature is preferably 30 to 60°C. When the temperature is lower than 30°C, the reaction between the oxide scale and the acid is difficult to proceed, and the Fe oxide scale is likely to remain. On the other hand, if the temperature exceeds 60°C, the effect of Fe oxidation becomes greater, and the function of removing the oxide scale becomes weaker. It is preferred to remove oxides such as FeO, Fe2O3, and Fe3O4 by pickling. For example, it can be confirmed that these substances have been removed by analyzing the diffraction image of a transmission electron microscope.
[0187] <Cold rolling process>
[0188] (About cold rolling rate)
[0189] The hot-rolled steel sheet is cold-rolled after pickling to become a cold-rolled steel sheet. The cold rolling rate in the cold rolling can be set to, for example, 30 to 90%, preferably 40% to 70%.
[0190] <Annealing process>
[0191] The cold rolled steel sheet obtained by the above treatment is continuously annealed (recrystallization annealed) and hot dipped in a hot dip coating line. Annealing in the hot dip coating line can be performed using a full reduction furnace using radiation tube heating or an oxidation-reduction furnace, etc. The full reduction furnace uses radiation tube heating, and the oxidation-reduction furnace is provided with an oxidation furnace using combustion gas heating, which is generally called a Sendzimir type annealing furnace, and a reduction furnace using radiation tube heating. However, this embodiment can be realized regardless of which type of heating furnace is used.
[0192] In the case of annealing after aluminum plating, the temperature rise rate is relatively slow due to the low emissivity of the aluminum plating layer on the surface. Therefore, the annealing time becomes longer and the productivity may not be high. In addition, when the annealing time is long, the concentration of corrosion resistance improving elements (B group elements) in the Al-Fe alloy plating layer after the plating process and the heating process during hot pressing becomes insufficient, and it is possible that the corrosion resistance after hot pressing cannot be ensured. Therefore, hot dip plating is performed after annealing.
[0193] In addition, when the Al-Fe alloy coating is formed by heating with a laser or the like, it is easy to form a uniform phase in a wide range. In this case, it becomes difficult to obtain the Al-Fe alloy coating and the concentration distribution of the corrosion resistance improving element (B group element) which are preferred for obtaining corrosion resistance after hot pressing, so it is not preferred.
[0194] The highest plate temperature T during annealing process max The temperature is preferably 700 to 900°C.
[0195] In addition, when the position t is measured from the surface of the steel plate toward the center of the plate thickness at a position t / 4 Q The total concentration of each corrosion resistance improving element (B group element) is ΣFQi When , it is preferred to satisfy the following formula.
[0196] 1.00≤T max ×ΣF Qi ≤900
[0197] ΣF Qi is at a distance t / 4 from the surface Q The concentration (mass %) of each corrosion resistance improving element (B group element) was measured by EPMA point analysis and their values were summed up. In the case of EPMA analysis, a position t t / 4 from the surface was selected in the low-magnification secondary electron image at a position 10 mm or more from the end of the steel plate. Q At this position, the measurement is performed with a magnification of 3000 times or more, an acceleration voltage of the electron beam of 10 kV to 30 kV, and an irradiation current of 10 to 30 nA. The quantitative value obtained here is used as the concentration (mass %) of each corrosion resistance improving element (B group element).
[0198] In T max ×ΣF Qi When it is less than 1.00, the concentration of the corrosion resistance improving element (B group element) in the Al-Fe alloy plating layer after the plating step and the heating step during hot pressing becomes small, and the corrosion resistance after hot pressing may be reduced.
[0199] On the other hand, if T max ×ΣF Qi If the temperature exceeds 900, the alloy cost, heating cost and productivity are at a disadvantage. Therefore, T max ×ΣF Qi It is preferably in the range of 1.00 to 900. max ×ΣF Qi It is more preferably 30 or more and 600 or less, and further preferably 50 or more and 500 or less.
