A method for producing a positive electrode material precursor
Through specific ternary solution preparation and processing methods, the problem of cracking of the high-nickel precursor during the drying process was solved, and a multi-headed large particle ultra-high nickel core-shell precursor that was not easy to break was prepared, which improved the cycle life and capacity of the battery. stability.
Patent Information
- Application Number
- CN202211329637.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-27
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-10-27
AI Technical Summary
High-nickel precursors with large particles and high sphericity are prone to cracking during the drying process, causing damage to the cathode material products and affecting battery cycle life and capacity stability.
Using a specific preparation method of ternary core solution and shell solution, heating and stirring with deionized water, controlling the pH and alkalinity in the reaction kettle, adding nitrogen replacement, concentrating the mother liquor, washing and pressure filtration, and finally in a rotary kiln Low-temperature drying and high-temperature calcination ensure that the precursor does not crack during the entire process.
It effectively avoids the cracking of the precursor during the drying and calcination process, and prepares a multi-head large particle ultra-high nickel core-shell precursor, which improves the cycle life and capacity stability of the battery.
Smart Images

Figure CN115676914B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of inorganic metal materials, and in particular relates to a method for producing a positive electrode material precursor. Background Art
[0002] High-nickel precursors with large particles and high sphericity are prone to cracking during the drying process. The use of such precursors in the preparation of positive electrode materials is prone to damage and cracking of the product, which seriously affects the battery cycle life and capacity stability. Patent CN111908517A uses a segmented intermittent process method to mechanically mix small-size and medium-size precursor particles during the synthesis of high-nickel precursors to maintain the diameter span within a wide range. The collision of particles plays a buffering role and avoids the cracking of particles during the synthesis process, but it cannot effectively avoid the collision and cracking of large particles during the growth process, and only reduces the probability of cracking. Summary of the invention
[0003] In view of the problems in the prior art, the present invention provides a method for producing a positive electrode material precursor. The precursor prepared by the method of the present invention will not crack during the drying and calcining process and has high capacity and stability.
[0004] The present invention adopts the following technical solutions:
[0005] A method for producing a positive electrode material precursor comprises the following steps:
[0006] (1) preparing a ternary core solution having a molar ratio of nickel, cobalt and manganese of (95.5-96.5):(1.5-2.5):(1.5-2.5) and a ternary shell solution having a molar ratio of nickel, cobalt and manganese of (64.5-65.5):(14.5-15.5):(19.5-20.5); adding deionized water to a reactor, heating the reactor and stirring; the deionized water added to the reactor accounts for 74%-76% of the volume of the reactor;
[0007] (2) After nitrogen is introduced into the reactor for replacement, a ternary nuclear solution, liquid alkali, and ammonia solution are added to the reactor for reaction for 80 h to 90 h to obtain a mother liquor; the addition rate of the ternary nuclear solution is 295 L / h to 305 L / h, the addition rate of the liquid alkali is 107 L / h to 113 L / h, and the addition rate of the ammonia solution is 16 L / h to 20 L / h, and the pH in the reactor is controlled to be 11.0 to 12.0 and the total alkalinity is 17.0 g / L to 19.0 g / L;
[0008] (3) After the mother liquor is concentrated, the ternary shell solution is replaced with the ternary core solution and added into the reactor to continue the reaction for 2.5 h to 3.5 h to obtain a precursor slurry;
[0009] (4) washing the precursor slurry with 2.5 g / L-3.5 g / L alkaline solution and 55° C.-65° C. deionized water, and then filtering to obtain a filter cake;
[0010] (5) Drying the filter cake and then calcining it to obtain a precursor oxide.
[0011] Furthermore, in step (1), the reaction kettle is heated to 50°C-60°C and the stirring speed is turned on at 100r / min-120r / min.
[0012] Furthermore, the process conditions for introducing nitrogen into the reactor for replacement in step (2) are: nitrogen purity ≥ 99.99%, nitrogen introduction time is 30min-50min; liquid alkali concentration is 30%-34%, and ammonia solution concentration is 16%-20%.
[0013] Furthermore, in step (3), the mother liquor is concentrated by a concentrator for 79h-81h; the particle size D50 of the precursor slurry is 11μm-12μm.
[0014] Furthermore, in step (4), the washing time of the precursor slurry with alkaline solution and deionized water is 1.0h-2.0h, and the ratio of the solid content of the precursor slurry, the volume of the alkaline solution, and the volume of the deionized water is 1.0:(0.4-0.6):(5-6); SO4 in the filter cake 2- Content less than 600ppm, Na + The content is less than or equal to 500ppm.