[0200] In addition, regarding the concentration gradient of the corrosion resistance improving element in the base steel plate of the hot-pressed component, as described above, it is preferable that C2 / C8 be 1.1 or more and 4.0 or less.
[0201] C2 and C8, through the Q The same method as the measurement at the positions was used, and low-magnification secondary electron images were selected at positions 2.0 μm and 8.0 μm from the surface of the Al-Fe alloy coating, and the concentration was measured by EPMA point analysis at these positions.
[0202] In addition, during annealing, when the sheet temperature is in the range of 650 to 900° C., the annealing atmosphere is preferably an atmosphere with an oxygen potential value of -3.0 to 0.5, where the oxygen potential is determined by the water vapor partial pressure PH2O Divided by the hydrogen partial pressure P H2 The common logarithm of the obtained value is log(P H2O / P H2 ) is expressed. The reason is that: in log(P H2O / P H2 ) is less than -3.0, the oxidizable elements Mn and Si cannot be selectively oxidized and reduced, and the wettability of the components of the plating bath in the hot dip plating process in the subsequent step is insufficient. As a result, plating defects may occur, and the cost of H2 gas required to reduce the oxygen potential is incurred, which is not economical. On the other hand, when log(P H2O / P H2 ) exceeds 0.5, the amount of oxide generated increases, so the wettability of the components of the plating bath in the hot dip plating treatment in the subsequent step is insufficient, resulting in the possibility of plating defects.
[0203] In addition, it is preferred to adjust log(P H2O / P H2 ) is greater than -3.0 and less than 0.5, and is set to 60 to 500 seconds. For example, when the highest plate temperature is set to 750°C, the temperature range for controlling the oxygen potential is preferably set to a range where the plate temperature is greater than 650°C and less than 750°C, and the annealing time in this temperature range is preferably set to greater than 60 seconds and less than 500 seconds. When the annealing time is less than 60 seconds, more oxides remain on the surface of the steel plate, so the wettability of the components of the plating bath in the hot dip treatment in the subsequent process is insufficient. As a result, plating defects may occur. On the other hand, if the annealing time exceeds 500 seconds, due to the presence of oxides of easily oxidizable elements, the wettability of the components of the plating bath in the hot dip treatment in the subsequent process is insufficient. As a result, plating defects may occur. Moreover, there is a concern that productivity will be reduced.
[0204] <Hot-dip galvanizing process>
[0205] The annealed cold-rolled steel sheet is hot-dip plated (hot-dip aluminum plated) to obtain a hot-dip plated steel sheet.
[0206] Regarding the plating bath in the hot-dip plating treatment, in the case of obtaining a hot-pressed part having an Al-Fe alloy plating layer, for example, the following bath is used to manufacture an aluminum-plated steel sheet, and the bath contains, in terms of mass %, in a manner that totals 100%: 80% to 97% Al, 0% to 15% Si, 0% to 5% Zn, 0% to 5% Fe, 0% to 3% or more selected from Mg, Ca, Sr and Li, and impurities in total.
[0207] (Si: 0-15.0%)
[0208] The Si contained in the coating of the aluminum-plated steel sheet affects the reaction between Al and Fe generated during hot pressing. In the heating process during hot pressing, if Al and Fe react excessively, the press formability of the Al-Fe alloy coating itself may be impaired. On the other hand, in the heating process during hot pressing, if the reaction is excessively suppressed, Al may adhere to the pressing die. In order to avoid this problem, the Si content in the molten aluminum bath is preferably 0% or more and 15.0% or less.
[0209] (Mg, Ca, Sr, Li: 0 to 3.0% in total)
[0210] In order to improve the oxidation resistance of the coating, it may also contain at least one of magnesium (Mg), calcium (Ca), strontium (Sr) and lithium (Li) in a total amount of less than 3.0%, and it is particularly preferred to contain at least one of Mg, Ca, Sr and Li in a total amount of more than 0.01% and less than 3.0% relative to the molten aluminum bath.
[0211] When the total content of Mg, Ca, Sr and Li in the coating is set to 0.01% or more, the oxidation resistance of the coating can be improved. The total content of Mg, Ca, Sr and Li is more preferably 0.05% or more. However, even if a coating bath containing no Mg, Ca, Sr and Li is used, an aluminum-plated steel sheet having excellent corrosion resistance and thermal properties can be manufactured, so the total content of Mg, Ca, Sr and Li in the coating bath may be 0%. In addition, Mg and / or Ca may be contained in order to form an oxide layer composed of Al oxide and Mg and / or Ca oxide.
[0212] On the other hand, when the total content of Mg, Ca, Sr and Li exceeds 3.0%, excessive oxides are generated, which may cause problems of non-plating during hot dip plating. The total content of Mg, Ca, Sr and Li is more preferably 1.0% or less.
[0213] (Zn: 0-5.0%)
[0214] In order to improve the sacrificial corrosion resistance of the coating, the coating bath may also contain zinc (Zn). When the exposed portion of the steel substrate such as the cut surface is exposed to rainwater or salt water, Zn has a lower potential than the steel substrate, so it can be dissolved instead of the steel substrate to prevent the steel substrate as the base material from being corroded. The Zn content in the hot dip coating bath is preferably 0% or more and 5.0% or less.
[0215] (Fe: 0~5.0%)
[0216] In order to ensure the adhesion of the coating of the aluminum-plated steel sheet, the coating bath may contain iron (Fe). By containing Fe, an Al-Fe intermetallic compound layer is formed at the interface between the coated steel sheet and the steel sheet, thereby improving the adhesion. The Fe content in the hot-dip coating bath is preferably 0% or more and 5.0% or less, including iron dissolved by continuously immersing the steel sheet in the bath and iron dissolved from equipment and containers present in the bath.
[0217] The hot-dip coating bath preferably contains the above-mentioned components, Al, and impurities so that the total amount becomes 100%.
[0218] (Aluminum coating adhesion)
[0219] In the case of aluminum-plated steel sheets, after the above-mentioned annealing, the steel sheets are continuously immersed in a hot dip bath (molten aluminum bath) during cooling, and the adhesion amount of the bath components is controlled by wiping treatment to form an aluminum coating. The adhesion amount of the aluminum coating is not particularly limited, for example, it is preferably 20 g / m2 on one side of the steel sheet. 2 Above and 130g / m 2 the following.
[0220] When the adhesion is less than 20g / m 2 In the case of 30 g / m, the corrosion resistance after hot pressing is sometimes insufficient. More preferably, 30 g / m 2 above.
[0221] On the other hand, when the adhesion exceeds 130 g / m 2 In the case of 100 g / m2, the time until Fe is fully diffused in the heating process of hot pressing becomes longer. As a result, productivity may be reduced or the coating may peel off during hot pressing. The amount of aluminum coating is more preferably 100 g / m2. 2 the following.
[0222] (About the method for measuring the amount of aluminum plating)
[0223] As a method for determining the amount of aluminum plating, for example, a sodium hydroxide-hexamethylenetetramine-hydrochloric acid peeling weight method can be cited. Specifically, as described in JIS G 3314: 2011, a predetermined area S (m 2 ) (e.g., 50 mm × 50 mm) test piece, and pre-measure the weight w1 (g). Then, immerse in sodium hydroxide aqueous solution and hydrochloric acid aqueous solution with hexamethylenetetramine added in sequence until the foaming caused by the dissolution of the coating subsides, then immediately rinse with water and measure the weight w2 (g) again. At this time, the adhesion amount of the aluminum coating (g / m 2 ) can be calculated from (w1-w2) / S.
[0224] <Hot pressing process>
[0225] The aluminum-plated steel sheet obtained through the above steps is hot-pressed to obtain a hot-pressed component.