[0015] Furthermore, in step (5), the filter cake is conveyed to a rotary kiln for drying and then calcined, and the drying temperature of the filter cake is conveyed to the rotary kiln for drying is 180°C-220°C, and the drying time is 2h-3h; the calcination temperature of the filter cake is conveyed to the rotary kiln for drying and then calcined is 450°C-550°C, and the calcination time is 4h-5h.
[0016] Beneficial technical effects of the present invention: The method of the present invention can prepare multi-head large-particle ultra-high nickel core-shell precursors. The precursors prepared by the present invention do not crack during the drying and calcination processes, effectively solving the problem of high-nickel large-particle products cracking, resulting in reduced battery cycle life and capacity attenuation. The method of the present invention solves the problem of cracking of the particles themselves due to surface tension during the growth of large particles in the normal growth process, and achieves the purpose of preparing large particles that do not crack by agglomerating multi-head particles into balls and wrapping with nanolayers to reduce the surface tension of the particles themselves. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is a SEM image of the ultra-high nickel precursor hydroxide prepared in Example 1 of the present invention;
[0018] Figure 2 This is a Ni-EPMA image of the ultra-high nickel precursor hydroxide prepared in Example 1 of the present invention;
[0019] Figure 3 This is a SEM image of the oxide after calcination of the ultra-high nickel precursor prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0020] A method for producing a positive electrode material precursor of the present invention comprises the following steps:
[0021] (1) Preparation process: prepare a ternary core solution with a molar ratio of Ni:Co:Mn=(95.5-96.5):(1.5-2.5):(1.5-2.5) and a ternary shell solution with a molar ratio of Ni:Co:Mn=(64.5-65.5):(14.5-15.5):(19.5-20.5); add deionized water to a reactor, heat the reactor to 50°C-60°C and start stirring at a stirring speed of 100r / min-120r / min. The deionized water added to the reactor accounts for 74%-76% of the volume of the reactor.
[0022] (2) Reaction process: After nitrogen is introduced into the reactor for substitution, materials are added simultaneously, and the ternary nuclear solution, liquid alkali and ammonia solution are added into the reactor for reaction for 80h-90h to obtain a mother liquor; the concentration of the liquid alkali is 30%-34%, and the concentration of the ammonia solution is 16%-20%. The addition flow rate of the ternary nuclear solution is 295L / h-305L / h, the addition flow rate of the liquid alkali is 107L / h-113L / h, and the addition flow rate of the ammonia solution is 16L / h-20L / h, and the pH in the reactor is controlled to be 11.0-12.0 and the total alkalinity is 17.0g / L-19.0g / L; the process conditions for introducing nitrogen into the reactor for substitution are: nitrogen purity ≥99.99%, and the nitrogen introduction time is 30min-50min.
[0023] (3) During the reaction, the mother liquor is concentrated by a concentrator for 79 h to 81 h, and then the ternary shell solution is replaced by the ternary core solution and added to the reactor to continue the reaction for 2.5 h to 3.5 h. The reactor is then shut down to obtain a precursor slurry. The particle size D50 of the precursor slurry is 11 μm to 12 μm.
[0024] (4) Washing process: The precursor slurry is washed with 2.5g / L-3.5g / L alkaline solution and 55℃-65℃ deionized water, and then filtered to obtain a filter cake, which is washed by a filter press to remove SO4 2- and Na + The precursor slurry is washed with alkaline solution and deionized water for 1.0h-2.0h. The solid content (T) of the precursor slurry and the volume (m 3), volume of deionized water (m 3 ) is 1.0:(0.4-0.6):(5-6); SO4 in the filter cake obtained by washing and drying with a filter press 2- Content less than 600ppm, Na + The content is less than or equal to 500ppm.
[0025] (5) Dry the filter cake and calcine it to obtain a precursor oxide. The filter cake is transported to a rotary kiln for drying and calcination. The drying temperature of the filter cake is 180°C-220°C and the drying time is 2h-3h; the calcination temperature of the filter cake is 450°C-550°C and the calcination time is 4h-5h. The drying and calcination process transports the filter cake to a rotary kiln for drying and calcination. The rotary kiln is a two-stage type. The first stage is a low-temperature drying stage controlled at 180-220°C to obtain a precursor hydroxide, and the second stage is a calcination stage controlled at 450°C-550°C to obtain a precursor oxide.