[0226] (About hot pressing)
[0227] Hot pressing is one of the important processes in manufacturing hot-pressed parts with excellent corrosion resistance after painting. By using this process to control the concentration of corrosion resistance improving elements (B group elements) in the Al-Fe alloy plating layer, hot-pressed parts with excellent corrosion resistance after painting can be obtained.
[0228] Specifically, the aluminum-plated steel sheet obtained above is heated to 850°C or higher under predetermined heating conditions and then formed using a die while being rapidly cooled at an average cooling rate of 30°C / sec or higher, thereby manufacturing a hot-pressed component having excellent corrosion resistance after coating.
[0229] As heating conditions, when the time from room temperature to 600°C during hot pressing is set to t1 (seconds), and the time from exceeding 600°C until being extracted from the heating furnace is set to t2 (seconds), by satisfying the following formula (1), the corrosion resistance improving element (B group element) can be diffused into the Al-Fe alloy plating layer. In this case, the corrosion resistance of the hot pressed part after coating is improved.
[0230] On the other hand, when t2 is less than 0.9×t1, the corrosion resistance improving elements (B group elements) do not migrate sufficiently to the alloy plating layer, so that the corrosion resistance after painting is not improved.
[0231] On the other hand, when t2 exceeds 20×t1, alloying proceeds too much and plating peeling increases, which is not preferable from the viewpoint of ensuring plating adhesion.
[0232] 0.9×t1≤t2…Formula (1)
[0233] Furthermore, it is more preferable that during the heating process of the hot pressing step, the position t / 4 of the base steel plate Q The total concentration of each corrosion resistance improving element (B group element) ΣF Qi And the time t2 from when the temperature exceeds 600° C. until the temperature is taken out from the heating furnace satisfies the following formula (2).
[0234] At 10000×(ΣF Qi ) / t2 is less than 0.05, the diffusion of the corrosion resistance improving elements (B group elements) into the Al-Fe alloy plating layer becomes insufficient, and the corrosion resistance may not be sufficiently improved. Qi When ) / t2 exceeds 500, alloying of the Al—Fe alloy plating layer proceeds too much, and plating peeling increases, which is not preferable from the perspective of ensuring plating adhesion.
[0235] 0.05≤10000×(ΣF Qi ) / t2≤500···Formula (2)
[0236] When C2 / C8 is set in the range of 1.1 to 4.0, the relationship between the time t1 (seconds) from room temperature to 600°C during hot press heating and the time t2 (seconds) from exceeding 600°C until being removed from the heating furnace preferably satisfies the following equation.
[0237] 15≤t2×t2 / (t1+t2)≤2300
[0238] As a heating method during hot pressing, furnace heating using a common electric heater, or a heating method using radiant heat such as far infrared rays, mid infrared rays, or near infrared rays can be used.
[0239] In addition, in this heating process, the maximum plate temperature is set to 850°C or more. The reasons for setting the maximum plate temperature to 850°C or more are as follows. The first reason is to heat the steel plate to the austenite region and then quench it. The second reason is to allow Fe to fully diffuse to the surface of the aluminum-plated steel plate and alloy the Al-Fe alloy coating. The maximum plate temperature during hot press heating is preferably 870°C or more.
[0240] On the other hand, the upper limit of the maximum plate temperature of the aluminum-plated steel sheet during hot press heating is not particularly limited, but from the viewpoint of the durability of the heater and the heating furnace, the maximum plate temperature is preferably 1050° C. or less. The maximum plate temperature during hot press heating is more preferably 1000° C. or less.
[0241] (Regarding hot press forming and cooling speed)
[0242] Next, the heated aluminum-plated steel sheet is placed between a pair of upper and lower forming dies for press forming, and rapidly cooled during the press forming to form the desired shape. The aluminum-plated steel sheet is kept stationary at the lower dead point of the press for several seconds, so that it can be quenched by contact cooling of the forming dies to obtain a hot press formed component.
[0243] The cooling rate during cooling is preferably set to 30°C / second or more so that at least a portion of the structure of the base steel plate of the hot-pressed component contains a martensite phase or a bainite phase. The cooling rate is a value obtained by dividing the difference between the starting temperature of forced cooling using the mold (i.e., the plate temperature of the material when the mold and the material are initially in contact) and the ending temperature (i.e., the plate temperature of the material when the mold and the material are separated) by the time of forced cooling, which is the so-called average cooling rate. A more preferred cooling rate is 50°C / second or more. In addition, the upper limit of the cooling rate is not particularly limited, but the cooling rate can be set, for example, to 1000°C / second or less. A more preferred cooling rate is 500°C / second or less.
[0244] The method for manufacturing the hot press component according to the present embodiment has been described in detail above.
[0245] Example
[0246] Next, the embodiments of the present invention are described, but the conditions in the embodiments are one condition example adopted to confirm the feasibility and effect of the present invention, and the present invention is not limited to this one condition example. The present invention can adopt various conditions within the limit of not departing from the gist of the present invention and achieving the purpose of the present invention.
[0247] <Aluminum-coated steel sheet>
[0248] Steel billets having the chemical composition shown in Table 1-1 and Table 1-2 (the balance is Fe and impurities) are used, heated, hot-rolled, and then coiled at the temperature shown in Table 2. Thereafter, pickling, cold rolling, continuous annealing, and continuous hot-dip aluminum plating are performed to produce coated steel sheets with a thickness of 0.5 to 3.5 mm. The finishing temperature during hot rolling is 800 to 1000°C, and the cumulative reduction rate during cold rolling is 30 to 80%. In continuous annealing, the highest plate temperature T max The temperature of the aluminum plating bath is set to 700-900°C and 660-690°C. max ×ΣF Qi 、The log(P H2O / P H2 ) and log(P H2O / P H2 ) is -3.0 or more and 0.5 or less as shown in Table 5-1 and Table 5-2. The composition of the plating bath is shown in Table 3. The coating weight was adjusted by wiping treatment so that it became 40 g / m on both sides. 2 ~160 / m 2 .
[0249] Thus, an aluminum-plated steel sheet was manufactured.
[0250] Table 1-1
[0251]
[0252] Table 1-2
[0253]
[0254] Table 2
[0255]
[0256] Table 3
[0257]
[0258] <Hot-pressed parts>
[0259] The manufactured aluminum-plated steel sheet is cut into 300mm×220mm, and the atmosphere temperature of the heating furnace is set to 870℃~980℃ in such a way as to achieve the hot pressing heating conditions shown in Table 4, Table 5-1, and Table 5-2. The time from room temperature to 600℃ is set to t1 seconds, and the time from exceeding 600℃ until being extracted from the heating furnace is set to t2 seconds. The atmosphere gas is set to a mixed gas of O2 and N2. During heating, in order to control t1 and t2, the atmosphere temperature is changed during heating as needed. After heating, the mold is cooled at a cooling rate of more than 40℃ / second, and the holding time at the lower dead point is set to 8 seconds, thereby hot pressing is performed to obtain a hot pressed part.
[0260] Table 4
[0261]
[0262] The thickness of the Al-Fe alloy coating, the Al concentration, and the content of C max , C Q The types and concentrations of group B elements, the types of other included elements, the types of intermetallic compounds when the Fe-Al alloy plating layer contains intermetallic compounds, the thickness of the oxide layer composed of Al oxide and Mg and / or Ca oxides, C2 / C8, etc. In addition, the coverage of the Al-Fe alloy plating layer on the surface area of the steel sheet was also calculated.
[0263] The results are shown in Table 5-3 and Table 5-4.
[0264] In Table 5-3 and Table 5-4, when a plurality of B group elements are contained in the Al-Fe alloy plating layer, they are described as B1, B2, and B3 in descending order of maximum concentration.