[0026] The technical solution of the present invention is further explained below by way of embodiments.
[0027] Example 1
[0028] Prepare a ternary core solution with a molar ratio of nickel, cobalt and manganese of 96:2:2 and a ternary shell solution with a molar ratio of nickel, cobalt and manganese of 65:15:20; add deionized water to the reactor, heat the reactor to 55°C and start stirring at a stirring speed of 110 r / min. The deionized water added to the reactor accounts for 75% of the volume of the reactor.
[0029] After nitrogen is introduced into the reactor for replacement, the ternary nuclear solution, liquid alkali and ammonia solution are added into the reactor for reaction for 85 hours to obtain a mother liquor; the concentration of the liquid alkali is 32%, and the concentration of the ammonia solution is 18%. The addition flow rate of the ternary nuclear solution is 300L / h, the addition flow rate of the liquid alkali is 110L / h, and the addition flow rate of the ammonia solution is 18L / h. The pH in the reactor is controlled to be 11.0-12.0 and the total alkalinity is 17.0g / L-19.0g / L; the process conditions for introducing nitrogen into the reactor for replacement are: nitrogen purity ≥99.99%, and the introduction time of nitrogen is 30min.
[0030] After the mother liquor was concentrated by a concentrator for 80 hours, the ternary shell solution was added to the reactor to replace the ternary core solution and the reaction was continued for 3.0 hours to obtain a precursor slurry; the particle size D50 of the precursor slurry was 11.526 μm.
[0031] The precursor slurry was washed with 3.0 g / L alkaline solution and 60°C deionized water, and then filtered to obtain a filter cake; the precursor slurry was washed with alkaline solution and deionized water for 1.5 h, and the solid content (T) of the precursor slurry and the volume (m 3 ), volume of deionized water (m 3 ) is 1:0.5:6; SO4 in the filter cake 2- The content is 520ppm, Na + The content is 390ppm.
[0032] The filter cake is dried and calcined to obtain the precursor oxide. The filter cake is transported to a rotary kiln for drying and calcining. The drying temperature of the filter cake is 200°C and the drying time is 2.5 hours. The calcination temperature of the filter cake is 500°C and the calcination time is 4.5 hours.
[0033] Example 2
[0034] Prepare a ternary core solution with a molar ratio of nickel, cobalt and manganese of 95.5:2.5:2 and a ternary shell solution with a molar ratio of nickel, cobalt and manganese of 65.5:15.0:19.5; add deionized water to the reactor, heat the reactor to 60°C and start stirring at a stirring speed of 120 r / min. The deionized water added to the reactor accounts for 76% of the volume of the reactor.
[0035] After nitrogen is introduced into the reactor for replacement, the ternary nuclear solution, liquid alkali and ammonia solution are added into the reactor for reaction for 90 hours to obtain a mother liquor; the concentration of the liquid alkali is 34%, and the concentration of the ammonia solution is 20%. The addition flow rate of the ternary nuclear solution is 305L / h, the addition flow rate of the liquid alkali is 113L / h, and the addition flow rate of the ammonia solution is 20L / h. The pH in the reactor is controlled to be 11.0-12.0 and the total alkalinity is 17.0g / L-19.0g / L; the process conditions for introducing nitrogen into the reactor for replacement are: nitrogen purity ≥99.99%, and the introduction time of nitrogen is 50min.
[0036] After the mother liquor was concentrated by a concentrator for 81 hours, the ternary shell solution was added to the reactor to replace the ternary core solution and the reaction was continued for 3.5 hours to obtain a precursor slurry; the particle size D50 of the precursor slurry was 11.952 μm.
[0037] The precursor slurry was washed with 3.5 g / L alkaline solution and 65°C deionized water, and then filtered to obtain a filter cake; the precursor slurry was washed with alkaline solution and deionized water for 1 h, and the solid content (T) of the precursor slurry and the volume (m 3 ), volume of deionized water (m 3 ) is 1:0.5:6; SO4 in the filter cake2- The content is 305ppm, Na + The content is 485ppm.
[0038] The filter cake is dried and calcined to obtain the precursor oxide. The filter cake is transported to a rotary kiln for drying and calcining. The drying temperature of the filter cake is 220°C and the drying time is 2 hours. The calcination temperature of the filter cake is 550°C and the calcination time is 4 hours.