[0265] In addition, regarding Examples No. A1 to A43, A45 to A49, and a1 to a12, the Al-Fe alloy plating layer was composed of the intermetallic compounds shown in Table 5-3 and Table 5-4. Regarding A44, even the limited field electron beam diffraction function and EDS function of FE-TEM could not be used for identification.
[0266] In addition, the corrosion resistance after painting and the coating adhesion were evaluated according to the following procedures. In addition, the secondary adhesion was also evaluated.
[0267] <Corrosion resistance after painting>
[0268] The corrosion resistance after painting is evaluated by the following method. After the phosphoric acid chemical conversion treatment is implemented by immersion treatment using the method described in, for example, Japanese Industrial Standard (JIS) K 3151-1996, the flat part of the hot-pressed part with an electrodeposition coating of 20 μm thickness is linearly processed to a length of 70 mm and a width of 1 mm to reach the steel substrate. Then, the cyclic corrosion test (salt spray for 2 hours, drying for 4 hours, and wetting for 2 hours) specified in JASO M609 formulated by the Japan Automobile Technology Association is performed. After 90 cycles or 120 cycles, the sample is taken out and divided into 7 places for every 10 mm defect length, and the maximum width of each side of the rust that has expanded to both sides of the defect is measured. The average value of the 7 places is calculated, and the corrosion resistance after painting is evaluated using the following benchmark.
[0269] In the case of evaluation A and B, it is considered that excellent corrosion resistance is obtained even when exposed to a corrosive environment for a long time, and it is judged as passing. On the other hand, in the case of evaluation C, it is considered that excellent corrosion resistance is not obtained when exposed to a corrosive environment for a long time, and it is judged as failing.
[0270] [Evaluation criteria]
[0271] A: less than 0.10mm
[0272] B: 0.10mm or more and less than 0.40mm
[0273] C: 0.40mm or more
[0274] <Plating Adhesion>
[0275] The coating adhesion was evaluated as follows. The test was conducted according to the tensile test method described in JIS H 8504:1999, and the coating adhesion was evaluated according to the following criteria based on the degree of peeling. After the tensile test was conducted at various elongations, a 2 cm diameter section near the center of the parallel portion of the plate was tested. 2When the adhesive tape specified in JIS Z1522:2009 is pasted on the surface of the sample and it is quickly and forcefully torn off, if part of the sample is within the above 2 cm 2 1cm 2 If the adhesive tape is attached to the adhesive tape, it is considered to be peeled off. If it is less than 1cm 2 , it is considered as no peeling.
[0276] [Evaluation criteria]
[0277] A: No peeling at 2% elongation
[0278] B: There is peeling at 2% elongation, but no peeling at 1% elongation
[0279] C: Peeling occurs at 1% elongation
[0280] In the case of evaluation A and B, it is considered that excellent coating adhesion is obtained even under strict processing conditions and it is judged as acceptable. On the other hand, in the case of evaluation C, it is considered that excellent coating adhesion is not obtained and it is judged as unacceptable.
[0281] <Secondary Adhesion>
[0282] The secondary adhesion is evaluated as follows. After the sample is subjected to phosphoric acid chemical conversion treatment by immersion treatment using the method described in, for example, Japanese Industrial Standard (JIS) K3151-1996, an electroplating coating with a thickness of 10 μm is applied and baked at 170°C for 15 minutes. Then, it is immersed in deionized water at 50°C for 360 hours, and then 100 checkerboards with 1 mm intervals are cut out with a cutter, and the number of peeled parts of the checkerboard part is visually determined, thereby calculating the area ratio of the peeled part. Scoring is performed based on the calculated area ratio.
[0283] (score)
[0284] A: The peeling area is 0% or more and less than 5%
[0285] B: The peeling area is 5% or more and less than 20%
[0286] C: The peeling area is 20% or more and 100% or less
[0287] The above results are shown in Tables 5-1 to 5-4. Tables 5-1 to 5-4 show that Examples A1 to A49 of the present invention have excellent plating adhesion and excellent corrosion resistance even when exposed to a corrosive environment for a long period of time.