[0039] Example 3
[0040] Prepare a ternary core solution with a molar ratio of nickel, cobalt and manganese of 96.5:1.5:2 and a ternary shell solution with a molar ratio of nickel, cobalt and manganese of 64.5:15.5:20; add deionized water to the reactor, heat the reactor to 50°C and start stirring at a stirring speed of 100 r / min. The deionized water added to the reactor accounts for 74% of the volume of the reactor.
[0041] After nitrogen is introduced into the reactor for replacement, the ternary nuclear solution, liquid alkali and ammonia solution are added into the reactor for reaction for 80 hours to obtain a mother liquor; the concentration of the liquid alkali is 30%, and the concentration of the ammonia solution is 16%. The addition flow rate of the ternary nuclear solution is 295L / h, the addition flow rate of the liquid alkali is 107L / h, and the addition flow rate of the ammonia solution is 16L / h. The pH in the reactor is controlled to be 11.0-12.0 and the total alkalinity is 17.0g / L-19.0g / L; the process conditions for introducing nitrogen into the reactor for replacement are: nitrogen purity ≥99.99%, and the nitrogen introduction time is 30min.
[0042] After the mother liquor was concentrated by a concentrator for 79 hours, the ternary shell solution was added to the reactor to replace the ternary core solution and the reaction was continued for 2.5 hours to obtain a precursor slurry; the particle size D50 of the precursor slurry was 11.025 μm.
[0043] The precursor slurry was washed with 2.5 g / L alkaline solution and 55°C deionized water, and then filtered to obtain a filter cake; the precursor slurry was washed with alkaline solution and deionized water for 1.2 h, and the solid content (T) of the precursor slurry and the volume (m 3 ), volume of deionized water (m 3 ) is 1:0.5:6; SO4 in the filter cake 2- The content is 592ppm, Na + The content is 239ppm.
[0044] The filter cake is dried and calcined to obtain a precursor oxide. The filter cake is transported to a rotary kiln for drying and calcining. The drying temperature of the filter cake is 180°C and the drying time is 3 hours. The calcination temperature of the filter cake is 450°C and the calcination time is 5 hours.
Claims
1. A method for producing a positive electrode material precursor, characterized in that: The method comprises the following steps: (1) preparing a ternary core solution having a molar ratio of nickel, cobalt and manganese of (95.5-96.5):(1.5-2.5):(1.5-2.5) and a ternary shell solution having a molar ratio of nickel, cobalt and manganese of (64.5-65.5):(14.5-15.5):(19.5-20.5); adding deionized water to a reactor, heating the reactor to 50° C.-60° C. and stirring at a stirring speed of 100 r / min-120 r / min; the deionized water added to the reactor accounts for 74%-76% of the volume of the reactor; (2) After nitrogen is introduced into the reactor for replacement, a ternary nuclear solution, liquid alkali, and ammonia solution are added to the reactor for reaction for 80 h to 90 h to obtain a mother liquor; the addition rate of the ternary nuclear solution is 295 L / h to 305 L / h, the addition rate of the liquid alkali is 107 L / h to 113 L / h, and the addition rate of the ammonia solution is 16 L / h to 20 L / h, and the pH in the reactor is controlled to be 11.0 to 12.0 and the total alkalinity is 17.0 g / L to 19.0 g / L; (3) After the mother liquor is concentrated by a concentrator for 79 h to 81 h, the ternary shell solution is replaced by the ternary core solution and added to the reactor to continue the reaction for 2.5 h to 3.5 h to obtain a precursor slurry, wherein the particle size D50 of the precursor slurry is 11 μm to 12 μm; (4) The precursor slurry is washed with 2.5g / L-3.5g / L alkaline solution and 55℃-65℃ deionized water for 1.0h-2.0h, and the ratio of the solid content of the precursor slurry, the volume of the alkaline solution, and the volume of the deionized water is 1.0:(0.4-0.6):(5-6); then the filter is filtered to obtain a filter cake. SO4 2- Content less than 600ppm, Na + Content is less than or equal to 500ppm; (5) The filter cake is conveyed to a rotary kiln for drying and then calcined. The drying temperature of the filter cake is 180°C-220°C and the drying time is 2h-3h. The filter cake is conveyed to a rotary kiln for drying and then calcined. The calcination temperature is 450°C-550°C and the calcination time is 4h-5h to obtain a precursor oxide.
2. The method for producing a cathode material precursor according to claim 1, characterized in that: The process conditions for introducing nitrogen into the reactor for replacement in step (2) are as follows: nitrogen purity ≥ 99.99%, nitrogen introduction time 30 min-50 min; liquid alkali concentration 30%-34%, ammonia solution concentration 16%-20%.