[0288] On the other hand, it is found that in Comparative Examples a1 to a12 in Tables 5-1 to 5-4, at least one of the corrosion resistance after painting and the coating adhesion does not satisfy the acceptance criteria.
[0289]
[0290]
[0291]
[0292]
[0293] Industrial Applicability
[0294] According to the above-mentioned method of the present invention, a hot-pressed component having excellent coating adhesion and excellent corrosion resistance even when exposed to a corrosive environment for a long time, and a hot-pressed steel sheet for obtaining the hot-pressed component can be provided. The above-mentioned method of the present invention can obtain a hot-pressed component having excellent corrosion resistance, which contributes to the lightweighting of automobile bodies and the improvement of collision safety.
Claims
1. A hot pressing component, characterized in that: A hot-pressed component comprising a base steel plate, an Al-Fe alloy coating formed on the base steel plate, and an oxide layer formed on the surface of the Al-Fe alloy coating and consisting of Al oxide and one or two oxides of Mg and Ca and having a thickness of 0.05 μm to 3.0 μm, characterized in that: The Al-Fe alloy plating layer has a thickness of 10.0 μm or more and contains, by mass%, 30% or more of Al and one or more selected from W, Mo, Sb, Sn, Cr, Co, Cu, Ni, Ta, Ca, Mg, Sr, Se, Re, and Hf as corrosion resistance improving elements. The element having the highest concentration among the corrosion resistance improving elements in the range from the surface of the Al-Fe alloy plating layer to the center of the plate thickness of the hot-pressed part up to 8.0 μm is defined as B1 element, and the maximum concentration of the B1 element is defined as C max , the plate thickness of the hot press component is t, and the position t / 4 from the surface of the hot press component toward the center of the plate thickness is t Q , the t Q The concentration of the B1 element at the position is set to C Q In the case of C max / C Q is 0.05 or more and 30.00 or less, When the concentration of the B1 element at a position 2.0 μm from the surface of the Al-Fe alloy plating layer toward the center of the plate thickness is set to C2, and the concentration of the B1 element at a position 8.0 μm from the surface toward the center of the plate thickness is set to C8, C2 / C8 is greater than or equal to 1.1 and less than or equal to 4.
0.
2. The hot pressing component according to claim 1, characterized in that: The Al-Fe alloy plating layer is composed of one or more intermetallic compounds.
3. The hot pressing component according to claim 1 or 2, characterized in that: The base steel plate has the following chemical composition: in terms of mass%, it contains C: 0.03-0.60%, Si: 0.005-2.00%, Mn: 0.10-3.00%, P: 0.001-0.100%, S: 0.0001-0.100%, Al: 0.010-0.500% and N: 0.001-0.010%, and W: 0.01-3.00%, Mo: 0.005-2.00%, Sb: 0.005-0.30%, Sn: 0.005-0.50%, Cr: One or more of the following: 0.005~2.00%, Co: 0.01~2.00%, Cu: 0.01~2.00%, Ni: 0.01~2.00%, Ta: 0.0001~0.300%, Ca: 0.0001~0.300%, Mg: 0.0001~0.300%, Sr: 0.0001~0.300%, Se: 0.0001~0.300%, Re: 0.0001~0.300% and Hf: 0.0001~0.300%, and the balance comprises Fe and impurities.
4. The hot pressing component according to claim 3, characterized in that: The chemical composition of the base steel plate further contains, in mass%, one or more selected from the group consisting of B: 0.0002-0.0100%, V: 0.005-0.500%, Ti: 0.005-0.500%, Nb: 0.010-0.500%, Zr: 0.005-0.500%, O: 0.0001-0.0070% and REM: 0.0001-0.3000%.